Starch-based hard carbon negative electrode material and preparation method and application thereof

Starch-based hard carbon anode material prepared by treating corn starch with melamine crosslinking agent, combined with activated carbon cathode, solves the problem of anode-cathode mismatch in hybrid supercapacitors, realizing a hybrid lithium-ion supercapacitor with high energy and high power density.

CN119008253APending Publication Date: 2024-11-22CHINA UNIV OF GEOSCIENCES (WUHAN)
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411167641.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In existing hybrid supercapacitors, the kinetic mismatch between the anode and cathode leads to low power density, and existing crosslinking agents such as maleic anhydride are expensive and cannot improve the specific capacity of biomass hard carbon.

Method used

Using melamine as a crosslinking agent, starch-based hard carbon anode material was prepared by esterification of corn starch followed by carbonization at 900-1300℃. Combined with activated carbon as the cathode material, a hybrid lithium-ion supercapacitor was constructed.

Benefits of technology

This technology enables rapid and efficient lithium-ion transport, improves the lithium storage capacity and electrochemical stability of materials, enhances the matching between the anode and cathode, and increases the energy and power density of hybrid supercapacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008253A_ABST
    Figure CN119008253A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of hard carbon materials, in particular to a starch-based hard carbon negative electrode material and a preparation method and application thereof. According to the invention, the corn starch with a spherical structure is used as a precursor, melamine is introduced as a cross-linking agent for esterification, and starch-based hard carbon is finally obtained after carbonization, so that large-capacity storage of lithium ions is realized, reaction kinetics is promoted at the same time, and the performance of the lithium ion battery is improved. The starch-based hard carbon negative electrode material prepared by the invention shows large lithium ion storage capacity and good charge / discharge rate in a wide potential window. In addition, the hybrid lithium ion supercapacitor with high energy density and power density is assembled by taking the lithium ion battery as an anode and commercial activated carbon as a cathode. The material realizes the technical breakthrough of high capacity and high rate performance in lithium ion battery negative electrodes and mixed lithium ions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hard carbon materials, and in particular to a starch-based hard carbon negative electrode material and a preparation method and application thereof. Background Art

[0002] Hybrid supercapacitors are popular because they combine the advantages of high energy storage of lithium-ion batteries with the fast charge and discharge of supercapacitors. However, since its inception, the combination of a high-capacity anode that can reversibly embed lithium ions with a carbon-based fast-rate capacitor cathode has been an important direction of its development. Several recent studies on hybrid supercapacitors have reported high energy storage of up to 150–200 Whkg -1 The high energy density of hybrid supercapacitors is a huge leap forward compared to supercapacitors. Nevertheless, hybrid supercapacitors still face the problem of being able to maintain high energy density only at low power density. This is due to the kinetic mismatch between slow lithium insertion in the anode and rapid ion adsorption at the cathode / electrolyte interface. Therefore, improving the anode lithium storage rate to shorten the kinetic gap is an important issue in improving the power density of hybrid supercapacitors.

[0003] Hard carbon is one of the most promising negative electrode materials for lithium-ion batteries because of its stable structure, excellent conductivity and easy processing. It also has excellent cycle performance at high current density and has become a popular choice for negative electrode materials for lithium-ion batteries. Starch is a low-cost, easily available, green and pollution-free biomass hard carbon that has been widely studied and applied. Among all biomass precursors, starch as a precursor has the highest degree of control over the microstructure, morphology and properties of the final hard carbon. Compared with other biomass precursors, starch exhibits an original natural spherical morphology, which makes it one of the most advantageous candidate materials for the preparation of spherical carbon materials. However, direct carbonization of starch easily leads to the rupture of the starch sphere morphology and low compaction density. Therefore, it is necessary to provide a means to maintain the starch sphere morphology and improve its lithium storage performance. During the heat treatment process, the introduction of the crosslinking agent promotes the effective connection of the aromatic units inside the starch. This highly crosslinked nanostructure not only keeps the final hard carbon in a good spherical morphology. The research and development of crosslinking agents has brought bright prospects for the application of starch in the negative electrode of lithium-ion batteries.

