Self-supporting SiC / ZnS heterojunction nano array, preparation method thereof and application of self-supporting SiC / ZnS heterojunction nano array in photoelectrochemical photoelectric detector

By forming SiC/ZnS heterojunction nanoarrays on SiC substrates, the problems of slow photoresponse and high dark current of pure SiC photoanode materials are solved, and an efficient ultraviolet photodetector is realized, with significant photocurrent improvement and rapid response. Ability, suitable for large-scale production.

CN119008760APending Publication Date: 2024-11-22NINGBO UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411009400.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing UV detectors have problems such as poor environmental adaptability, insufficient response to low-energy UV light, expensive and complex production processes, especially pure SiC as a photoanode material, slow light response and high dark current.

Method used

The self-supported SiC/ZnS heterojunction nanoarray was used to grow ZnS by anodizing and chemical bath deposition on the SiC substrate to form the SiC/ZnS heterojunction nanoarray as the working electrode of the photoelectrochemical ultraviolet photodetector. The method includes 3 pulse oxidation on a SiC substrate and oil bath deposition in a Zn source solution, controlling the oxidation time and temperature to ensure uniform distribution and synthesis of ZnS.

Benefits of technology

It significantly improves the photocurrent intensity and response speed of the ultraviolet photodetector, improves the photoelectric conversion efficiency, and achieves efficient absorption and rapid response to light in the wavelength range of 200-480nm. It has a simple process and low cost, which is suitable for large-scale production. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008760A_ABST
    Figure CN119008760A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ultraviolet photoelectric detection, and relates to a self-supporting SiC / ZnS heterojunction nano array, a preparation method thereof and application of the self-supporting SiC / ZnS heterojunction nano array in a photoelectrochemical photoelectric detector. The self-supporting SiC / ZnS heterojunction nano array is prepared by adopting an anodic oxidation method and a chemical bath deposition method, the process is simple, the cost is low, conditions are created for large-scale production, the ultraviolet photoelectric detector has a wide prospect in practical application, the service life of a current carrier is prolonged due to a proper amount of defects at an interface of the nano array, and the performance of the ultraviolet photoelectric detector is improved. And additional active sites are also provided, so that the generation of light current is further enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ultraviolet photoelectric detection, and relates to a self-supporting SiC / ZnS heterojunction nanoarray and a preparation method thereof, and application in a photoelectrochemical photoelectric detector. Background Art

[0002] UV detectors have attracted extensive attention due to their wide applications in the fields of missile warning, bioanalysis, environmental sensors, and space exploration. At present, wide bandgap semiconductor materials such as Ga2O3, GaN, ZnS, diamond, TiO2, ZnO, and SiC have been introduced one after another, which has greatly promoted the development of high-sensitivity UV detectors. However, traditional UV PDs still have various limitations that restrict their application, such as poor environmental adaptability, insufficient response to low-energy UV light, and expensive and complex manufacturing processes. Therefore, it is crucial to develop new UV detectors with high photoresponsivity, high spectral sensitivity, and high stability to meet the growing demand. In recent years, PEC UV PDs are emerging as a new high-performance device with remarkable qualities such as light weight, environmental protection, and affordable manufacturing processes, making them very promising in the future of smart electronics. Through photoelectrochemical technology, PEC PDs can efficiently convert light energy into electrical energy. They are effectively used for environmental remediation of pollutant degradation, sustainable fuel and chemical production, and advanced analytical systems for environmental and biological monitoring, thanks to their efficient method of converting electromagnetic radiation into chemical fuels and electricity through PEC cells. When designing PEC PDs, not only the photoelectric conversion of the material but also the efficiency of the interfacial chemical reaction should be considered. The one-dimensional (1D) nanowire structure provides a larger solid-liquid reaction interface and shows a natural advantage in PEC electrodes. The low-dimensional nanowire structure can shorten the carrier transport time and limit the active area of ​​the charge carriers. These advantages lead to the constructed PEC PDs with high photoconductivity gain and responsiveness.

[0003] Among various wide bandgap semiconductors, 4H-SiC materials, as typical third-generation semiconductors, are widely considered to be one of the most suitable candidates for UV PD due to their wide bandgap, high carrier mobility, excellent physical / chemical stability and unique photoelectric properties. So far, some studies have focused on the traditional UV PD applications of SiC nanomaterials and demonstrated their excellent light detection performance. However, to the best of our knowledge, there are few studies on PEC UV PD based on SiC nanomaterials. The main reasons can be summarized as follows: First, in PEC UV PD, the charge transfer process at the interface between the semiconductor and the electrolyte solution has high requirements for the photoanode material. Usually, one-dimensional nanostructured semiconductor materials are required to provide more charge transfer sites, promote the ion migration rate, and achieve fast and efficient photoelectric conversion. Secondly, pure SiC is limited by its own photoelectrochemical properties and cannot produce a good photoelectrochemical effect with the electrolyte solution when used as a single photoanode material. The number of electron-hole pairs generated under illumination is limited, and its interface characteristics with the electrolyte solution are not conducive to efficient photoelectrochemical reactions. Summary of the invention

[0004] In view of the deficiencies in the above-mentioned prior art, the present invention aims to provide a self-supporting SiC / ZnS heterojunction nanoarray, which effectively solves the problems of slow light response and high dark current of the array constructed of pure SiC as a photoanode.

