Edge removing method and system for reducing edge fault group after epitaxy, medium and equipment

By first depositing the LTO film on the silicon wafer, then defiling and POLY film deposition, and combining polishing treatment, the problem of chamfered LTO layer cracking in the super back sealing process is solved, reducing edge layer errors and improving client electricity Sexual performance and user experience.

CN119008387APending Publication Date: 2024-11-22SHANGHAI SEMICON WAFER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411145129.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the super back sealing process, the LTO layer on the chamfer is prone to cracking and forming particles during high temperatures, resulting in layer errors at the edge of the silicon wafer, affecting the electrical performance and user experience of the client.

Method used

The LTO film was deposited by APCVD normal pressure chemical vapor deposition and defiled, and then the POLY film was deposited by LPCVD low pressure chemical vapor deposition after cleaning, and the front polishing was performed to control the demarcation amount and polishing conditions to reduce edge layer errors.

Benefits of technology

Without affecting the back sealing function, the incidence of edge layer errors after the extension is reduced, and the electrical uniformity and user experience of the client are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008387A_ABST
    Figure CN119008387A_ABST
Patent Text Reader

Abstract

The invention provides an edge removing method, system, medium and equipment for reducing edge stacking fault groups after epitaxy, and the method comprises the steps: 1, carrying out APCVD normal pressure chemical vapor deposition on a silicon wafer, and depositing an LTO film; 2, film removing is conducted on edge removing equipment, and the edge removing amount is controlled to be within a preset range; 3, after cleaning, LPCVD low-pressure chemical vapor deposition is carried out, and a POLY film is deposited; and 4, front face polishing is carried out. According to the invention, under the condition that the back sealing function is not influenced, the occurrence of edge stacking fault after the client is used is reduced, and the occurrence rate of influencing the use experience of the client is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of silicon wafer edge removal technology, and in particular to an edge removal method, system, medium and equipment for reducing edge stacking fault groups after epitaxy. Background Art

[0002] At present, due to customer demand, a large number of back-sealing processes are super back-sealing processes. That is, LTO deposition is performed first, and then POLY film deposition is performed. This form of back-sealing process has excellent self-doping inhibition effect, and is more excellent in the electrical performance of epitaxial client. However, after polishing the front side, the POLY layer coated on part of the chamfer will also be thrown away, resulting in the LTO layer coated on the chamfer being exposed on the chamfer of the silicon wafer. Because part of the LTO film on the chamfer is prone to cracking and forming particles during the high temperature epitaxial process, it contaminates the edge of the silicon wafer and forms a stacking fault group at the edge of the silicon wafer, such as Figure 2 . Summary of the invention

[0003] In view of the defects in the prior art, the object of the present invention is to provide a method, system, medium and equipment for reducing edge stacking fault groups after epitaxy.

[0004] The method for removing edge for reducing edge stacking fault groups after epitaxy provided by the present invention comprises:

[0005] Step 1: Perform APCVD atmospheric pressure chemical vapor deposition on the silicon wafer to deposit the LTO film;

[0006] Step 2: De-filming is performed on the de-edging equipment, and the de-edging amount is controlled within a preset range;

[0007] Step 3: After cleaning, perform LPCVD low-pressure chemical vapor deposition to deposit a POLY film;

[0008] Step 4: Polish the front side.

[0009] Preferably, step 1 includes: APCVD atmospheric pressure chemical vapor deposition temperature range is 400℃~700℃, tray transmission speed is within 0.1 m / min, thin film is deposited after mixing silane gas and oxygen, silane gas flow rate is 0.1L / min-0.2L / min, oxygen flow rate is 0.1L / min-0.2L / min.

[0010] Preferably, step 3 comprises: placing the silicon wafer on a silicon boat, then raising the silicon boat into a furnace chamber, and depositing a thin film under silane at a temperature of 500° C. to 700° C., with a silane gas flow rate of 0.5 L / min to 1.5 L / min.

