Method and system for evaluating fusion degree of recycled asphalt mixture in hot mixing process

Through infrared spectroscopy and thermal imaging technology, the carbonyl index and temperature distribution of regenerated asphalt mixtures are evaluated, which solves the problem that the degree of fusion between old and new asphalt cannot be evaluated in real time in the prior art, and achieves rapid and accurate quality control in the asphalt pavement regeneration process. Improves the performance stability of the mixture.

CN119000784AActive Publication Date: 2024-11-22EAST CHINA JIAOTONG UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411125290.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The prior art cannot evaluate the degree of integration between new and old asphalt in real time and quickly during the asphalt pavement regeneration process, limiting the process optimization and quality control of regenerated asphalt mixtures.

Method used

Infrared spectroscopy technology is used to determine the carbonyl index, combined with thermal imaging technology, the cross-sectional temperature data of the regenerated asphalt mixture is collected, and by calculating the proportion of the area of ​​the low-temperature area, a relationship model of the degree of fusion between old and new bitumen is constructed to realize automated quantitative analysis.

Benefits of technology

Real-time and accurate evaluation of the degree of integration of new and old asphalt in recycled asphalt mixture at the production site, improve the accuracy and operability of evaluation, optimize the production process of recycled asphalt mixture, and improve the overall performance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119000784A_ABST
    Figure CN119000784A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of asphalt pavement regeneration, in particular to a method and a system for evaluating the fusion degree of a regenerated asphalt mixture in a hot mixing process, and the method comprises the following steps: acquiring spectral data of mixed and molten asphalt by using an infrared spectrum technology, calculating a carbonyl index, and establishing a relationship between an old asphalt proportion and the carbonyl index; determining the content of the old asphalt through an extraction method; utilizing infrared thermal imaging to obtain a mixture section temperature diagram, and analyzing temperature distribution to calculate the area proportion of a low-temperature region; and combining a mathematical model to evaluate the fusion degree. According to the method, through real-time data acquisition and analysis, the fusion degree of the new asphalt and the old asphalt is rapidly and accurately evaluated, the production process of the recycled asphalt mixture is optimized, and the use performance and the quality control efficiency of the material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of asphalt pavement regeneration, and in particular to a method and system for evaluating the fusion degree of regenerated asphalt mixture in a hot mix process. Background Art

[0002] Asphalt pavement occupies an important position in modern transportation infrastructure, especially in high-grade pavement, its proportion exceeds 90%. However, after long-term use, the performance of asphalt pavement declines and diseases appear, which affects driving safety and comfort, so it needs to be maintained and renovated. With the improvement of environmental protection requirements, the maintenance of asphalt pavement gradually tends to adopt asphalt pavement regeneration technology. The core of regeneration technology lies in the effective utilization of waste asphalt mixture to reduce resource waste and environmental pollution. The existing technology (Chinese invention patent, publication number: CN114324983B, name: Quantification method and system for the degree of fusion of new and old asphalt in hot regenerated asphalt mixture) quantitatively evaluates the degree of fusion of new and old asphalt by testing the micro-scale modulus of recycled asphalt and nano-tracing methods. Although these methods can reflect the fusion situation, they rely on indoor tests and cannot be evaluated in real time and quickly at the production site, which limits the process optimization and quality control of recycled asphalt mixture in actual engineering. Summary of the invention

[0003] In view of the many problems existing in the above-mentioned prior art, the present invention provides a method and system for evaluating the degree of fusion of recycled asphalt mixture in the hot mix process. The present invention determines the carbonyl index of completely mixed asphalt through infrared spectroscopy technology, thereby constructing a relationship model between the proportion of old asphalt and the carbonyl index, and collects the cross-sectional temperature data of the recycled asphalt mixture in combination with thermal imaging technology. By calculating the area ratio of the low-temperature area, the degree of fusion of the new and old asphalt is finally evaluated. The present invention can not only obtain the temperature distribution of the mixture and the fusion of the new and old asphalt in real time, but also construct a mathematical model based on the data to realize automated quantitative analysis. The implementation of the present invention is helpful to optimize the production process of the recycled asphalt mixture and improve the overall performance stability of the mixture.

[0004] like Figure 1 As shown, the method for evaluating the degree of fusion of recycled asphalt mixture in the hot mix process includes the following steps:

[0005] The infrared spectra of completely mixed asphalt with different ratios of new and old asphalt are obtained by infrared spectrometer, the carbonyl index is calculated, and a linear relationship equation between the ratio of old asphalt and the carbonyl index is constructed;

[0006] The content of old asphalt in the waste asphalt mixture is tested by extraction method, and the mass proportion of old asphalt in the recycled asphalt mixture is calculated;

[0007] An infrared thermal imager is used to collect the cross-sectional temperature image of the recycled asphalt mixture after hot mixing to obtain temperature distribution data;

[0008] The mixed asphalt on the surface of the cube tracer aggregate was recovered by extraction and rotary evaporation, the carbonyl index was calculated by infrared spectroscopy, and the proportion of old asphalt in the mixed asphalt was calculated based on the linear relationship equation.

