Preparation method of neodymium-iron-boron magnet

Through the preparation methods of neodymium iron boron magnets, including smelting, hydrogen breaking, crushing, sintering and praseodymium copper alloy treatment, the grain boundary structure is optimized, and the problem of low coercivity of neodymium iron boron magnets is solved, and the coercivity of magnets is realized. promote.

CN119008212AInactive Publication Date: 2024-11-22AAC KAITAI TECHNOLOQIES (MAANSHAN) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410962781.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN119008212A_ABST
    Figure CN119008212A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a neodymium-iron-boron magnet. The preparation method comprises the following steps: obtaining a neodymium-iron-boron magnet raw material; a neodymium-iron-boron magnet raw material is subjected to smelting treatment to obtain a rapid hardening sheet; performing hydrogen decrepitation treatment on the rapid hardening sheet to obtain coarse magnetic powder; crushing the coarse magnetic powder to obtain fine magnetic powder; pressing the fine magnetic powder into a magnet green body; the magnet green body is put into a sintering furnace to be sintered, and sintered neodymium iron boron is obtained; spraying the praseodymium-copper alloy mixture on the surface of the sintered neodymium iron boron to obtain an intermediate; the intermediate is put into a tempering furnace to be subjected to high-temperature diffusion treatment, and a second intermediate is obtained; tempering the second intermediate in a tempering furnace; and discharging to obtain the neodymium-iron-boron magnet. Compared with the prior art, the method has the advantages that the grain boundary structure is optimized, the exchange coupling effect of the main phase is reduced, and the coercive force of the neodymium-iron-boron magnet can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to NdFeB magnet material technology, and in particular to a method for preparing a NdFeB magnet. [Background technology]

[0002] NdFeB magnet is a man-made permanent magnet and the strongest permanent magnet in the existing technology. Its maximum magnetic energy product (BHmax) is more than 10 times higher than that of ferrite. In the state of bare magnet, its magnetic force can reach about 3500 Gauss. NdFeB magnet has the characteristics of high cost performance, small size, light weight, good mechanical properties and strong magnetism. It is widely used in electric vehicles, hybrid vehicles, wind power generation, variable frequency air conditioners, medical equipment, elevators, audio equipment and mineral sorting.

[0003] The finished product obtained by the existing NdFeB magnet preparation method has uneven distribution of grain boundary phase, agglomeration of Nd-rich phase in some areas, and low coercive force of the magnet.

[0004] Therefore, it is necessary to propose a new method for preparing NdFeB magnets to solve the above problems. [Summary of the invention]

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a NdFeB magnet capable of improving the coercive force of the magnet.

[0006] In order to solve the above technical problems, the present invention provides a method for preparing a neodymium iron boron magnet, the preparation method comprising the following steps:

[0007] Obtaining raw materials of NdFeB magnets;

[0008] The raw materials of NdFeB magnets are smelted to obtain quick-setting sheets;

[0009] The quick-setting sheet is subjected to hydrogen rupture treatment to obtain coarse magnetic powder;

[0010] The coarse magnetic powder is crushed to obtain fine magnetic powder;

[0011] Processing fine magnetic powder into a magnet green body by pressing;

[0012] The green magnet is placed in a sintering furnace for sintering to obtain sintered NdFeB;

[0013] Spraying the praseodymium-copper alloy mixture onto the surface of the sintered NdFeB to obtain an intermediate;

[0014] placing the intermediate into a tempering furnace for high temperature diffusion treatment to obtain a second intermediate;

[0015] tempering the second intermediate in a tempering furnace;

[0016] Take it out of the furnace and get the NdFeB magnet.

[0017] Preferably, the raw materials of the NdFeB magnets are configured according to mass as follows:

[0018] Nd 30.2 Fe bal B 1.0 Al 0.8 Cu 0.2 Ga 0.45 Zr 0.15 .