[0004] In the prior art, maleic anhydride is often used as a cross-linking agent. However, the maleic anhydride cross-linking agent has a high raw material cost and cannot play a role in improving the limited specific capacity of biomass hard carbon. Summary of the invention

[0005] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and to provide a starch-based hard carbon negative electrode material and a preparation method and application thereof.

[0006] The invention discloses a method for preparing a starch-based hard carbon negative electrode material. Corn starch is esterified with melamine and then carbonized to obtain the starch-based hard carbon negative electrode material.

[0007] Furthermore, the carbonization temperature is 900-1300° C., and the carbonization time is 1-8 hours.

[0008] Furthermore, the heating rate of carbonization is 1 to 10°C / min.

[0009] Furthermore, the specific operation of esterifying corn starch with melamine is: vacuum drying the corn starch, and then hydrothermally reacting it with melamine to obtain esterified starch.

[0010] Furthermore, the mass ratio of corn starch to melamine is 4:1.

[0011] Furthermore, the hydrothermal reaction temperature is 50-150°C.

[0012] A starch-based hard carbon negative electrode material prepared by the above-mentioned preparation method.

[0013] An application of the starch-based hard carbon negative electrode material as described above is applied to the negative electrode of a lithium-ion battery and the anode of a hybrid lithium-ion supercapacitor.

[0014] A hybrid lithium-ion supercapacitor adopts the above-mentioned starch-based hard carbon negative electrode material as the negative electrode active material to prepare the negative electrode, and activates it; adopts activated carbon material as the positive electrode active material to prepare the positive electrode sheet, adopts the above-mentioned activated starch-based hard carbon negative electrode as the anode, and adopts the positive electrode prepared by activated carbon as the cathode to assemble into a hybrid lithium-ion supercapacitor.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] (1) The cross-linked spherical structure of esterified starch promotes the + The present invention uses melamine as a cross-linking agent to achieve nitrogen doping to provide additional active sites and enhance lithium storage capacity. In addition, the wide working potential (0–3V vs Li / Li + ) and its capacitive properties can achieve high reversible capacity.

[0017] (2) The starch-based hard carbon material prepared by the present invention has uniform particles, and the spherical structure of corn starch remains stable and interconnected after esterification. The introduction of melamine cross-linking agent effectively inhibits the volume expansion of esterified starch during the carbonization process.

[0018] (3) The starch-based hard carbon material prepared by the present invention has a wide potential window (relative to Li / Li +It exhibits a large lithium-ion storage capacity (375.4 mAh g) within 0–3 V. -1 ) and good charge / discharge rate. During the cycle test, the low polarization of the negative electrode and the minimal morphological structure change promoted its electrochemical stability, and the capacity retention rate was still above 90% after 100 cycles. This material has achieved a technological breakthrough in the negative electrode of lithium-ion batteries with high capacity and high rate performance. In addition, the starch-based hard carbon anode and the commercial activated carbon cathode were assembled into a hybrid lithium-ion supercapacitor. The good matching of the anode and the cathode realized the large-capacity storage of lithium ions and promoted the reaction kinetics.

[0019] (4) The material has good electronic conductivity, high lithium storage capacity, small volume change, large specific surface area, uniform particles, and excellent rate and cycle performance. It is suitable for lithium-ion battery negative electrodes and hybrid lithium-ion supercapacitor anodes.

[0020] (5) The present invention uses starch-based hard carbon material as the anode and activated carbon as the cathode to construct a hybrid lithium-ion supercapacitor with both high energy density and high power density, solving the problem of mismatch between the positive and negative electrodes and providing a new idea for the research and application of hybrid supercapacitors. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the SEM image of the starch-based hard carbon negative electrode material prepared in Example 2.

[0022] Figure 2 XRD diagrams of starch-based hard carbon composite graphite negative electrode materials prepared in Examples 1-3 and Comparative Example 1.