[0009] According to the heat transfer model between materials, the theoretical temperature values ​​reached by different materials during hot mixing are calculated as the temperature threshold;

[0010] Taking the temperature threshold as the standard, the percentage of pixels below the threshold in the temperature image of the recycled asphalt mixture cross section is calculated to obtain the area percentage of the low temperature area.

[0011] Based on the data set of the degree of fusion of new and old asphalt and the proportion of low-temperature areas in thermal images, a relationship model between the two was constructed and a linear regression analysis was performed;

[0012] Based on the thermal image acquisition results and the low-temperature area ratio relationship model, the fusion degree of new and old asphalt in the recycled asphalt mixture is calculated and evaluated.

[0013] Preferably, the method for calculating the carbonyl index includes:

[0014] Obtain the infrared spectrum of the completely mixed asphalt through an infrared spectrum tester;

[0015] Carbonyl Index I C=O The calculation is as follows:

[0016]

[0017] Among them, A C=O is the area of ​​the carbonyl functional group region; A Referance is the area of ​​the reference functional group region.

[0018] Preferably, the mass ratio of old asphalt in the recycled asphalt mixture is calculated by the following formula:

[0019]

[0020] Among them, x RAP is the mass ratio of old asphalt to total asphalt; C RHMA P is the designed asphalt content of recycled asphalt mixture; RAPi is the usage ratio of the i-th size waste asphalt mixture; C RAPi is the content of old asphalt in the i-th size waste asphalt mixture.

[0021] Preferably, the old asphalt ratio of the asphalt mixed on the surface of the cubic tracer aggregate is x iThe calculation is based on the carbonyl index I C=O , determined by the following relational expression:

[0022] I C=O =a×x i +b

[0023] Among them, x i is the proportion of old asphalt in the fully mixed asphalt; a and b are the specific values ​​of the constant terms in the linear regression model.

[0024] Preferably, the theoretical temperature value T f Calculated by the following formula:

[0025]

[0026] Among them, T f It is the theoretical value of the temperature that can be reached after the materials in the recycled asphalt mixture are mixed with each other; C i is the specific heat capacity of the i-th material; m i is the quality of the i-th material; T i is the initial mixing temperature of the ith material.

[0027] Preferably, the low temperature area accounts for P T Calculated by the following formula:

[0028]

[0029] Among them, P T T is the area ratio of low temperature area in the thermal imaging image of the recycled asphalt mixture cross section; min T is the lowest temperature in the thermal imaging image of the recycled asphalt mixture cross section; f T is the theoretical temperature that can be reached after different materials in the recycled asphalt mixture are mixed together; max The highest temperature in the thermal imaging image of the recycled asphalt mixture cross section; N i is the number of pixels corresponding to temperature i in the thermal imaging image of the recycled asphalt mixture cross section.

[0030] Preferably, the degree of fusion of new and old asphalt is Y BD The proportion of low temperature area x PT The relationship model is expressed by the following linear regression equation:

[0031] Y BD =d×x PT +e

[0032] Among them, Y BD is the calculated value of the mixing degree in the recycled asphalt mixture; x PTis the area ratio of low temperature area in the cross-sectional temperature image obtained by infrared thermal imager during the mixing process of recycled asphalt mixture; d and e are the specific values ​​of constant terms in the linear regression model.

[0033] Preferably, the test environment conditions of the infrared spectrum tester include: the test environment temperature is 25℃±0.5℃, the test resolution is 4cm -1 , the background and sample scan times were 32 times, and the wave number range was 4000cm -1 Up to 400cm -1 .

[0034] Preferably, the infrared thermal imager is used to collect the cross-sectional temperature image of the recycled asphalt mixture in real time, and process it through the thermal image data analysis module to determine the area proportion of the low-temperature area.

[0035] like Figure 2 As shown, a system for implementing the method for evaluating the degree of fusion of recycled asphalt mixture in a hot mix process comprises:

[0036] Infrared spectrum test module, used to obtain infrared spectra of completely mixed asphalt with different ratios of new and old asphalt, calculate the carbonyl index, and construct a linear relationship equation between the ratio of old asphalt and the carbonyl index;

[0037] The extraction analysis module is used to test the content of old asphalt in the waste asphalt mixture by extraction method and calculate the mass proportion of old asphalt in the recycled asphalt mixture;

[0038] Infrared thermal imaging module, used to collect cross-sectional temperature images of recycled asphalt mixture after hot mixing to obtain temperature distribution data;