[0005] One object of the present invention can be achieved by the following technical solutions:

[0006] A self-supporting SiC / ZnS heterojunction nanoarray is provided. The nanoarray is prepared by performing anodization on a SiC substrate and then performing chemical bath deposition to grow ZnS on the SiC substrate.

[0007] The present invention also provides a method for preparing the above self-supporting SiC / ZnS heterojunction nanoarray, the method comprising the following steps:

[0008] S1, placing SiC in an electrolyte for anodization to obtain a single crystal integrated self-supporting SiC nanowire array;

[0009] S2. placing the single crystal integrated self-supporting SiC nanowire array in a Zn source solution in an oil bath, and finally washing and drying to obtain a self-supporting SiC / ZnS heterojunction nanoarray.

[0010] In the above-mentioned method for preparing a self-supporting SiC / ZnS heterojunction nanoarray, the electrolyte is a mixture of C2H5OH, HF and H2O2 in a volume ratio of (5-8):(2-5):1.

[0011] In the above-mentioned method for preparing a self-supporting SiC / ZnS heterojunction nanoarray, the number of anodizations is 3 times, wherein each anodization specifically comprises the following steps: first, anodizing at 15-20V for 0.5-2min, with a cycle of 0.6-1.0ms (T on =0.3-0.5ms, T off =0.3-0.5ms), then anodized at 25-35V for 150-250s, and after removing the surface cap layer, anodized again at 15-20V for 8-12min.

[0012] The present invention needs to strictly control the anodization time, because if the time is too short, the array structure cannot be formed on the surface of the SiC wafer, which reduces the light absorption capacity of the material. If the time is too long, the anodization depth is too large, the carrier transmission path is too long, resulting in carrier recombination and reducing the photoelectric performance.

[0013] In the above-mentioned method for preparing a self-supporting SiC / ZnS heterojunction nanoarray, the method for preparing a Zn source solution includes the following steps: uniformly mixing Zn(CH3COOH)2·2H2O and polyvinyl pyrrolidone to obtain a mixed solution, and then pouring the mixed solution into an aqueous solution containing CH3CSNH2 to mix to obtain a Zn source solution.

[0014] In the above-mentioned method for preparing a self-supporting SiC / ZnS heterojunction nanoarray, the mass ratio of Zn(CH3COOH)2·2H2O, polyvinyl pyrrolidone and CH3CSNH2 is (2.5-3.5):(1-5):1. The present invention strictly controls the ratio of Zn(CH3COOH)2·2H2O, polyvinyl pyrrolidone and CH3CSNH2, which can ensure that the reactants can be fully utilized and avoid the waste of raw materials. This precise ratio not only improves the synthesis efficiency of ZnS, but also enables ZnS to be evenly distributed in the SiC nanowire array, thereby optimizing the structure and performance of the SiC / ZnS heterojunction nanoarray. This uniform distribution helps to improve the carrier transmission performance and increase the photocurrent, and finally realizes a high-performance photoelectrochemical ultraviolet photodetector.

[0015] In the above-mentioned method for preparing a self-supporting SiC / ZnS heterojunction nanoarray, the oil bath temperature in step S2 is 80-120°C and the time is 20-30min. The present invention ensures that ZnS can be uniformly synthesized on the SiC nanowire array by controlling the oil bath temperature while avoiding unnecessary safety risks. If the temperature is too high, it may cause the solution to boil violently, increase the danger in the preparation process, and may destroy the uniform distribution of ZnS on the SiC nanowire array. On the other hand, if the temperature is too low, the synthesis process may become abnormally slow or even stop completely, which will directly affect the synthesis efficiency and quality of ZnS, and may ultimately lead to synthesis failure. Therefore, it is crucial for the present invention to accurately control the oil bath temperature to ensure that ZnS is uniformly synthesized into the SiC nanowire array and maintain a good reaction rate and safety.

[0016] In the above-mentioned method for preparing a self-supporting SiC / ZnS heterojunction nanoarray, the wavelength range of the light source absorbed by the self-supporting SiC / ZnS heterojunction nanoarray is 200-480nm.