[0011] Preferably, step 4 comprises: polishing to a pressure less than 1 kg / cm2 ; Add abrasives, control the pH of the solution within 11±1, and the abrasive flow rate is 1L / min-2L / min.

[0012] The edge removal system for reducing edge stacking fault groups after epitaxy provided by the present invention comprises:

[0013] Module M1: Perform APCVD atmospheric pressure chemical vapor deposition on silicon wafers to deposit LTO thin films;

[0014] Module M2: De-filming is performed on the de-edging equipment to control the de-edging amount within a preset range;

[0015] Module M3: After cleaning, LPCVD low-pressure chemical vapor deposition is performed to deposit POLY film;

[0016] Module M4: front side polishing.

[0017] Preferably, the module M1 includes: APCVD atmospheric pressure chemical vapor deposition temperature range is 400℃~700℃, tray transmission speed is within 0.1 m / min, thin film is deposited after mixed processing of silane gas and oxygen, silane gas flow rate is 0.1L / min-0.2L / min, oxygen flow rate is 0.1L / min-0.2L / min.

[0018] Preferably, the module M3 comprises: placing the silicon wafer on a silicon boat, then raising the silicon boat into a furnace chamber, and depositing a thin film under silane at a temperature of 500° C. to 700° C., with a silane gas flow rate of 0.5 L / min to 1.5 L / min.

[0019] Preferably, the module M4 includes: polishing with a pressure less than 1kg / cm 2 ; Add abrasives, control the pH of the solution within 11±1, and the abrasive flow rate is 1L / min-2L / min.

[0020] According to the computer-readable storage medium storing a computer program provided by the present invention, when the computer program is executed by a processor, the steps of the method for removing edges to reduce edge stacking fault groups after epitaxy are implemented.

[0021] The electronic device provided according to the present invention comprises a memory, a processor and a computer program stored in the memory and executable on the processor. When the computer program is executed by the processor, the steps of the method for reducing edge stacking fault groups after epitaxy are implemented.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention first performs APCVD atmospheric pressure chemical vapor deposition on the silicon wafer to deposit an LTO film, then performs film removal on an edge removal device, and then performs LPCVD low pressure chemical vapor deposition after cleaning to deposit a POLY film, and finally performs front polishing. Without affecting the back sealing function itself, the edge stacking faults that occur after use by the client are reduced, thereby reducing the incidence of affecting the client's usage experience. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0025] Figure 1 The state of the silicon wafer with whitish edges under the spotlight;

[0026] Figure 2 This is the state of a silicon wafer with a large number of stacking faults visible under a microscope at 500X;

[0027] Figure 3 This is the state of the silicon wafer after AP (LTO) + LP (POLY) in the original process diagram;

[0028] Figure 4 This is the state of the silicon wafer after polishing in the original process diagram;

[0029] Figure 5 This is the state of the silicon wafer after AP (LTO) in the current process diagram;

[0030] Figure 6 This is the state of the silicon wafer after the narrow edge removal process in the current process diagram;

[0031] Figure 7 This is the state of the silicon wafer after AP (LTO) + LP (POLY) in the current process diagram;

[0032] Figure 8 This is the state of the silicon wafer after polishing in the current process diagram;

[0033] Fig. 9 The present invention is a flow chart of the method for reducing edge stacking fault groups after epitaxy. DETAILED DESCRIPTION

[0034] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0035] Example 1

[0036] The present invention provides a method for reducing edge stacking fault groups after epitaxy, comprising:

[0037] 1. After LTO film formation, the edge is extremely narrowly trimmed to partially remove the LTO film on the chamfer. The trimming amount needs to be greater than 100um. At the same time, in order not to affect the effect of subsequent back sealing to inhibit self-doping, the edge trimming amount needs to be less than 400um.