[0039] The tracer recovery module recovers the mixed asphalt on the surface of the cube tracer aggregate by extraction and rotary evaporation, calculates the carbonyl index by infrared spectroscopy, and calculates the proportion of old asphalt in the mixed asphalt based on a linear relationship equation;

[0040] The temperature calculation module calculates the theoretical temperature values ​​reached by different materials during the hot mixing process as the temperature threshold according to the heat transfer model between the materials;

[0041] The area analysis module uses the temperature threshold as the standard to calculate the percentage of pixels below the threshold in the temperature image of the recycled asphalt mixture cross section, and obtains the area percentage of the low-temperature area;

[0042] The relationship modeling module builds a relationship model between the two based on the data set of the degree of integration of new and old asphalt and the proportion of low-temperature areas in thermal images, and performs linear regression analysis;

[0043] The fusion degree evaluation module calculates and evaluates the fusion degree of new and old asphalt in the recycled asphalt mixture based on the thermal image acquisition results and the low-temperature area ratio relationship model.

[0044] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0045] By introducing infrared spectroscopy and thermal imaging technology, the present invention realizes real-time and accurate evaluation of the degree of integration of new and old asphalt in recycled asphalt mixture;

[0046] Compared with the indoor experiments relied on by the prior art, the present invention can directly analyze the recycled asphalt mixture at the production site and quickly provide quantitative results of the degree of fusion;

[0047] The combination of infrared spectrum testing and thermal image analysis effectively solves the shortcomings of existing technologies in terms of real-time performance and convenience.

[0048] The present invention also uses a linear regression model to construct a relationship model between the degree of fusion of new and old asphalt and the area ratio of the low-temperature area in the thermal imaging image, thereby improving the accuracy and operability of the assessment. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 It is a schematic diagram of the process of the present invention;

[0050] Figure 2 It is a structural block diagram of the system of the present invention;

[0051] Figure 3 The infrared spectrum test results of the old asphalt and SBS modified asphalt used in the embodiments of the present invention;

[0052] Figure 4 Four design gradation diagrams of recycled asphalt mixtures used in the embodiments of the present invention;

[0053] Figure 5 This is a cross-sectional thermal image of the recycled asphalt mixture after mixing in solution 1 adopted in the embodiment of the present invention;

[0054] Figure 6 This is a schematic diagram of the statistical results of the temperature distribution in the cross-section thermal image after the mixing of the regenerated asphalt mixture is completed in Scheme 1 adopted in the embodiment of the present invention;

[0055] Figure 7 This is a graph showing the degree of fusion of new and old asphalt in the regenerated asphalt mixture in an embodiment of the present invention and the changing trend of the area ratio of the low-temperature region in the thermal image obtained by in-situ measurement. DETAILED DESCRIPTION

[0056] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In the following detailed description, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of the embodiments of the present disclosure. However, it is obvious that one or more embodiments may also be implemented without these specific details. In addition, in the following description, descriptions of known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.

[0057] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.

[0058] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art, unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification, and should not be interpreted in an idealized or overly rigid manner.

[0059] The present invention provides a method and system for evaluating the degree of fusion of recycled asphalt mixture in a hot mix process, comprising the following steps:

[0060] Step S01: The waste asphalt mixtures used in the present invention have specifications of 0-8 mm, 8-12 mm, and 12-20 mm. The three types of waste asphalt mixtures are dried in an electric blast drying oven at 40°C until the quality remains unchanged, so as to completely remove the moisture in the three types of waste asphalt mixtures.

[0061] The three types of waste asphalt mixtures after drying were weighed 2000g respectively, and the old asphalt in the waste asphalt mixtures was recovered by extraction and rotary evaporation.

[0062] The new asphalt in the recycled asphalt mixture is SBS modified asphalt.

[0063] New asphalt and old asphalt are sampled in the ratio of 100%:0%, 70%:30%, 50%:50%, 30%:70% and 0%:100% respectively. The total mass of the new and old asphalt that are completely fused is designed to be 50g. The new asphalt and old asphalt sampled according to the designed ratio are added to a mixing mold. A mixer is used to stir the new and old asphalt in the mold at a speed of 500rpm for no less than 15 minutes to obtain completely fused asphalt.

[0064] The completely fused new and old asphalt was sampled according to the test requirements of infrared spectrum test, and the infrared spectrum tester was used. The test environment temperature was 25℃±0.5℃, the test resolution was 4cm-1, the background and sample scanning times were 32 times, and the test wave number range was 4000cm-1~400cm-1. According to the above parameter requirements, the infrared spectra of completely fused asphalt with different ratios of new asphalt and old asphalt were tested respectively. The test results of the infrared spectra of old asphalt and SBS modified asphalt are as follows Figure 4 shown.

[0065] According to formula 1, combined with the infrared spectrum test results, the carbonyl index of the fully fused asphalt at different fusion ratios of new asphalt and old asphalt was calculated. The results are shown in Table 1.

