Method for detecting charge concentration of mobile ions in surface oxide layer of silicon-based wafer

By forming an aluminum metal electrode region on the surface of the silicon-based wafer and combining the hydrogen alloy process, the capacitance-voltage curve measurement is used to solve the detection problem of moving ion charge concentration in the oxide layer on the surface of the silicon-based wafer, and the wafer process is realized The precise control improves product quality.

CN119008445APending Publication Date: 2024-11-22江苏新顺微电子股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411104357.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the silicon-based wafer manufacturing process, the introduction of impurities causes the presence of moving ion charges in the oxide layer on the wafer surface, affecting the electrical characteristics and equipment environment, causing quality problems and yield losses.

Method used

By forming an aluminum metal electrode region on the surface of a silicon-based wafer, combining the hydrogen alloy process, the moving ion concentration in the silicon dioxide oxide layer is determined using capacitance-voltage curve measurement, and a metal probe and current voltage meter are used for testing, combining high temperature and The bias voltage acts to drive away the ions to determine their concentration.

Benefits of technology

Directly calculate the concentration of moving ion charges per unit area, improve the control efficiency of the process, avoid the hidden dangers of quality problems, and improve product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008445A_ABST
    Figure CN119008445A_ABST
Patent Text Reader

Abstract

The invention relates to a method for detecting the charge concentration of mobile ions in a surface oxide layer of a silicon-based wafer, which comprises the following steps of: heating the silicon-based wafer in an oxidizing furnace to generate a silicon dioxide oxide layer on the front surface of the silicon-based wafer; metalizing the front surface of the oxidized silicon-based wafer to deposit a layer of aluminum metal on the front surface of the silicon-based wafer; sequentially carrying out glue uniformizing, exposure and development on the aluminum metal layer on the front surface of the silicon-based wafer by adopting a photolithography mask, then corroding the aluminum metal layer and removing glue, and leaving a plurality of aluminum metal electrode areas on the silicon dioxide oxide layer of the silicon-based wafer; putting the silicon-based wafer into a hydrogen alloying furnace, introducing hydrogen, heating, and carrying out alloying operation to obtain a test piece; and placing the back surface of the test piece on a metal disc, enabling the front surface of the test piece to face upwards, enabling a metal probe to be in contact with the aluminum metal electrode area, respectively connecting the metal probe and the metal disc into a current and voltage instrument, measuring to obtain a capacitance-voltage curve, and determining the concentration of the moving ions in the silicon dioxide oxide layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor technology, and in particular relates to a method for detecting the charge concentration of mobile ions in an oxide layer on the surface of a silicon-based wafer. Background Art

[0002] During the manufacturing process of silicon-based wafers, some impurities may be introduced on the surface of the wafer. If these impurities are not completely removed in the subsequent cleaning steps, they will flow into the next step for processing, introducing mobile ion charges inside the wafer structure layer, affecting the electrical properties of the chip. Wafers that contain impurities themselves will also pollute the internal environment of the equipment cavity, and then affect the products of subsequent multiple batches of operations, causing significant quality impacts and yield losses. The introduction of the above impurities is mainly caused by personnel factors in the process connection link. Although the wafer production workshop will implement on-site standardized operations, wear cleanroom clothing, isolate regional environments and other measures to minimize the introduction of impurities, impurities will still be introduced occasionally.

[0003] The mobile ion charge of the wafer itself is widely present near the interface between SiO2 film and Si, mainly Na + , K + Various process materials, such as water, chemical reagents, glassware, quartz or human body, are the sources of mobile ionic charge. These charged ions can move in the SiO2 film under the action of temperature and electric field, resulting in a decrease in dielectric strength and even failure of product parameters. Summary of the invention

[0004] In view of the above problems, the present invention provides a method for detecting the charge concentration of mobile ions in an oxide layer on the surface of a silicon-based wafer, comprising the following steps:

[0005] S1: placing a round silicon-based wafer into an oxidation furnace and heating it so that a silicon dioxide oxide layer is formed on the front side of the silicon-based wafer;

[0006] S2: performing a metallization process on the front side of the oxidized silicon-based wafer so as to deposit a layer of aluminum metal on the front side of the silicon-based wafer;

[0007] S3: using a photomask to perform coating, exposure, and development on the aluminum metal layer on the front side of the silicon-based wafer in sequence, and then corroding the aluminum metal layer. After the coating is removed, a number of aluminum metal electrode areas are left on the silicon dioxide oxide layer of the silicon-based wafer;

[0008] S4: placing the silicon-based wafer obtained in step S3 into a hydrogen alloy furnace, introducing hydrogen and heating, performing an alloying operation, completing the alloying process between the silicon dioxide oxide layer and the aluminum metal electrode area, so that the two are more densely combined, and obtaining a test piece;

[0009] S5: Place the back of the test piece on the metal plate with the front of the test piece facing upward, and use a metal probe to touch the aluminum metal electrode area. The metal probe and the metal plate are respectively connected to a current and voltage meter to measure the capacitance-voltage curve, and then determine the mobile ion concentration in the silicon dioxide oxide layer.

[0010] Optionally, in step S1, the silicon-based wafer used as a raw material is a silicon wafer with a resistivity of 2-5Ω·cm, a thickness of 500±50μm, and a crystal orientation of <100> The silicon wafer is a single-sided polished wafer with an N-type conductivity. The silicon-based wafer material can be a 5-inch or 6-inch wafer, or a wafer of a commonly used size, so that the present invention can be applicable to most wafers.