[0023] Figure 3 The battery assembled with starch-based hard carbon negative electrode materials prepared in Example 2 (left figure) and Comparative Example 1 (right figure) at a low current density of 25 mA g -1 The charge and discharge curve diagram below.

[0024] Figure 4 The battery assembled with the starch-based hard carbon negative electrode material prepared in Example 2 of the present invention was subjected to a low current density of 25 mA g -1 GCD performance graph below.

[0025] Figure 5 The battery assembled with the starch-based hard carbon composite graphite negative electrode material prepared in Examples 1-3 of the present invention and Comparative Example 1 was subjected to a current density of 0.1 Ag. -1 The following cycle performance comparison chart.

[0026] Figure 6 The batteries assembled from the materials prepared in Examples 1-3 of the present invention and Comparative Example 1 were respectively subjected to a current density of 25 mA g. -1Comparison of the constant current intermittent titration (GITT) curves under lithiation and the calculated diffusion coefficient D during lithiation and delithiation processes.

[0027] Figure 7 CV, GCD and cycle performance diagram of the hybrid lithium-ion supercapacitor assembled in Example 4 of the present invention. DETAILED DESCRIPTION

[0028] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0029] <Example 1>

[0030] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.

[0031] S2. Carbonization: Under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 900°C at a rate of 1-2°C / min, kept at this temperature for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon negative electrode material.

[0032] S3. Preparation of negative electrode: The starch-based hard carbon negative electrode material is used as the negative electrode active material to prepare the negative electrode sheet. The negative electrode material is evenly ground with the conductive agent and the binder in a mass ratio of 8:1:1, and then mixed with N-methylpyrrolidone to prepare the negative electrode slurry, which is coated on the current collector, placed in a vacuum oven at 100°C for 10 hours, and dried and cut into disc-shaped negative electrode sheets.

[0033] S4, half-cell assembly: lithium sheet is used as the counter electrode, and the electrolyte is composed of 1.0 mol LiPF 6 The starch-based negative electrode sheet was prepared in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1), and assembled into a button cell in a glove box under an argon atmosphere.

[0034] <Example 2>

[0035] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.

[0036] S2. Carbonization: Under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1100°C at a rate of 1-2°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon negative electrode material.

[0037] S3. Preparation of negative electrode: The starch-based hard carbon negative electrode material is used as the negative electrode active material to prepare the negative electrode sheet. The negative electrode material is evenly ground with the conductive agent and the binder in a mass ratio of 8:1:1, and then mixed with N-methylpyrrolidone to prepare the negative electrode slurry, which is coated on the current collector, placed in a vacuum oven at 100°C for 10 hours, and dried and cut into disc-shaped negative electrode sheets.

[0038] S4, half-cell assembly: lithium sheet is used as the counter electrode, and the electrolyte is composed of 1.0 mol LiPF 6 The starch-based negative electrode sheet was prepared in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1), and assembled into a button cell in a glove box under an argon atmosphere.

[0039] <Example 3>

[0040] S1. Pretreatment of starch-based raw materials: taking a certain amount of corn starch and putting it into a container, putting the container containing soluble starch into a vacuum drying oven at 50-100° C. for drying for 24 hours, then taking out the container, adding it into a reactor according to a starch to melamine mass ratio of 4:1, and performing dry powder hydrothermal treatment at 50-150° C. to obtain a precursor material, and then crushing it to obtain precursor particles, the precursor particle size is 40-500 mesh.

[0041] S2. Carbonization: Under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1300°C at a rate of 1-2°C / min, kept at this temperature for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon negative electrode material.

[0042] S3. Preparation of negative electrode: The starch-based hard carbon negative electrode material is used as the negative electrode active material to prepare the negative electrode sheet. The negative electrode material is evenly ground with the conductive agent and the binder in a mass ratio of 8:1:1, and then mixed with N-methylpyrrolidone to prepare the negative electrode slurry, which is coated on the current collector, placed in a vacuum oven at 100°C for 10 hours, and dried and cut into disc-shaped negative electrode sheets.