[0066] Formula 1:

[0067]

[0068] In the formula, I C=O A is the carbonyl index of the fully fused asphalt; C=O A is the area of ​​the carbonyl functional group region, which is the area of ​​the closed region formed by connecting the upper wavelength limit (1722 cm-1) and the lower wavelength limit (1672 cm-1) of the functional group; Referance is the area of ​​the reference functional group region, which is the area of ​​the closed region formed by connecting the upper limit of the reference functional group (3026 cm-1) and the lower limit of the wavelength (2766 cm-1);

[0069] Old asphalt ratio / % 0 30 50 70 100 Carbonyl Index 0.00008853 0.00456 0.00764 0.00938 0.0149

[0070] Table 1 Calculation results of carbonyl index of fully fused asphalt at different fusion ratios of new asphalt and old asphalt

[0071] According to Formula 2, the relationship equation between the proportion of old asphalt in the completely mixed asphalt with different proportions of new asphalt to old asphalt and the carbonyl index IC=O is constructed:

[0072] Formula 2:

[0073] I C=O =a×x i +b

[0074] In the formula, x i is the proportion of old asphalt in the fully mixed asphalt; a and b are the specific values ​​of the constant terms in the linear regression model;

[0075] Using the data in Table 1 and formula 2, the mathematical relationship between the old asphalt ratio and the carbonyl index is obtained as follows:

[0076] I C=O =1.4307×10 -4 ×i +8.8980×10 -5

[0077] Step S02: Weigh 1200g of the dried waste asphalt mixtures with specifications of 0-8mm, 8-12mm, and 12-20mm respectively, and use the extraction method to test the aggregate masses of the waste asphalt mixtures of different specifications after extraction, which are 1133.64g, 1160.28g, and 1159.08g respectively. The masses of the old asphalt are calculated to be 66.36g, 39.72g, and 40.92g respectively. Using formula 3, the asphalt contents of the waste asphalt mixtures with specifications of 0-8mm, 8-12mm, and 12-20mm are calculated to be 5.53%, 3.31%, and 3.41% respectively.

[0078] Formula 3:

[0079]

[0080] In the formula, C RAP is the content of old asphalt in waste asphalt mixture; m1 is the mass of old asphalt in waste asphalt mixture obtained by extraction test; m RAP The total mass of waste asphalt mixture used for extraction test;

[0081] The proportion of waste asphalt mixture added to the recycled asphalt mixture is designed to be 40%, of which the proportions of 0-8mm, 8-12mm, and 12-20mm waste asphalt mixtures are 13%, 13%, and 14%, respectively. Considering four factors that affect the fusion of new and old asphalt in the recycled asphalt mixture, namely, gradation type, asphalt content, mixing time, and RAP preheating temperature, the material composition and mixing process parameters of the recycled asphalt mixture are designed. The composition of each parameter is shown in Table 2. The four gradation types in Table 2 are as follows: Figure 4 shown.

[0082]

[0083] Table 2 Design material composition and mixing process parameters of recycled asphalt mixture

[0084] According to the design scheme in Table 2, using Formula 4, it is calculated that the mass proportion of old asphalt contained in the waste asphalt mixture in the recycled asphalt mixture at asphalt contents of 3.7%, 4.0%, 4.3%, and 4.6% is 44.3%, 40.8%, 37.9%, and 35.3% of the total asphalt, respectively.

[0085] Formula 4:

[0086]

[0087] In the formula, x RAPC is the mass ratio of old asphalt to total asphalt in recycled asphalt mixture; RHMA P is the designed asphalt content of recycled asphalt mixture; RAPi is the proportion of waste asphalt mixture of size i in recycled asphalt mixture; C RAPi is the content of old asphalt in the waste asphalt mixture of size i; n is the number of sizes of waste asphalt mixture in the recycled asphalt mixture;

[0088] Step S03: There are three types of cubic artificial aggregates used in the mixing process of the recycled asphalt mixture. The cubic artificial aggregate is limestone, and the limestone aggregates with cube sizes of 13.2±0.5mm, 16.0±0.5mm, and 19.0±0.5mm are obtained by cutting;

[0089] The composition of the recycled asphalt mixture includes waste asphalt mixture, new aggregate, SBS modified asphalt, and mineral powder. The four materials need to be heated to the designed preheating temperature before mixing. The preheating temperature of the waste asphalt mixture is shown in Table 2, and the preheating temperatures of the new aggregate, SBS modified asphalt, and mineral powder are 195°C, 170°C, and 170°C, respectively. After the different materials are heated to the designed preheating temperature, the recycled asphalt mixture is mixed. The mixing process of the recycled asphalt mixture is to first mix the waste asphalt mixture, then add new aggregate and new asphalt to mix, and finally add mineral powder to mix, so as to obtain the recycled asphalt mixture. The mixing time of the three stages is the same, and the total time is controlled according to the design scheme. The total mixing time used in this embodiment is 60s, 120s, 150s, and 180s, respectively, corresponding to the mixing time of each stage of 20s, 40s, 50s, and 60s, respectively.