[0011] Optionally, the heating temperature in the oxidation furnace is 1000-1100°C, the heating time is 60-70 minutes, and the thickness of the silicon dioxide oxide layer is

[0012] Optionally, in step S2, the oxidized silicon-based wafer is placed in an evaporation table, and a layer of aluminum metal is deposited on the front side of the silicon-based wafer to cover the front side of the silicon-based wafer, with a thickness of 1.0±0.2 μm.

[0013] Optionally, in step S3, the aluminum metal electrode regions formed on the silicon dioxide oxide layer of the silicon-based wafer are all circular, so as to reduce the additional impact caused by the sharp corners of the electrode region edges;

[0014] Different electrode areas are not interconnected by metal, and the distance between two adjacent electrode areas is not less than 5 mm.

[0015] Further optionally, the aluminum metal electrode area is divided into a first electrode area, a second electrode area and a third electrode area in order of diameter from small to large, the diameter of the first electrode area is 700-750μm, the diameter of the second electrode area is 800-850μm, and the diameter of the third electrode area is 1000-1050μm. The electrode areas have different diameters to facilitate adaptation to test probes of different thicknesses.

[0016] Further optionally, a plurality of first electrode regions, a plurality of second electrode regions and a plurality of third electrode regions are arranged on the front side of the silicon-based wafer.

[0017] A first electrode area is set at the center of the front side of the silicon-based wafer, and the electrode areas are arranged cyclically in the order of the first electrode area, the second electrode area and the third electrode area along the radial direction of the silicon-based wafer; the radius of the electrode area on the front side of the silicon-based wafer is evenly arranged along the circumference of the silicon-based wafer, and the spacing between adjacent electrode areas in the same radial direction is equal, that is, electrode areas of the same size are set on a circle with the same radius from the center of the circle, and the spacing between adjacent electrode areas on the same circle is equal.

[0018] Optionally, step S5 specifically includes:

[0019] (1) The back of the test piece is vacuum-adsorbed on the metal disk to ensure that the two are tightly fitted; the tip of the metal probe touches the inside of any aluminum metal electrode area, and the other end of the metal probe and the metal disk are connected to the current and voltage meter respectively; at room temperature, a test scan is performed to obtain the first capacitance-scanning voltage curve;

[0020] (2) The metal disk is heated to raise the temperature of the back side of the test piece to 250°C and maintained at a constant temperature for 5-8 minutes. During the constant temperature period, a forward bias voltage of +10V is applied to the same aluminum metal electrode area and the metal disk (i.e., the silicon-based substrate of the test piece). After the constant temperature is terminated and cooled to room temperature, a second capacitance-scanning voltage curve is obtained by scanning;

[0021] (3) The metal disk is heated to 250°C again and kept at a constant temperature for 5-8 minutes. During the constant temperature period, a negative bias voltage of -10V is applied to the same aluminum metal electrode area and the metal disk respectively. After the constant temperature is ended and the metal disk is cooled to room temperature, the third capacitance-scanning voltage curve is obtained by scanning.

[0022] (4) The mobile ion concentration in the silicon dioxide oxide layer is obtained by using the flat band voltage offset of the above three capacitance-scanning voltage curves.

[0023] In step (2), the kinetic energy of the mobile ions is stimulated by high temperature, and when a forward bias voltage is applied, the mobile ion charges in the silicon dioxide oxide layer are driven by the electric field to move toward the aluminum metal electrode area. In step (3), under the action of a reverse bias voltage, the mobile ion charges in the silicon dioxide oxide layer are driven by the electric field to move toward the metal disk (i.e., silicon-based substrate).

[0024] Further optionally, in steps (1)-(3), the measured capacitance value is within 10-300pF.

[0025] The test piece of the present invention forms an aluminum metal electrode area, a silicon dioxide oxide layer and a silicon-based substrate structure from top to bottom. The structure is similar to the MOS structure of metal-oxide-semiconductor. The oxide between the capacitor plates accumulates the capacitor C ox Determined by the following formula:

[0026] C OX =K0×ε0×A / t OX

[0027] Among them, C OX is the accumulation capacitance of the silicon dioxide oxide layer, pF; K0 is the relative dielectric constant, dimensionless; ε0 is the vacuum permittivity, F / cm; A is the area of ​​a single aluminum metal electrode region, cm 2 ;t ox is the thickness of the silicon dioxide oxide layer, It can be seen that K0 and ε0 are constants, C ox Only with A and t ox related.

[0028] Optionally, in step (4), the mobile ion concentration N in the silicon dioxide oxide layer is m Determined by the following formula:

[0029] N m =△V fb ×C fb / q

[0030] Among them, N m is the mobile ion concentration in the silicon dioxide oxide layer, cm -2 ; △V fb is the flat band voltage offset, V; q is the unit charge, and the charge carried by a unit charge is approximately 1.60217×10 -19 C; C fb represents the flat-band capacitance between the electrode regions, pF.

[0031] C fb Determined by the following formula: C fb =C OX / A=K0×ε0 / t OX

[0032] Therefore, the mobile ion concentration N in the silicon dioxide oxide layer is m The formula is:

[0033] N m =0.62415×10 19 ×△V fb ×K0×ε0 / t OX

[0034] From the above formula, we can know that the mobile ion concentration N m It is not affected by A, so probes of different sizes can be selectively applied to aluminum metal electrode areas of suitable sizes. Use probes of different sizes to test electrode areas of corresponding sizes and test the distribution of mobile ion charge concentration inside the surface oxide layer at different positions of silicon-based wafers.