[0019] Preferably, the praseodymium-copper alloy mixture is prepared by adding praseodymium-copper alloy powder into polyethylene glycol and stirring the mixture thoroughly.

[0020] Preferably, the process of high temperature diffusion treatment is specifically as follows:

[0021] Set the temperature to 860°C and keep it for 16 hours, then cool it to room temperature.

[0022] Preferably, the tempering process is specifically as follows:

[0023] Set the temperature to 550°C and keep it for 5 hours, then cool it to room temperature.

[0024] Compared with the related art, the preparation method of the NdFeB magnet of the present invention includes the following steps: obtaining raw materials of NdFeB magnet; subjecting the raw materials of NdFeB magnet to smelting treatment to obtain quick-setting sheets; subjecting the quick-setting sheets to hydrogen cracking treatment to obtain coarse magnetic powder; subjecting the coarse magnetic powder to crushing treatment to obtain fine magnetic powder; subjecting the fine magnetic powder to pressing treatment to form a magnet green body; placing the magnet green body into a sintering furnace for sintering treatment to obtain sintered NdFeB; spraying a praseodymium-copper alloy mixture onto the surface of the sintered NdFeB to obtain an intermediate; placing the intermediate into a tempering furnace for high-temperature diffusion treatment to obtain a second intermediate; tempering the second intermediate in the tempering furnace; and taking out of the furnace to obtain a NdFeB magnet. Compared with the related art, the present invention realizes the entry of praseodymium-copper elements into the grain boundary phase of NdFeB through the combination of high-temperature diffusion and tempering treatment technology, optimizes the grain boundary structure, reduces the exchange coupling effect of the main phase, and can improve the coercive force of the NdFeB magnet.

Brief Description of the Drawings

[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:

[0026] Figure 1 It is a flowchart of the steps of the method for preparing a NdFeB magnet provided by an embodiment of the present invention. [Specific implementation method]

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] See also Figure 1 As shown, Figure 1 The present invention provides a method for preparing a NdFeB magnet, which comprises the following steps:

[0029] S1. Obtaining raw materials of NdFeB magnets;

[0030] S2, smelting the raw materials of NdFeB magnets to obtain quick-setting sheets; this step is carried out in a smelting furnace;

[0031] S3, subjecting the quick-setting sheet to hydrogen rupture treatment to obtain coarse magnetic powder; this step is carried out in a hydrogen rupture furnace;

[0032] S4, crushing the coarse magnetic powder to obtain fine magnetic powder; this step is carried out in a jet mill;

[0033] S5, processing the fine magnetic powder into a magnet green body by pressing; this step is performed in a press;

[0034] S6, placing the magnet green body into a sintering furnace for sintering to obtain sintered NdFeB;

[0035] S7, spraying the praseodymium-copper alloy mixture onto the surface of the sintered NdFeB to obtain an intermediate;

[0036] S8, placing the intermediate into a tempering furnace for high temperature diffusion treatment to obtain a second intermediate;

[0037] S9, tempering the second intermediate in a tempering furnace;

[0038] S10, taking out of the furnace to obtain a NdFeB magnet.

[0039] The raw materials of the NdFeB magnets are configured according to quality as follows:

[0040] Nd 30.2 Fe bal B 1.0 Al 0.8 Cu 0.2 Ga 0.45 Zr 0.15During the implementation process, the weight ratio of raw materials is accurately obtained through electronic scales and other weighing methods.

[0041] The praseodymium-copper alloy mixture is prepared by adding praseodymium-copper alloy powder into polyethylene glycol and stirring the mixture thoroughly.

[0042] The specific process of high temperature diffusion treatment is as follows:

[0043] Set the temperature to 860°C and keep it for 16 hours, then cool it to room temperature.