[0090] The designed total mixing mass of the recycled asphalt mixture is 5000g, and 100g±10g of the three types of cubic limestone artificial aggregates are used in each scheme of this embodiment, and the total added mass of the cubic limestone artificial aggregates is 300g±30g.

[0091] After three stages of mixing, the recycled asphalt mixture is obtained. The cross-sectional thermal images of the recycled asphalt mixtures with different design schemes are collected using an infrared thermal imager. Taking the implementation scheme 1 in Table 2 as an example, the thermal imaging results are as follows: Figure 5 shown.

[0092] After the thermal images were collected, cubic tracer aggregates of mixed asphalt formed by mixing new asphalt and old asphalt wrapped in recycled asphalt mixtures of different design schemes were obtained in situ by manual selection.

[0093] Step S04: Use extraction and rotary evaporation to recover the mixed asphalt on the surface of the asphalt-coated cubic tracer aggregate of different design schemes, and use the same infrared spectrum test conditions as in step S01 to obtain the infrared spectrum of the mixed asphalt at 4000-400 cm-1. Use formula 1 in step S01 to calculate the carbonyl index I of the mixed asphalt on the surface of the tracer aggregate C=O , and the relationship equation between the old asphalt ratio and the carbonyl index obtained in step S01 is used (I C=O =1.4307×10 -4 × i +8.8980×10 -5 ), calculate the proportion of old asphalt in the mixed asphalt, and obtain the mixed asphalt proportion results of 16 design schemes, see Table 3.

[0094] Trial plan Carbonyl Index Old asphalt ratio / % Trial plan Carbonyl Index Old asphalt ratio / % 1 0.00314 21.33 9 0.00439 30.04 2 0.00428 29.27 10 0.00436 29.82 3 0.00389 26.54 11 0.00416 28.48 4 0.00441 30.20 12 0.00417 28.55 5 0.00436 29.87 13 0.00467 32.03 6 0.00385 26.32 14 0.00498 34.21 7 0.00456 31.25 15 0.00366 24.98 8 0.00458 31.42 16 0.00537 36.93

[0095] Table 3 Calculation results of the proportion of mixed asphalt on the surface of tracer aggregate

[0096] According to the calculation results of the mixed asphalt ratio on the surface of the tracer aggregate obtained in Table 3, combined with the mass ratio of old asphalt to total asphalt in the recycled asphalt mixture x RAP Formula 5 is used to calculate the fusion degree BD of new and old asphalt in the recycled asphalt mixture after the hot mixing process. The results are shown in Table 4.

[0097] Formula 5:

[0098]

[0099] In the formula, x a is the calculated value of the proportion of old asphalt in the mixed asphalt; x RAP It is the calculated value of the mass ratio of old asphalt to total asphalt in the recycled asphalt mixture;

[0100]

[0101] Table 4 Calculation results of the fusion degree of new and old asphalt in recycled asphalt mixture after hot mixing in different test schemes

[0102] Step S05: Analyze the infrared thermal imager to analyze the temperature distribution characteristics of the regenerated asphalt mixture cross section in the 16 test schemes in Table 2. Taking test scheme 1 in Table 2 as an example, the data in the infrared thermal imager are analyzed to obtain the statistical results of the temperature distribution of the regenerated asphalt mixture cross section in test scheme 1. Figure 6 shown.

[0103] By testing the specific heat capacity of SBS modified asphalt and aggregate used in this scheme, the specific heat capacity of SBS modified asphalt is 1.763 kJ / kg·℃, and the specific heat capacity of limestone aggregate is 0.92 kJ / kg·℃. The heating temperature of waste asphalt mixture in recycled asphalt mixture is shown in Table 2. The preheating temperatures of new aggregate, SBS modified asphalt and mineral powder are 195℃, 170℃ and 170℃ respectively.

[0104] According to the ratio of waste asphalt mixture, new aggregate and SBS modified asphalt in the recycled asphalt mixture, taking 5000g recycled asphalt mixture as an example, the theoretical temperature T that different materials in the recycled asphalt mixture can reach when in contact with each other is calculated using Formula 6. f , which is the temperature threshold, and the calculation results of the temperature thresholds of 16 test schemes are shown in Table 5. In the calculation process, the waste asphalt mixture is a mixture of old asphalt and aggregate. In the process of calculating the temperature threshold, the mass ratios of old asphalt and aggregate are considered respectively.