[0035] The technical solution of the present invention can directly calculate the concentration of mobile ion charges per unit area, and display the invisible, unquantifiable and relatively abstract ion charges in the control of silicon-based wafer process through intuitive data, so as to conduct targeted investigation and testing, and take corrective and preventive measures in time, thus avoiding the previous clueless containment and screening, greatly improving work efficiency, and playing a key role in ensuring the steady improvement of product quality.

[0036] The present invention also provides a testing device capable of testing multiple test pieces at one time, the device comprising a dark box and a sample clamping unit and a probe moving unit inside the dark box, the sample clamping unit comprising at least one pair of clamping rods and at least one row of circular sample seats arranged in a straight line, each sample seat being rotatably connected to the clamping rod through an openable and closable clamping ring, one end of the clamping rod passing through the dark box, and being used to control the opening and closing of the pair of clamping rods;

[0037] The clamping ring includes two semicircular sub-rings, and each clamping rod is provided with a semicircular slide groove at a position corresponding to the sample holder, the slide groove protrudes to the outside of the sample holder, and the sub-ring is slidably connected to the corresponding slide groove of the corresponding clamping rod;

[0038] The probe moving unit comprises a moving track and a probe rack. The probe rack is cylindrical and parallel to the clamping rod. The probe rack comprises at least three probe seats. Each probe seat comprises a plurality of probe holes. The probe holes correspond to the sample seats one by one.

[0039] Optionally, the sample clamping unit includes a plurality of sample placement components, which are arranged horizontally and parallel to each other, and the sample placement components are parallel to one side of the dark box, so as to facilitate the setting of the moving track and the probe rack;

[0040] The sample placement assembly includes a pair of clamping rods and a plurality of sample seats arranged in a straight line, the clamping rods are parallel to the straight line formed by the sample seats, and the plurality of sample seats are evenly arranged along the length direction of the clamping rods;

[0041] The sub-circles of the clamping ring are slidably connected to the corresponding sliding grooves of the clamping rods through sliders, and the diameter of the sample seat and the inner diameter of the clamping ring are equal to the diameter of the test piece; after the test piece is placed on the sample seat, the two clamping rods approach each other, so that the two sub-circles approach each other and clamp the sample seat and the test piece. At this time, the sub-circles are merged into a circle (i.e., the clamping ring), and the sample seat can drive the clamping ring and the test piece to rotate along the corresponding sliding groove, thereby adjusting the angle of the test piece so that a certain aluminum metal electrode area on the front of the test piece can correspond to the probe of the probe hole up and down.

[0042] Optionally, the lower surface of the cover is provided with at least one row of infrared alignment devices, the infrared alignment devices comprising a plurality of infrared emitting and receiving sensors, the infrared emitting and receiving sensors corresponding to the sample holder one by one; the infrared emitting and receiving sensors corresponding to the same position of the sample holder,

[0043] When the infrared transmitting and receiving sensors emit infrared rays downward and irradiate the corresponding position of the test piece, the light returns to the infrared transmitting and receiving sensors and detects the reflectivity. Since the reflectivity of the aluminum metal electrode area and the silicon dioxide oxide layer to infrared rays is different, the reflectivity can be used to determine whether the infrared rays are irradiated on the aluminum metal electrode area.

[0044] Optionally, the probe rack includes a plurality of probe seats, which are evenly distributed along the circumference of the probe rack. Probes of the same thickness are installed on the same probe seat, and probes of different thicknesses are installed on different probe seats. Along the clockwise direction of the probe rack, the diameter of the probes installed on the probe seats gradually increases or decreases, which facilitates the use of probes of different thicknesses to detect the same test piece multiple times.

[0045] Further optionally, a rotating motor is provided at one end of the probe frame connected to the vertical track for controlling the rotation of the probe frame. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 The CV curve obtained by testing the first electrode region with the probe;

[0047] Figure 2 The CV curve obtained by testing the second electrode region with the probe;

[0048] Figure 3 It is a structural schematic diagram of the testing device in the embodiment;

[0049] Figure 4 is a schematic diagram of a probe holder;

[0050] Figure 5 is a schematic diagram of the clamping rod and the sample holder;

[0051] Figure 6 Schematic diagram of the coordination between the clamping rod and the sample holder;

[0052] Figure 7 Schematic diagram of the test piece.

[0053] In the accompanying drawings, 1-dark box, 2-clamping rod, 3-sample holder, 4-clamping ring, 5-slide groove, 6-dividing ring, 7-probe holder, 8-probe hole, 9-probe, 10-cover, 11-test piece, 12-electrode area, 13-operating table, 14-horizontal track, 15-vertical track, 16-silicon dioxide oxide layer, 17-silicon-based substrate. DETAILED DESCRIPTION

[0054] This embodiment provides a method for detecting the charge concentration of mobile ions in an oxide layer on the surface of a silicon-based wafer, comprising the following steps:

[0055] S1: placing a circular silicon-based wafer into an oxidation furnace and heating it so that a silicon dioxide oxide layer 16 is formed on the front side of the silicon-based wafer;

[0056] S2: performing a metallization process on the front side of the oxidized silicon-based wafer so as to deposit a layer of aluminum metal on the front side of the silicon-based wafer;

[0057] S3: using a photomask to perform coating, exposure, and development on the aluminum metal layer on the front side of the silicon-based wafer in sequence, and then corroding the aluminum metal layer. After the coating is removed, a number of aluminum metal electrode areas are left on the silicon dioxide oxide layer of the silicon-based wafer;

[0058] S4: placing the silicon-based wafer obtained in step S3 into a hydrogen alloy furnace, introducing hydrogen and heating, performing an alloying operation, completing the alloying process between the silicon dioxide oxide layer and the aluminum metal electrode area, so that the two are more densely combined, and obtaining a test piece;

[0059] S5: Place the back of the test piece on the metal plate with the front of the test piece facing upward, and use a metal probe to touch the aluminum metal electrode area. The metal probe and the metal plate are respectively connected to a current and voltage meter to measure the capacitance-voltage curve, and then determine the mobile ion concentration in the silicon dioxide oxide layer.