[0044] The specific process of tempering treatment is as follows:

[0045] The temperature is set at 550℃ and kept for 5 hours, then cooled to room temperature. Through the sequential treatment of high-temperature diffusion and tempering, the praseodymium-copper elements on the surface of sintered NdFeB can enter the NdFeB grain boundary phase, thereby optimizing the grain boundary structure of the magnet.

[0046] Compared with the related art, the preparation method of the NdFeB magnet of the present invention includes the following steps: obtaining raw materials of NdFeB magnet; subjecting the raw materials of NdFeB magnet to smelting treatment to obtain quick-setting sheets; subjecting the quick-setting sheets to hydrogen cracking treatment to obtain coarse magnetic powder; subjecting the coarse magnetic powder to crushing treatment to obtain fine magnetic powder; subjecting the fine magnetic powder to pressing treatment to form a magnet green body; placing the magnet green body into a sintering furnace for sintering treatment to obtain sintered NdFeB; spraying a praseodymium-copper alloy mixture onto the surface of the sintered NdFeB to obtain an intermediate; placing the intermediate into a tempering furnace for high-temperature diffusion treatment to obtain a second intermediate; tempering the second intermediate in the tempering furnace; and taking out of the furnace to obtain a NdFeB magnet. Compared with the related art, the present invention realizes the entry of praseodymium-copper elements into the grain boundary phase of NdFeB through the combination of high-temperature diffusion and tempering treatment technology, optimizes the grain boundary structure, reduces the exchange coupling effect of the main phase, and can improve the coercive force of the NdFeB magnet.

[0047] The above description is only an implementation mode of the present invention. It should be pointed out that, for ordinary technicians in this field, improvements can be made without departing from the creative concept of the present invention, but these all belong to the protection scope of the present invention.

Claims

1. A method for preparing a neodymium iron boron magnet, characterized in that: The preparation method comprises the following steps: Obtaining raw materials of NdFeB magnets; The raw materials of NdFeB magnets are smelted to obtain quick-setting sheets; The quick-setting sheet is subjected to hydrogen rupture treatment to obtain coarse magnetic powder; The coarse magnetic powder is crushed to obtain fine magnetic powder; Processing fine magnetic powder into a magnet green body by pressing; The green magnet is placed in a sintering furnace for sintering to obtain sintered NdFeB; Spraying the praseodymium-copper alloy mixture onto the surface of the sintered NdFeB to obtain an intermediate; placing the intermediate into a tempering furnace for high temperature diffusion treatment to obtain a second intermediate; tempering the second intermediate in a tempering furnace; Take it out of the furnace and get the NdFeB magnet.

2. The method for preparing a NdFeB magnet according to claim 1, wherein: The raw materials of the NdFeB magnets are configured by mass as follows: Nd 30.2 Fe bal B 1.0 Al 0.8 The 0.2 Won't 0.45 Zr 0.15 。 3. The method for preparing a NdFeB magnet according to claim 1, characterized in that: The praseodymium-copper alloy mixture is prepared by adding praseodymium-copper alloy powder into polyethylene glycol and stirring the mixture thoroughly.

4. The method for preparing a NdFeB magnet according to claim 1, characterized in that: The specific process of high temperature diffusion treatment is as follows: Set the temperature to 860°C and keep it for 16 hours, then cool it to room temperature.

5. The method for preparing a NdFeB magnet according to claim 1, characterized in that: The specific process of tempering treatment is as follows: Set the temperature to 550°C and keep it for 5 hours, then cool it to room temperature.

Citation Information

Patent Citations

  • Method for preparing high coercive force, high corrosion resistance magnet by nanocopper

    CN101090013A

  • Method for improving magnetic performance of sintered neodymium iron boron magnet

    CN105489367A

  • Grain boundary diffusion method for preparing high-performance special-shaped neodymium-iron-boron magnet

    CN115116728A

  • Sintered neodymium iron boron permanent magnet and preparation method thereof

    CN115798910A

  • Low-neodymium, non-heavy-rare-earth and high performance magnet and preparation method

    US20130154778A1