[0105] Formula 6:

[0106]

[0107] Where, T f C is the theoretical temperature that can be reached after different materials in the recycled asphalt mixture are mixed together; i is the specific heat capacity of the i-th material in the recycled asphalt mixture; m i is the usage quality of material i in recycled asphalt mixture; T i is the initial mixing temperature of material i in the recycled asphalt mixture;

[0108]

[0109]

[0110] Table 5 Temperature threshold calculation results

[0111] According to the temperature threshold calculation results in Table 5, combined with the temperature distribution statistics of the cross-sectional temperature image after hot mixing of the recycled asphalt mixture obtained by the infrared thermal imager, the temperature distribution of the cross-sectional temperature image less than the temperature threshold T is calculated using Formula 7. f The proportion of the number of pixels, that is, the area proportion of the low temperature area in the thermal image P T , the results are shown in Table 6.

[0112] Formula 7:

[0113]

[0114] Where P T T is the area ratio of low temperature area in the thermal imaging image of the recycled asphalt mixture cross section;min T is the lowest temperature in the thermal imaging image of the recycled asphalt mixture cross section; f T is the theoretical temperature that can be reached after different materials in the recycled asphalt mixture are mixed together; max The highest temperature in the thermal imaging image of the recycled asphalt mixture cross section; N i is the number of pixels corresponding to temperature i in the thermal imaging image of the recycled asphalt mixture cross section;

[0115]

[0116]

[0117] Table 6 Area proportion of low temperature area in thermal imaging

[0118] Step S06: In this embodiment, 16 test schemes are designed as shown in Table 2. The cubic aggregate tracing method is used to obtain mixed asphalt of different schemes and infrared thermal images of in-situ tests. The degree of fusion of new and old asphalt and the area ratio of low-temperature areas in the thermal images are calculated. The results are shown in Tables 4 and 6, respectively. A data set of the degree of fusion of new and old asphalt and the area ratio of low-temperature areas in the thermal images is constructed.

[0119] Step S07: Based on the data set of the fusion degree of new and old asphalt and the low temperature area ratio in the thermal image obtained by in-situ measurement in Table 4 and Table 6, the change trend of the fusion degree of new and old asphalt and the low temperature area ratio in the thermal image obtained by in-situ measurement is as follows: Figure 7 It can be seen that there is a significant correlation between the degree of fusion of new and old asphalt and the proportion of low-temperature areas in the thermal image obtained by in-situ measurement.

[0120] Using the relational modeling module, taking the linear model as an example, a linear model of the proportion of low-temperature areas and the degree of fusion of new and old asphalt is constructed as follows:

[0121] Y BD =-15.033x PT +152.58

[0122] Where Y BD is the degree of fusion of new and old asphalt in recycled asphalt mixture; x PT The area ratio of low temperature area in the thermal image of the cross-section temperature of recycled asphalt mixture;

[0123] The goodness of fit of the linear model is 0.88, indicating that there is a significant linear relationship between the proportion of the low-temperature area and the degree of fusion of the new and old asphalt. The linear model can be used to characterize the relationship between the proportion of the low-temperature area and the degree of fusion of the new and old asphalt.

[0124] Step S08: Using the waste asphalt mixture, SBS modified asphalt, new aggregate, and tracer artificial aggregate used in the present invention, 6 groups of test schemes are designed as shown in Table 7 to verify the accuracy of the linear model in predicting the degree of fusion of new and old asphalt in the recycled asphalt mixture. In the 6 groups of test schemes, the preheating temperatures of the waste asphalt mixture, SBS modified asphalt, new aggregate (tracer artificial aggregate), and mineral powder are 130°C, 195°C, 170°C, and 170°C, respectively, to prepare 5000g of recycled asphalt mixture, collect thermal images of the cross-section of the recycled asphalt mixture in the 6 groups of test schemes, and obtain the artificial aggregate wrapped with new and old asphalt in situ.

[0125] Trial plan Gradation type Asphalt content / % Mixing time / s 1 Grading Ⅰ 4.0 60 2 Grading ⅠⅠ 4.0 120 3 Grading ⅠⅠⅠⅠ 4.0 150 4 Grading IV 4.0 180 5 Grading ⅠⅠ 4.3 150 6 Grading ⅠⅠ 4.3 150

[0126] Table 7 Test scheme for recycled asphalt mixture

[0127] According to the composition of recycled asphalt mixture in 6 test schemes, the temperature threshold of the recycled asphalt mixture section under ideal conditions is calculated, and the area proportion of the low-temperature area below the temperature threshold in the thermal imaging image is calculated.

[0128] According to the area ratio of the low-temperature area below the temperature threshold in the thermal imaging image, the relationship model (Y BD =-15.033x PT +152.58), and the predicted values ​​of the fusion degree of new and old asphalt in the recycled asphalt mixture during the hot mix process of the six test schemes were obtained. The results are shown in Table 7.