[0060] The metal disk is a sample holder, and one sample holder is equipped with a current and voltage meter. The power supply and the current and voltage meter are arranged outside the dark box and are connected by electric wires.

[0061] In step S1, the silicon-based wafer used as the raw material is a silicon wafer with a resistivity of 2-5Ω·cm, a thickness of 500±50μm, and a crystal orientation of <100> The silicon wafer is a single-sided polished wafer with N-type conductivity. The raw material of the silicon-based wafer is a 5-inch wafer.

[0062] The heating temperature in the oxidation furnace is 1000°C, the heating time is 70 minutes, and the thickness of the silicon dioxide oxide layer is

[0063] Since silicon-based wafers are in sheet form, they are placed vertically on a support boat (ceramic). Each support boat has one or more slots, and a silicon-based wafer is placed in each slot to prevent the silicon-based wafer from falling over or stacking. The back of the silicon-based wafer is protected in advance with a film. Affected by the oxidizing atmosphere inside the furnace tube, after the oxidation step, a thin oxide layer grows on the front and back of the silicon-based wafer. After cooling, the back of the silicon-based wafer is placed in a 5% HF solution for corrosion for 60 seconds, then cleaned and dried, and the surface protective film is removed to obtain a silicon-based wafer with an oxide layer on the front and silicon on the back.

[0064] In step S2, the oxidized silicon-based wafer is placed in an evaporation table at an evaporation temperature of 100°C and an evaporation rate of A layer of aluminum metal is deposited on the front side of the silicon-based wafer with a thickness of 1.0±0.2μm.

[0065] In step S3, the aluminum metal electrode areas formed on the silicon dioxide oxide layer of the silicon-based wafer are all circular, different electrode areas are not interconnected by metal, and the distance between two adjacent electrode areas is not less than 5 mm.

[0066] The aluminum metal electrode area is divided into a first electrode area, a second electrode area and a third electrode area in order of diameter from small to large. The diameter of the first electrode area is 700μm, the diameter of the second electrode area is 800μm, and the diameter of the third electrode area is 1000μm. The electrode areas have different diameters to facilitate adaptation to test probes of different thicknesses.

[0067] The front side of the silicon-based wafer is provided with a plurality of first electrode regions, a plurality of second electrode regions and a plurality of third electrode regions.

[0068] A first electrode area is set at the center of the front side of the silicon-based wafer, and the electrode areas are arranged cyclically in the order of the first electrode area, the second electrode area and the third electrode area along the radial direction of the silicon-based wafer; the radius of the electrode area on the front side of the silicon-based wafer is evenly arranged along the circumference of the silicon-based wafer, and the spacing between adjacent electrode areas in the same radial direction is equal, that is, electrode areas of the same size are set on a circle with the same radius from the center of the circle, and the spacing between adjacent electrode areas on the same circle is equal.

[0069] In step S3, the thickness of the photoresist film is required to be (1.0±0.2) μm, contact exposure is adopted, and the development time is controlled within 5-10 s.

[0070] In step S4, high-purity hydrogen is used with a purity of 99.99%; the heating temperature of this step is 400° C. and the heating time is 10 min.

[0071] Step S5 specifically includes:

[0072] (1) The back of the test piece is vacuum-adsorbed on the metal plate (i.e., the sample holder) to ensure that the two are tightly fitted; the tip of the metal probe touches the inside of any aluminum metal electrode area, and the other end of the metal probe and the metal plate are respectively connected to the current and voltage meter; at room temperature, a test scan is performed to obtain the first capacitance-scanning voltage curve without applying a bias voltage;

[0073] (2) The metal disk is heated to raise the temperature of the back side of the test piece to 250° C. and the temperature is maintained constant for 5 min. During the constant temperature period, a forward bias voltage of +10 V (equivalent to the voltage applied to the silicon substrate 17 of the test piece) is applied to the same aluminum metal electrode area and the metal disk respectively. After the constant temperature is terminated and the test piece is cooled to room temperature, a second capacitance-scanning voltage curve is obtained by scanning.

[0074] (3) The metal disk is heated to 250°C again and kept at a constant temperature for 5 minutes. During the constant temperature period, a negative bias voltage of -10 V is applied to the same aluminum metal electrode area and the metal disk respectively. After the constant temperature is ended and the metal disk is cooled to room temperature, the third capacitance-scanning voltage curve is obtained by scanning.

[0075] (4) Using the flat band voltage offset of the above three capacitance-scanning voltage curves, the mobile ion concentration in the silicon dioxide oxide layer is obtained. The abscissa of the above three capacitance-scanning voltage curves is the scanning voltage (V), and the ordinate is the capacitance (pF).

[0076] In step (2), the kinetic energy of the mobile ions is stimulated by the high temperature, and when a forward bias voltage is applied, the mobile ion charges in the silicon dioxide oxide layer are driven by the electric field to move toward the aluminum metal electrode area. In step (3), under the action of the reverse bias voltage, the mobile ion charges in the silicon dioxide oxide layer are driven by the electric field to move toward the metal disk (i.e., silicon-based substrate 17).