[0043] S4, half-cell assembly: lithium sheet is used as the counter electrode, and the electrolyte is composed of 1.0 mol LiPF 6 The starch-based negative electrode sheet was prepared in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1), and assembled into a button cell in a glove box under an argon atmosphere.

[0044] <Example 4>

[0045] S1. Preparation of positive electrode: commercial activated carbon material is used as the positive electrode active material to prepare the positive electrode sheet. The positive electrode material is evenly ground with the conductive agent and the binder in a mass ratio of 8:1:1, and then mixed with N-methylpyrrolidone to prepare the negative electrode slurry, which is coated on the current collector, placed in a vacuum oven at 100°C for 10 hours, and dried and cut into round positive electrode sheets.

[0046] S2. Activation of the negative electrode: The half-cell assembled in Example 2 was charged and discharged for 5 cycles at a current density of 100 mA / g, and finally discharged to 0 V. The half-cell was disassembled to obtain the activated starch-based hard carbon negative electrode.

[0047] S3. Hybrid lithium-ion supercapacitor assembly: The activated starch-based hard carbon negative electrode is used as the anode, the positive electrode prepared from commercial activated carbon is used as the cathode, and the electrolyte is composed of 1.0 mol LiPF 6 The hybrid lithium-ion supercapacitor was prepared in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1). The above-mentioned electrode was assembled into a hybrid lithium-ion supercapacitor in a glove box under an argon atmosphere.

[0048] <Comparative Example 1>

[0049] S1. Pretreatment of starch-based raw materials: a certain amount of corn starch is put into a container, and the container containing soluble starch is placed in a vacuum drying oven at 50-100°C for 24 hours. Then, the container is taken out, and the starch and maleic anhydride mass ratio is 5:1. The mixture is added into a reactor and subjected to dry powder hydrothermal treatment at 50-150°C to obtain a precursor material, and the precursor material is crushed to obtain precursor particles, and the precursor particle size is 40-500 mesh.

[0050] S2. Carbonization: Under the protection of argon atmosphere, the precursor particles obtained in S1 were heated to 1100°C at a rate of 1-2°C / min, kept warm for 2 hours, and cooled to room temperature with the furnace to obtain a starch-based hard carbon negative electrode material.

[0051] S3. Preparation of negative electrode: The starch-based hard carbon negative electrode material is used as the negative electrode active material to prepare the negative electrode sheet. The negative electrode material is evenly ground with the conductive agent and the binder in a mass ratio of 8:1:1, and then mixed with N-methylpyrrolidone to prepare the negative electrode slurry, which is coated on the current collector, placed in a vacuum oven at 100°C for 10 hours, and dried and cut into disc-shaped negative electrode sheets.

[0052] S4, half-cell assembly: lithium sheet is used as the counter electrode, and the electrolyte is composed of 1.0 mol LiPF 6 The starch-based negative electrode sheet was prepared in a solution of ethylene carbonate, diethyl carbonate and dimethyl carbonate (EC / DEC / DMC, v / v / v=1:1:1), and assembled into a button cell in a glove box under an argon atmosphere.

[0053] Figure 1 This is a SEM image of the starch-based hard carbon negative electrode material prepared in Example 2. Figure 1 It can be seen that starch-based hard carbon shows a microscopic morphology with similar size and uniform distribution. Due to the introduction of melamine cross-linking agent, the spherical structure of starch is maintained during high-temperature carbonization.

[0054] Figure 2 The XRD patterns of starch-based hard carbon negative electrode materials prepared in Examples 1-3 and Comparative Example 1 are shown in FIG. Figure 2 It can be seen that with the increase of carbonization temperature, the intensity of the (002) peak increases, and the degree of graphitization of the material continues to increase.

[0055] Figure 3 The battery assembled with starch-based hard carbon negative electrode materials prepared in Example 2 and Comparative Example 1 of the present invention was subjected to a low current density of 25 mAg -1 The charge and discharge curves are shown below. Figure 3 It can be seen that at a low current density, the introduction of melamine in Example 2 resulted in a negative electrode material with high lithium storage capacity, which is higher than the 282.4 mAh g of starch-based hard carbon prepared with the traditional maleic anhydride crosslinking agent. -1 The specific capacity is as high as 375.6 mAh g -1 .