[0129]

[0130]

[0131] Table 7 Test scheme for recycled asphalt mixture

[0132] To verify the accuracy of the prediction results, the artificial aggregate wrapped with new and old asphalt obtained in situ was used to obtain mixed asphalt by extraction and rotary evaporation. The same infrared spectrum test conditions as in step S01 were used to obtain the infrared spectrum of the mixed asphalt at 4000-400 cm-1. The carbonyl index I of the mixed asphalt on the surface of the tracer aggregate was calculated using formula 1 in step S01. C=O , and the relationship equation between the old asphalt ratio and the carbonyl index obtained in step S01 is used (I C=O =1.4307×10 -4 × i +8.8980×10 -5 ), calculate the proportion of old asphalt in the mixed asphalt, and use the BD calculation formula for the fusion degree of new and old asphalt in the recycled asphalt mixture in step S04 to obtain the actual values ​​of the fusion degree of new and old asphalt in the 6 test schemes.

[0133] The actual values ​​of the fusion degree of the new and old asphalt in the six test schemes are compared with the predicted values ​​in Table 7, and the comparison results are shown in Table 8. It can be seen that the difference between the predicted values ​​and the actual values ​​is small.

[0134] Trial plan Prediction of the degree of fusion between new and old asphalt / % Actual value of the degree of fusion between new and old asphalt / % 1 63.3 65.1 2 75.6 74.2 3 82.7 82.4 4 89.4 88.6 5 85.1 87.9 6 85.1 86.4

[0135] Table 8 Comparison of predicted and actual values ​​of fusion degree in the recycled asphalt mixture test scheme

[0136] According to the comparison results between the predicted value and the actual value of the fusion degree of the new and old asphalt in the recycled asphalt mixture in Table 8, it is shown that the fusion degree of the new and old asphalt in the recycled asphalt mixture can be indirectly characterized by the proportion of the low-temperature area in the cross-sectional temperature distribution of the recycled asphalt mixture. By constructing a relationship model between the fusion degree of the new and old asphalt and the proportion of the low-temperature area, and collecting the cross-sectional temperature thermal image of the recycled asphalt mixture, the fusion degree of the recycled asphalt mixture can be predicted in real time, and the fusion degree of the new and old asphalt can be quantitatively characterized.

[0137] By adopting the method and system for evaluating the degree of fusion of new and old asphalt in the regenerated asphalt mixture in real time during hot mixing, the degree of fusion of new and old asphalt in the regenerated asphalt mixture can be tested in real time during the production of the regenerated asphalt mixture. The cross-sectional thermal image of the regenerated asphalt mixture is obtained by an infrared thermal imager, and the prediction result of the degree of fusion of new and old asphalt in the regenerated asphalt mixture is obtained in combination with the method and system proposed in the present invention, providing a rapid decision-making basis for the production quality control and process parameter adjustment of the regenerated asphalt mixture.

[0138] Those skilled in the art will appreciate that the embodiments of the present application may be provided as methods, systems or computer program products. Therefore, the present application may take the form of a complete hardware embodiment, a complete software embodiment, or an embodiment combining software and hardware.

[0139] The above are only embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.

Claims

1. A method for evaluating the degree of fusion of recycled asphalt mixture in a hot mix process, characterized in that: The following steps are involved: The infrared spectra of completely mixed asphalt with different ratios of new and old asphalt are obtained by infrared spectrometer, the carbonyl index is calculated, and a linear relationship equation between the ratio of old asphalt and the carbonyl index is constructed; The content of old asphalt in the waste asphalt mixture is tested by extraction method, and the mass proportion of old asphalt in the recycled asphalt mixture is calculated; An infrared thermal imager is used to collect the cross-sectional temperature image of the recycled asphalt mixture after hot mixing to obtain temperature distribution data; The mixed asphalt on the surface of the cube tracer aggregate was recovered by extraction and rotary evaporation, the carbonyl index was calculated by infrared spectroscopy, and the proportion of old asphalt in the mixed asphalt was calculated based on the linear relationship equation. According to the heat transfer model between materials, the theoretical temperature values ​​reached by different materials during hot mixing are calculated as the temperature threshold; Taking the temperature threshold as the standard, the percentage of pixels below the threshold in the temperature image of the recycled asphalt mixture cross section is calculated to obtain the area percentage of the low temperature area. Based on the data set of the degree of fusion of new and old asphalt and the proportion of low-temperature areas in thermal images, a relationship model between the two was constructed and a linear regression analysis was performed; Based on the thermal image acquisition results and the low-temperature area ratio relationship model, the fusion degree of new and old asphalt in the recycled asphalt mixture is calculated and evaluated.

2. The method for evaluating the degree of fusion of recycled asphalt mixture in hot mix process according to claim 1, characterized in that: The calculation method of the carbonyl index includes: Obtain the infrared spectrum of the completely mixed asphalt through an infrared spectrum tester; Carbonyl Index I C=O The calculation is as follows: Among them, A C=O is the area of ​​the carbonyl functional group region; A Referance is the area of ​​the reference functional group region.