[0077] In steps (1)-(3), the measured capacitance value is within 10-300pF.

[0078] In step (4), the mobile ion concentration N in the silicon dioxide oxide layer is m Determined by the following formula:

[0079] N m =0.62415×10 19 ×△V fb ×K0×ε0 / t OX

[0080] Among them, N m is the mobile ion concentration in the silicon dioxide oxide layer, cm -2 ; △V fb is the flat band voltage offset, in V; K0 is the relative dielectric constant, specifically 3.9; ε0 is the vacuum permittivity, specifically (8.85418×10 -14 )F / cm;t ox is the thickness of the silicon dioxide oxide layer, in units

[0081] △V fb Determined by the following formula:

[0082] △V fb =|V fb(1) -V fb(2) ∣

[0083] The second capacitance-scanning voltage curve and the third capacitance-scanning voltage curve are farthest apart from each other in the direction of the horizontal axis. The scanning voltage values ​​of the horizontal axis corresponding to the second capacitance-scanning voltage curve and the third capacitance-scanning voltage curve at this position are V fb(1) and V fb(2) , V.

[0084] Probes of different sizes are used to correspondingly test the electrode areas of the first electrode area and the second electrode area, and to test the distribution of mobile ion charge concentration inside the oxide layer on the surface of the silicon-based wafer.

[0085] Description: If Figure 1 As shown, on the vertical grid line corresponding to -2V, from top to bottom are the first capacitance-scanning voltage curve, the second capacitance-scanning voltage curve, and the third capacitance-scanning voltage curve; Figure 2 As shown, on the vertical grid line corresponding to -2V, from top to bottom are the first capacitance-scanning voltage curve, the third capacitance-scanning voltage curve, and the second capacitance-scanning voltage curve.

[0086] Table 1 Test results of the first electrode area and the second electrode area

[0087]

[0088] This embodiment provides a testing device, such as Figure 3-Figure 7 As shown, it includes a dark box 1 and a sample clamping unit and a probe moving unit inside the dark box 1. The sample clamping unit includes at least one pair of clamping rods 2 and at least one row of circular sample holders 3 arranged in a straight line. Each sample holder 3 is rotatably connected to the clamping rod 2 through an openable and closable clamping ring 4. One end of the clamping rod 2 passes through the dark box 1 and is used to control the opening and closing of the pair of clamping rods 2.

[0089] The clamping ring 4 includes two semicircular sub-rings 6. A semicircular slide groove 5 is provided at a position of each clamping rod 2 corresponding to the sample holder 3. The slide groove 5 protrudes toward the outside of the sample holder 3. The sub-ring 6 is slidably connected to the corresponding slide groove 5 of the corresponding clamping rod 2.

[0090] The probe moving unit includes a moving track and a probe rack 7 . The probe rack 7 is cylindrical and parallel to the clamping rod 2 . The probe rack 7 includes at least three probe seats. Each probe seat includes a plurality of probe holes 8 . The probe holes 8 correspond to the sample seats 3 one by one.

[0091] The dark box 1 is a cube with an openable lid 10 on the top. The test piece 11 is tested in the dark box 1 to prevent light from affecting the mobile ion charge in the silicon dioxide oxide layer. The present invention finds that light affects the number and distribution of mobile ion charges in the silicon dioxide oxide layer, resulting in inaccurate test results, which may be because light excites mobile ions in the oxide layer.

[0092] For ease of operation, open the cover, place the test pieces 11 with their front sides facing upward on the sample holder 3 one by one. When placing the test pieces 11, there is no need to consider the correspondence between the aluminum metal electrode area 12 on the test pieces 11 and the probes 9, and there is no need to align a certain aluminum metal electrode area of ​​each test piece 11 with the corresponding probe. This can avoid cumbersome operations, increase the placement speed, and reduce the difficulty of operation. Later, the aluminum metal electrode areas and probes can be uniformly aligned to automate the operation and reduce misoperation.

[0093] The sample clamping unit includes a plurality of sample placement components, which are arranged horizontally and parallel to each other, and the sample placement components are parallel to one side of the dark box 1, so as to facilitate the arrangement of the moving track and the probe holder 7;

[0094] The sample placement assembly includes a pair of clamping rods 2 and a plurality of sample holders 3 arranged in a straight line, the clamping rods 2 and the sample holders 3 are parallel to the straight line, and the plurality of sample holders 3 are evenly arranged along the length direction of the clamping rods 2;

[0095] The sub-circles 6 of the clamping ring 4 are slidably connected to the corresponding slide groove 5 of the clamping rod 2 through a slider, and the diameter of the sample holder 3 and the inner diameter of the clamping ring 4 are equal to the diameter of the test piece 11; after the test piece 11 is placed on the sample holder 3, the two clamping rods 2 approach each other, so that the two sub-circles 6 approach each other and clamp the sample holder 3 and the test piece 11. At this time, the sub-circles 6 are merged into a circle (i.e., the clamping ring 4), and the sample holder 3 can drive the clamping ring 4 and the test piece 11 to rotate along the corresponding slide groove 5, thereby adjusting the angle of the test piece 11 so that a certain aluminum metal electrode area on the front of the test piece 11 can correspond to the probe of the probe hole 8 up and down.

[0096] The clamping rod 2 is parallel to one side of the dark box 1. An operating table 13 is provided on the bottom of the dark box 1. The upper surface of the operating table 13 is smooth, flat and horizontal. The clamping rod 2 and the sample holder 3 are placed on the operating table 13 so that the clamping rod 2 does not change its upper and lower positions when it moves, thereby allowing the clamping ring 4 to accurately clamp the sample holder 3 and the test piece 11.