[0056] Figure 4 This is a GCD performance diagram of a battery assembled with starch-based hard carbon negative electrode materials prepared in Example 2 of the present invention. Figure 4 It can be seen that starch-based hard carbon anode materials have excellent rate performance. -1 Still has 140.5mAh g -1 This is attributed to the introduction of nitrogen into melamine, which gives it good kinetic properties and abundant lithium storage sites.

[0057] Figure 5 The battery assembled with starch-based hard carbon negative electrode materials prepared in Examples 1-3 of the present invention and Comparative Example 1 was subjected to a current density of 0.1 Ag. -1 The cycle performance comparison chart below. Figure 5 It can be seen that in the comparison of different carbonization temperatures and different cross-linking agents, the electrochemical performance is best when melamine is used as the cross-linking agent and carbonization is performed at 1100°C.

[0058] Figure 6 The batteries assembled from the materials prepared in Examples 1-3 of the present invention and Comparative Example 1 were respectively subjected to a current density of 25 mA g. -1 Comparison of the galvanostatic intermittent titration (GITT) curves and the calculated diffusion coefficients D during the lithiation and delithiation processes. Figure 6 It can be seen that the diffusion coefficient of Example 2 is the highest, indicating that it has more active sites, which is beneficial to the storage of lithium ions.

[0059] Figure 7 CV (A), GCD (B) and cycle performance diagram (C) of the hybrid lithium ion supercapacitor assembled in Example 4 of the present invention. The data show that the starch-based hard carbon material prepared by the present invention as the anode of the hybrid lithium ion supercapacitor achieves good matching between the anode and the cathode, and achieves a maximum of 229.5Wh kg -1 The energy density is 26kW kg -1 The power density can still be maintained at 180Wh kg -1 The energy density is 99% and the capacity retention rate is still over 99% after 500 cycles.

[0060] For matters not mentioned above, the prior art applies.

[0061] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modification, equivalent substitution, improvement, etc. made to the above embodiments based on the technical essence of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a starch-based hard carbon negative electrode material, Features: Corn starch is esterified with melamine and then carbonized to obtain the starch-based hard carbon negative electrode material.

2. The preparation method according to claim 1, Features: The carbonization temperature is 900-1300°C, and the carbonization time is 1-8h.

3. The preparation method according to claim 1, Features: The heating rate of carbonization is 1-10°C / min.

4. The preparation method according to claim 1, Features: The specific operation of esterifying corn starch with melamine is: vacuum drying the corn starch, and then hydrothermally reacting it with melamine to obtain esterified starch.

5. The preparation method according to claim 4, Features: The mass ratio of corn starch to melamine is 4:

1.

6. The preparation method according to claim 4, Features: The hydrothermal reaction temperature is 50-150°C.

7. A starch-based hard carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 6.

8. An application of the starch-based hard carbon negative electrode material as claimed in claim 7, Features: Used in lithium-ion battery negative electrodes and hybrid lithium-ion supercapacitor anodes.

9. A hybrid lithium-ion supercapacitor, Features: The starch-based hard carbon negative electrode material as described in claim 7 is used as the negative electrode active material to prepare the negative electrode, and it is activated; the activated carbon material is used as the positive electrode active material to prepare the positive electrode sheet, the above-mentioned activated starch-based hard carbon negative electrode is used as the anode, and the positive electrode prepared with activated carbon is used as the cathode to assemble into a hybrid lithium-ion supercapacitor.

Citation Information

Cited By

  • Starch-coated hard carbon negative electrode material, preparation method thereof and sodium ion battery

    CN119612490A

  • Preparation method and application of starch-based hard carbon material

    CN120518056A

  • Asphalt-modified starch-based hard carbon negative electrode material and preparation method thereof

    CN121044568A