[0038] After verification, the data is as follows:

[0039] De-edging amount 50um 100um 150um 200um 250um 300um 350um 400um Epitaxial resistivity uniformity 1.40% 1.56% 1.45% 1.67% 1.97% 2.04% 2.27% 2.45% Edge white border have none none none none none none none

[0040] like Figure 1 , which is a picture of the whitened edge under the spotlight. The results show that the whitened edge phenomenon can be effectively solved with a de-edging amount of 100um. With a de-edging amount of 400um, the resistivity uniformity of less than 2.5% can meet the requirements.

[0041] 2. Graphical representation of the original process:

[0042] (1) After AP (LTO) + LP (POLY), such as Figure 3 ;

[0043] (2) After polishing, Figure 4 ;

[0044] The POLY layer on the chamfer is removed, leaving the LTO layer exposed on the outside.

[0045] 3. Current process diagram:

[0046] (1) After AP (LTO), such as Figure 5 ;

[0047] (2) After the narrow edge removal process, such as Figure 6 ;

[0048] (3) After AP (LTO) + LP (POLY), such as Figure 7 ;

[0049] (4) After polishing, Figure 8 .

[0050] like Fig. 9 , the specific implementation steps are as follows:

[0051] (1) The product needs to be processed by APCVD first to deposit the LTO film. APCVD is carried out at a temperature of 400°C-700°C, with a tray transmission speed of less than 0.1 m / min, and silane gas with a flow rate of 0.1L / min-0.2L / min mixed with oxygen 0.1-0.2L / min to deposit the film.

[0052] (2) De-filming is performed on a specific de-edging device, using the corresponding tooling to ensure that the de-edging amount is between 100um and 400um;

[0053] (3) After LPCVD pre-cleaning, the LPCVD equipment is deposited to deposit a POLY film; the silicon wafer is placed on a silicon boat, the silicon boat is raised into the furnace chamber, and the film is deposited at a temperature of 500°C to 700°C in silane with a gas flow rate of 0.5L / min to 1.5L / min.

[0054] (4) Finally, polish the front side. The polishing pressure is less than 1kg / cm 2 , add abrasive, control the pH of the liquid within 11±1, and the abrasive flow rate is 1L / min-2L / min. The removal amount needs to be greater than 15um.

[0055] The present invention provides a computer-readable storage medium storing a computer program, and when the computer program is executed by a processor, the steps of the edge removal method for reducing edge stacking fault groups after epitaxy are implemented.

[0056] The present invention provides an electronic device, comprising a memory, a processor and a computer program stored in the memory and executable on the processor. When the computer program is executed by the processor, the steps of the method for reducing edge stacking fault groups after epitaxy are implemented.

[0057] Example 2

[0058] The present invention provides a de-edging system for reducing edge stacking fault groups after epitaxy, comprising: module M1: performing APCVD atmospheric pressure chemical vapor deposition on a silicon wafer to deposit an LTO film; module M2: performing film removal on a de-edging device to control the de-edging amount within a preset range; module M3: performing LPCVD low pressure chemical vapor deposition after cleaning to deposit a POLY film; module M4: performing front polishing.

[0059] The module M1 includes: APCVD atmospheric pressure chemical vapor deposition temperature range is 400℃~700℃, tray transmission speed is within 0.1m / min, thin film is deposited after mixing silane gas and oxygen, silane gas flow rate is 0.1L / min-0.2L / min, oxygen flow rate is 0.1L / min-0.2L / min.

[0060] The module M3 includes: placing the silicon wafer on the silicon boat, then raising the silicon boat into the furnace chamber, and depositing a thin film under silane at a temperature of 500° C. to 700° C., with a silane gas flow rate of 0.5 L / min to 1.5 L / min.

[0061] The module M4 includes: polishing with a pressure less than 1kg / cm2 ; Add abrasives, control the pH of the solution within 11±1, and the abrasive flow rate is 1L / min-2L / min.