[0097] One end of the clamping rod 2 is inside the dark box 1, and the other end passes through the side of the dark box 1, so that the operator can operate the opening and closing of the pair of clamping rods 2 outside the dark box 1. When a row of sample holders 3 are all placed with test pieces 11, the operator operates externally to make the pair of clamping rods 2 approach each other, so that the clamping ring 4 is close to the outer side of the sample holder 3 and the test piece 11; when the test is completed and the test piece 11 needs to be taken out, the operator operates externally to make the pair of clamping rods 2 move away from each other, so that the sub-rings 6 of the clamping ring 4 also move away from each other, and release the sample holder 3 and the test piece 11.

[0098] A buckling device is provided at one end of a pair of clamping rods 2 exposed from the dark box 1. When the clamping ring 4 is closed, the buckling device connects the pair of clamping rods 2 to prevent the two clamping rods 2 from loosening. The buckling device is a prior art and is not specifically limited.

[0099] A motor is provided below the operating table 13 corresponding to each sample holder 3 or inside the operating table 13, and the rotating shaft of the motor is connected to the center of the circle of the lower surface of the sample holder 3, and is used to control the rotation of the sample holder 3, and the clamping ring 4 can rotate with the sample holder 3. The motor is connected to the power supply and control device outside the dark box 1 to control the rotation angle of the sample holder 3.

[0100] Each sample holder is provided with a heating plate or heating wire inside for heating the test piece. The wires of the sample holder pass through the operating table and the bottom or side of the dark box and are connected to an external power source.

[0101] The upper surface of the sample holder is evenly provided with a number of grooves protruding downward, each of which is provided with at least one through hole, which passes through the sample holder, and the lower part of the sample holder is connected to the air pump outside the dark box through an air extraction pipe, which passes through the bottom or side of the dark box. When the test piece is placed on the sample holder, and air is extracted through the air extraction pipe and the through hole, negative pressure is formed in the groove, thereby adsorbing the test piece.

[0102] One end of the clamping rod 2 in the dark box 1 is provided with a sleeve perpendicular to the clamping rod 2, that is, the end of one clamping rod 2 is fixedly connected to the inner rod, and the end of the other clamping rod 2 is fixedly connected to the outer tube. When the two clamping rods 2 move away from each other, the inner rod is pulled out of the outer tube but does not separate from the outer tube; when the two clamping rods 2 approach each other, the inner rod is inserted into the outer tube so that the ends of a pair of clamping rods 2 do not separate.

[0103] The lower surface of the cover is provided with at least one row of infrared alignment devices, the infrared alignment devices include a plurality of infrared emitting and receiving sensors, the infrared emitting and receiving sensors correspond to the sample holder 3 one by one; the infrared emitting and receiving sensors correspond to the same position of the sample holder 3,

[0104] When the infrared transmitting and receiving sensors emit infrared rays downward and irradiate the corresponding position of the test piece 11, the light returns to the infrared transmitting and receiving sensors and detects the reflectivity. Since the reflectivity of the aluminum metal electrode area and the silicon dioxide oxide layer to infrared rays is different, the reflectivity can be used to determine whether the infrared rays are irradiated on the aluminum metal electrode area.

[0105] The probes on a probe seat are in a straight line. When a probe seat moves to the top of a row of sample seats 3, the probes correspond to the same position on the sample seat 3, which is a circle, that is, the probes are on top and the sample seat 3 is on the bottom. When the sample seat 3 rotates, the probes form a circle at the corresponding positions on the sample seat 3, and the diameter of the circle corresponding to each probe on the sample seat 3 is the same.

[0106] Moreover, the aluminum metal electrode areas on the front of the test piece 11 of the present invention are symmetrically arranged with the center of the circle as the center. When a pair of clamping rods 2 clamp a row of test pieces 11, since the test piece 11 is placed on the sample holder 3 without requiring a placement angle, the probe corresponds to the circle of the test piece 11, which has an electrode area and an oxide layer. The test requires the probe to face any electrode area on the circle, so the infrared transmitting and receiving sensors are required to cooperate with the rotation of the test piece 11 to find the electrode area.

[0107] The infrared light of the infrared transmitting and receiving sensors is irradiated onto the test piece 11. The test piece 11 only needs to be rotated through the clamping ring 4. When the infrared light shines on the oxide layer and the motor area respectively, the reflectivity is different, so it can be identified whether the infrared transmitting and receiving sensors correspond to the electrode area on a specific circle of the test piece 11. Any electrode area on the specific circle can be irradiated. The diameters of the electrode areas on the same circle are the same, and the same size of probes can be used for testing. This increases and reduces the workload of positioning the test piece 11 and shortens the positioning time.

[0108] The movable track includes a horizontal track 14 and a vertical track 15. The bottom of the vertical track 15 is slidably connected to the horizontal track 14. One end of the probe rack 7 is slidably connected to the vertical track 15, and the other end is suspended. The probe rack 7 is perpendicular to the vertical track 15. The horizontal track 14 is perpendicular to the clamping rod 2. The vertical track 15 is perpendicular to the clamping rod 2. The horizontal track 14, the vertical track 15, and the probe rack 7 form a three-dimensional space.

[0109] The probe rack 7 includes a plurality of probe seats, which are evenly distributed along the circumference of the probe rack 7. The same probe seat is installed with probes of the same thickness, and different probe seats are installed with probes of different thicknesses. Along the clockwise direction of the probe rack 7, the diameter of the probes installed on the probe seats gradually increases or decreases, which is convenient for using probes of different thicknesses to detect the same test piece 11 multiple times.