3. The method according to claim 1, characterized in that The mass proportion of old asphalt in recycled asphalt mixture is calculated by the following formula: Among them, x RAP is the mass ratio of old asphalt to total asphalt; C RHMA P is the designed asphalt content of recycled asphalt mixture; RAPi is the usage ratio of the i-th size waste asphalt mixture; C RAPi is the content of old asphalt in the i-th size waste asphalt mixture.

4. The method according to claim 2, characterized in that: The proportion of old asphalt in the mixed asphalt on the surface of the cube tracer aggregate x i The calculation is based on the carbonyl index I C=O , determined by the following relational expression: I C=O =a×x i +b Among them, x i is the proportion of old asphalt in the fully mixed asphalt; a and b are the specific values ​​of the constant terms in the linear regression model.

5. The method according to claim 1, characterized in that The theoretical temperature value T f Calculated by the following formula: Among them, T f It is the theoretical value of the temperature that can be reached after the materials in the recycled asphalt mixture are mixed with each other; C i is the specific heat capacity of the i-th material; m i is the quality of the i-th material; T i is the initial mixing temperature of the ith material.

6. The method according to claim 1, characterized in that Low temperature area ratio P T Calculated by the following formula: Among them, P T T is the area ratio of low temperature area in the thermal imaging image of the recycled asphalt mixture cross section; min T is the lowest temperature in the thermal imaging image of the recycled asphalt mixture cross section; f T is the theoretical temperature that can be reached after different materials in the recycled asphalt mixture are mixed together; max N is the highest temperature in the thermal imaging image of the recycled asphalt mixture cross section; i is the number of pixels corresponding to temperature i in the thermal imaging image of the recycled asphalt mixture cross section.

7. The method according to claim 1, characterized in that The degree of integration of new and old asphalt constructed Y BD The proportion of low temperature area x PT The relationship model is expressed by the following linear regression equation: AND BD =d×x PT +e Among them, Y BD is the calculated value of the mixing degree in the recycled asphalt mixture; x PT is the area ratio of low temperature area in the cross-sectional temperature image obtained by infrared thermal imager during the mixing process of recycled asphalt mixture; d and e are the specific values ​​of constant terms in the linear regression model.

8. The method according to claim 1, characterized in that The test environment conditions of the infrared spectrum tester include: the test environment temperature is 25℃±0.5℃, the test resolution is 4cm -1 , the background and sample scan times were 32 times, and the wave number range was 4000cm -1 Up to 400cm -1 .

9. The method according to claim 1, characterized in that: The infrared thermal imager is used to collect the cross-sectional temperature image of the recycled asphalt mixture in real time, and process it through the thermal image data analysis module to determine the area proportion of the low-temperature area.

10. A system for implementing the method for evaluating the degree of fusion of recycled asphalt mixture in a hot mix process according to any one of claims 1 to 9, characterized in that: include: Infrared spectrum test module, used to obtain infrared spectra of completely mixed asphalt with different ratios of new and old asphalt, calculate the carbonyl index, and construct a linear relationship equation between the ratio of old asphalt and the carbonyl index; The extraction analysis module is used to test the content of old asphalt in the waste asphalt mixture by extraction method and calculate the mass proportion of old asphalt in the recycled asphalt mixture; Infrared thermal imaging module, used to collect cross-sectional temperature images of recycled asphalt mixture after hot mixing to obtain temperature distribution data; The tracer recovery module recovers the mixed asphalt on the surface of the cube tracer aggregate by extraction and rotary evaporation, calculates the carbonyl index by infrared spectroscopy, and calculates the proportion of old asphalt in the mixed asphalt based on a linear relationship equation; The temperature calculation module calculates the theoretical temperature values ​​reached by different materials during the hot mixing process as the temperature threshold according to the heat transfer model between the materials; The area analysis module uses the temperature threshold as the standard to calculate the percentage of pixels below the threshold in the temperature image of the recycled asphalt mixture cross section, and obtains the area percentage of the low-temperature area; The relationship modeling module builds a relationship model between the two based on the data set of the degree of integration of new and old asphalt and the proportion of low-temperature areas in thermal images, and performs linear regression analysis; The fusion degree evaluation module calculates and evaluates the fusion degree of new and old asphalt in the recycled asphalt mixture based on the thermal image acquisition results and the low-temperature area ratio relationship model.

Citation Information

Patent Citations

  • Recycled asphalt mixture design method based on new and old asphalt fusion degree model

    CN111268942A

  • Method for calculating effective rate of old asphalt based on infrared spectrum

    CN116893151A

  • New and old asphalt fusion effect quantitative evaluation method

    CN117191867A