[0062] Those skilled in the art know that, in addition to implementing the system, device and its various modules provided by the present invention in a purely computer-readable program code, it is entirely possible to implement the same program in the form of logic gates, switches, application-specific integrated circuits, programmable logic controllers and embedded microcontrollers by logically programming the method steps. Therefore, the system, device and its various modules provided by the present invention can be considered as a hardware component, and the modules included therein for implementing various programs can also be considered as structures within the hardware component; the modules for implementing various functions can also be considered as both software programs for implementing the method and structures within the hardware component.

[0063] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.

Claims

1. A method for reducing edge stacking fault groups after epitaxy, characterized in that: include: Step 1: Perform APCVD atmospheric pressure chemical vapor deposition on the silicon wafer to deposit the LTO film; Step 2: De-filming is performed on the de-edging equipment, and the de-edging amount is controlled within a preset range; Step 3: After cleaning, perform LPCVD low-pressure chemical vapor deposition to deposit a POLY film; Step 4: Polish the front side.

2. The method for reducing edge stacking fault groups after epitaxy according to claim 1, characterized in that: The step 1 includes: the APCVD atmospheric pressure chemical vapor deposition temperature range is 400°C to 700°C, the tray transmission speed is within 0.1 m / min, and the thin film is deposited after mixing silane gas and oxygen. The silane gas flow rate is 0.1L / min-0.2L / min, and the oxygen flow rate is 0.1L / min-0.2L / min.

3. The method for reducing edge stacking fault groups after epitaxy according to claim 1, characterized in that: The step 3 includes: placing the silicon wafer on a silicon boat, then raising the silicon boat into the furnace chamber, and depositing a thin film under silane at a temperature of 500° C. to 700° C., with a silane gas flow rate of 0.5 L / min to 1.5 L / min.

4. The method for reducing edge stacking fault groups after epitaxy according to claim 1, characterized in that: The step 4 comprises: polishing to a pressure less than 1 kg / cm 2 ; Add abrasives, control the pH of the solution within 11±1, and the abrasive flow rate is 1L / min-2L / min.

5. A system for reducing edge stacking fault groups after epitaxy, characterized in that: include: Module M1: Perform APCVD atmospheric pressure chemical vapor deposition on silicon wafers to deposit LTO thin films; Module M2: De-filming is performed on the de-edging equipment to control the de-edging amount within a preset range; Module M3: After cleaning, LPCVD low-pressure chemical vapor deposition is performed to deposit POLY film; Module M4: front side polishing.

6. The edge removal system for reducing edge stacking fault groups after epitaxy according to claim 5, characterized in that: The module M1 includes: APCVD atmospheric pressure chemical vapor deposition temperature range is 400℃~700℃, tray transmission speed is within 0.1m / min, thin film is deposited after mixing silane gas and oxygen, silane gas flow rate is 0.1L / min-0.2L / min, oxygen flow rate is 0.1L / min-0.2L / min.

7. The edge removal system for reducing edge stacking fault groups after epitaxy according to claim 5, characterized in that: The module M3 includes: placing the silicon wafer on the silicon boat, then raising the silicon boat into the furnace chamber, and depositing a thin film under silane at a temperature of 500° C. to 700° C., with a silane gas flow rate of 0.5 L / min to 1.5 L / min.

8. The edge removal system for reducing edge stacking fault groups after epitaxy according to claim 5, characterized in that: The module M4 includes: polishing with a pressure less than 1kg / cm 2 ; Add abrasives, control the pH of the solution within 11±1, and the abrasive flow rate is 1L / min-2L / min.

9. A computer-readable storage medium storing a computer program, characterized in that: When the computer program is executed by a processor, the steps of the method for reducing edge stacking fault groups after epitaxy according to any one of claims 1 to 4 are implemented.

10. An electronic device comprising a memory, a processor, and a computer program stored in the memory and executable on the processor, wherein: When the computer program is executed by a processor, the steps of the method for reducing edge stacking fault groups after epitaxy according to any one of claims 1 to 4 are implemented.