[0110] One end of the probe frame 7 connected to the vertical track 15 is provided with a rotating motor for controlling the rotation of the probe frame 7 .

[0111] A lifting device is provided below the operating platform 13 to control the overall rise or fall of the operating platform 13 .

[0112] When in use, the infrared alignment device, the probe holder 7 and the operating table 13 are arranged from top to bottom in the dark box 1, so that the probe holder 7 does not block the light path of the infrared alignment device first, and the infrared emitting and receiving sensors correspond to the sample holder 3 one by one up and down, and the lid is closed. Through the above method, each sample holder 3 and the test piece 11 corresponding to the same clamping rod 2 are rotated into place, so that the electrode area of ​​the test piece 11 of a certain size can correspond to the probe. Then close the infrared emitting and receiving sensors, move the probe holder 7 to the top of the sample holder 3 by moving the track, rotate the probe holder 7, so that the probe holder with the appropriate size of the probe is facing downward (the probe needle tip is facing downward, and the needle tip is on the same horizontal line), and the probe corresponds to the electrode area on the test piece 11 one by one, and the probe holder 7 moves downward along the vertical track 15 until the distance between the probe and the electrode area is very small (for example, the distance is 0.5-1cm). The lifting device moves the operating table 13 upward so that the needle tip pierces the electrode area, and then the test is carried out, so that multiple test pieces 11 can be tested at one time.

[0113] Then, the operating table 13 moves downward, and the probes are separated from the test pieces 11 . The test pieces 11 in the same row can be rotated to the same angle, and the electrode areas of the same area can be tested multiple times using probes of the same size.

[0114] The probe holder 7 can also be rotated to use probes of different sizes for testing. In this case, the sample holder 3 does not need to be rotated. The probe holder only needs to be moved accordingly (the vertical track 15 is moved to the position of the horizontal track 14) so ​​that probes of other sizes correspond to another electrode area. Perform multiple tests and take the average value.

[0115] The present invention finds that it is not easy to precisely control the downward movement size when the probe holder 7 is moved downward, especially when the thickness of the electrode area is thin. If the probe accidentally pierces the electrode area, not only can the test fail, but also the electrode areas of multiple test pieces 11 in the same row at that position are scrapped. The present invention moves the operating table 13 upward when the distance between the probe and the electrode area is very small. Compared with the downward movement, the upward movement is easier to precisely control and avoids excessive movement and damage to the electrode area.

Claims

1. A method for detecting the charge concentration of mobile ions in an oxide layer on a silicon-based wafer surface, characterized in that: The following steps are involved: S1: placing a round silicon-based wafer into an oxidation furnace and heating it so that a silicon dioxide oxide layer is formed on the front side of the silicon-based wafer; S2: performing a metallization process on the front side of the oxidized silicon-based wafer so as to deposit a layer of aluminum metal on the front side of the silicon-based wafer; S3: using a photomask to perform coating, exposure, and development on the aluminum metal layer on the front side of the silicon-based wafer in sequence, and then corroding the aluminum metal layer. After the coating is removed, a number of aluminum metal electrode areas are left on the silicon dioxide oxide layer of the silicon-based wafer; S4: placing the silicon-based wafer obtained in step S3 into a hydrogen alloy furnace, introducing hydrogen and heating, performing an alloying operation, completing the alloying process between the silicon dioxide oxide layer and the aluminum metal electrode area, so that the two are more densely combined, and obtaining a test piece; S5: Place the back of the test piece on the metal plate with the front of the test piece facing upward, and use a metal probe to touch the aluminum metal electrode area. The metal probe and the metal plate are respectively connected to a current and voltage meter to measure the capacitance-voltage curve, and then determine the mobile ion concentration in the silicon dioxide oxide layer.

2. The method for detecting the charge concentration of mobile ions in the oxide layer on the surface of a silicon-based wafer according to claim 1, characterized in that: In step S1, the silicon-based wafer used as the raw material is a silicon wafer with a resistivity of 2-5Ω·cm, a thickness of 500±50μm, and a crystal orientation of <100> , the silicon wafer is a single-sided polished wafer with N-type conductivity.

3. The method for detecting the charge concentration of mobile ions in the oxide layer on the surface of a silicon-based wafer according to claim 1, characterized in that: In step S1, the heating temperature in the oxidation furnace is 1000-1100°C, the heating time is 60-70 minutes, and the thickness of the silicon dioxide oxide layer is In step S2, the oxidized silicon-based wafer is placed in an evaporation table, and a layer of aluminum metal is deposited on the front side of the silicon-based wafer to cover the front side of the silicon-based wafer, with a thickness of 1.0±0.2 μm.

4. The method for detecting the charge concentration of mobile ions in the oxide layer on the surface of a silicon-based wafer according to claim 3, characterized in that: In step S3, the aluminum metal electrode areas formed on the silicon dioxide oxide layer of the silicon-based wafer are all circular, different electrode areas are not interconnected by metal, and the distance between two adjacent electrode areas is not less than 5 mm; The aluminum metal electrode area is divided into a first electrode area, a second electrode area and a third electrode area in order from small to large diameters. The diameter of the first electrode area is 700-750 μm, the diameter of the second electrode area is 800-850 μm, and the diameter of the third electrode area is 1000-1050 μm. The electrode areas have different diameters to facilitate adaptation to test probes of different thicknesses.

5. The method for detecting the charge concentration of mobile ions in the oxide layer on the surface of a silicon-based wafer according to claim 4, characterized in that: The front side of the silicon-based wafer is provided with a plurality of first electrode regions, a plurality of second electrode regions and a plurality of third electrode regions. A first electrode area is set at the center of the front side of the silicon-based wafer, and the electrode areas are arranged cyclically in the order of the first electrode area, the second electrode area and the third electrode area along the radial direction of the silicon-based wafer; the radius of the electrode area on the front side of the silicon-based wafer is evenly arranged along the circumference of the silicon-based wafer, the spacing between adjacent electrode areas in the same radial direction is equal, and electrode areas of the same size are set on a circle with the same radius from the center of the circle, and the spacing between adjacent electrode areas on the same circle is equal.

6. The method for detecting the charge concentration of mobile ions in the oxide layer on the surface of a silicon-based wafer according to claim 5, characterized in that: Step S5 specifically includes: (1) The back of the test piece is vacuum-adsorbed on the metal disk to ensure that the two are tightly fitted; the tip of the metal probe touches the inside of any aluminum metal electrode area, and the other end of the metal probe and the metal disk are connected to the current and voltage meters respectively; at room temperature, a test scan is performed to obtain the first capacitance-voltage curve; (2) The metal disk is heated to raise the temperature of the back side of the test piece to 250°C and maintained at a constant temperature for 5-8 minutes. During the constant temperature period, a forward bias voltage of +10V is applied to the same aluminum metal electrode area and the metal disk respectively. After the constant temperature is terminated and cooled to room temperature, a second capacitance-scanning voltage curve is obtained by scanning; (3) The metal disk is heated to 250°C again and kept at a constant temperature for 5-8 minutes. During the constant temperature period, a negative bias voltage of -10V is applied to the same aluminum metal electrode area and the metal disk respectively. After the constant temperature is terminated and cooled to room temperature, the third capacitance-scanning voltage curve is obtained by scanning; (4) The mobile ion concentration in the silicon dioxide oxide layer is obtained by using the flat band voltage offset of the above three capacitance-scanning voltage curves.

7. The method for detecting the charge concentration of mobile ions in the oxide layer on the surface of a silicon-based wafer according to claim 6, characterized in that: The following testing device is used, including a dark box and a sample clamping unit and a probe moving unit inside the dark box, wherein the sample clamping unit includes at least one pair of clamping rods and at least one row of circular sample seats arranged in a straight line, each sample seat is rotatably connected to the clamping rod through an openable and closable clamping ring, and one end of the clamping rod passes through the dark box and is used to control the opening and closing of the pair of clamping rods; The clamping ring includes two semicircular sub-rings, and each clamping rod is provided with a semicircular slide groove at a position corresponding to the sample holder, the slide groove protrudes to the outside of the sample holder, and the sub-ring is slidably connected to the corresponding slide groove of the corresponding clamping rod; The probe moving unit comprises a moving track and a probe rack. The probe rack is cylindrical and parallel to the clamping rod. The probe rack comprises at least three probe seats. Each probe seat comprises a plurality of probe holes. The probe holes correspond to the sample seats one by one.

8. The method for detecting the charge concentration of mobile ions in the oxide layer on the surface of a silicon-based wafer according to claim 7, characterized in that: The sample clamping unit includes a plurality of sample placement components, which are arranged horizontally and parallel to each other, and the sample placement components are parallel to one side of the dark box, so as to facilitate the arrangement of the moving track and the probe rack; The sample placement assembly includes a pair of clamping rods and a plurality of sample seats arranged in a straight line, the clamping rods are parallel to the straight line formed by the sample seats, and the plurality of sample seats are evenly arranged along the length direction of the clamping rods; The sub-circles of the clamping ring are slidably connected to the corresponding sliding grooves of the clamping rods through sliders, and the diameter of the sample seat and the inner diameter of the clamping ring are equal to the diameter of the test piece; after the test piece is placed on the sample seat, the two clamping rods approach each other, so that the two sub-circles approach each other and clamp the sample seat and the test piece. At this time, the sub-circles are merged into a circle, and the sample seat can drive the clamping ring and the test piece to rotate along the corresponding sliding groove, thereby adjusting the angle of the test piece so that a certain aluminum metal electrode area on the front of the test piece can correspond to the probe of the probe hole up and down.

9. The method for detecting the charge concentration of mobile ions in the oxide layer on the surface of a silicon-based wafer according to claim 8, characterized in that: The lower surface of the cover is provided with at least one row of infrared alignment devices, the infrared alignment devices include a plurality of infrared emitting and receiving sensors, the infrared emitting and receiving sensors correspond to the sample holders one by one; the infrared emitting and receiving sensors correspond to the same position of the sample holder, When the infrared transmitting and receiving sensors emit infrared rays downward and irradiate the corresponding position of the test piece, the light returns to the infrared transmitting and receiving sensors and detects the reflectivity. Since the reflectivity of the aluminum metal electrode area and the silicon dioxide oxide layer to infrared rays is different, the reflectivity can be used to determine whether the infrared rays are irradiated on the aluminum metal electrode area.

10. The method for detecting the charge concentration of mobile ions in the oxide layer on the surface of a silicon-based wafer according to claim 9, characterized in that: The probe rack includes a plurality of probe seats, which are evenly distributed along the circumference of the probe rack. The same probe seat is installed with probes of the same thickness, and different probe seats are installed with probes of different thicknesses. Along the clockwise direction of the probe rack, the diameters of the probes installed in the probe seats gradually increase or decrease, so that the same test piece can be detected multiple times using probes of different thicknesses. One end of the probe frame connected to the vertical track is provided with a rotating motor for controlling the rotation of the probe frame.