[0017] The present invention provides a photoelectrochemical ultraviolet photodetector, wherein the working electrode of the photoelectrochemical ultraviolet photodetector is the above-mentioned self-supporting SiC / ZnS heterojunction nanoarray.

[0018] Preferably, the photoelectrochemical ultraviolet photodetector comprises:

[0019] The above-mentioned self-supporting SiC / ZnS heterojunction nanoarray, Pt electrode and Ag / AgCl (saturated KCl solution) electrode, wherein the SiC / ZnS heterojunction nanoarray material, Pt electrode and Ag / AgCl (saturated KCl solution) electrode are the working electrode, counter electrode and reference electrode respectively.

[0020] The present invention also provides a method for preparing the above-mentioned photoelectrochemical ultraviolet photodetector, which comprises the following steps: using the above-mentioned self-supporting SiC / ZnS heterojunction nanoarray as a working electrode, a Pt electrode as a counter electrode, and an Ag / AgCl (saturated KCl solution) electrode as a reference electrode, and assembling them into a typical three-electrode system using an electrochemical workstation (CHI660D, Shanghai Chenhua Instrument Co., Ltd., China); an electrolyte solution is arranged in a reaction container, the above-mentioned self-supporting electrode is detachably arranged on the container cover, the three electrodes are immersed in the electrolyte solution, and the container cover is closed on the reaction container to form a SiC / ZnS-based photoelectrochemical ultraviolet photodetector.

[0021] In the above-mentioned photoelectrochemical ultraviolet photodetector, the ultraviolet photodetector is under a bias voltage of 0.6 V and 27.1 mW / cm 2At low light power density, the photocurrent in 0.5 mol / L Na2SO4 solution can reach 750-850 μA / cm 2 .

[0022] Preferably, when a bias voltage is applied and ultraviolet light is applied, the photocurrent of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector increases with the increase of light intensity.

[0023] Preferably, when bias voltage is applied and ultraviolet light is applied, the photocurrent of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector increases with the increase of electrolyte concentration.

[0024] Preferably, when bias voltage is applied and ultraviolet light is applied, the photocurrent of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector is one order of magnitude higher than that of the pure SiC nanowire array-based photoelectrochemical ultraviolet photodetector.

[0025] Preferably, when bias voltage is applied and ultraviolet light is applied, in a Na2SO4 solution, the photocurrent of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector increases with the increase of the concentration of the Na2SO4 solution.

[0026] Preferably, at 27.1 mW / cm 2 Under low light power density, the light response time of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector is as low as 5ms.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. The SiC / ZnS heterojunction nanoarray of the present invention has a highly efficient absorption capability for light in the wavelength range of 200-480nm, especially at a wavelength of 375nm, achieving maximum light energy conversion efficiency.

[0029] 2. The appropriate amount of defects at the interface of the SiC / ZnS heterojunction nanoarray of the present invention not only prolongs the lifetime of carriers, but also provides additional active sites, further enhancing the generation of photocurrent.

[0030] 3. Compared with pure SiC nanowire array-based ultraviolet photodetectors, the SiC / ZnS-based photoelectrochemical ultraviolet photodetector of the present invention has increased the photocurrent intensity by at least one order of magnitude, showing significant performance advantages. This is mainly due to the unique structure of the SiC / ZnS heterojunction nanoarray of the present invention, the built-in electric field formed on the heterojunction interface optimizes the transmission of carriers and significantly enhances the photocurrent.

[0031] 4. The SiC / ZnS-based photoelectrochemical ultraviolet photodetector of the present invention is as low as 27.1 mW / cm 2Under the light power density of 1.5 GHz, it showed fast response capability, with rise and fall times of only 5 ms and 9 ms respectively, reflecting its excellent time resolution. In Na2SO4 solution, the detector also showed long-term operation stability and anti-aging stability, ensuring its reliability in various environments.

[0032] 5. The self-supporting SiC / ZnS heterojunction nanoarray of the present invention is prepared by anodization and chemical bath deposition, which has a simple process and low cost, creating conditions for large-scale production, indicating a broad prospect for the ultraviolet photodetector in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the preparation process of the self-supporting SiC / ZnS heterojunction nanoarray in Example 1 of the present invention.

[0034] Figure 2 This is a surface scanning electron microscope (SEM) image of the self-supporting SiC / ZnS heterojunction nanoarray at 500 nm in Example 1 of the present invention.

[0035] Figure 3 This is a surface scanning electron microscope (SEM) image of the self-supporting SiC / ZnS heterojunction nanoarray at 200 nm in Example 1 of the present invention.

[0036] Figure 4 This is a surface scanning electron microscope (SEM) image of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0037] Figure 5 This is a scanning electron microscope (SEM) image of a cross section at 10 μm of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0038] Figure 6 This is a cross-sectional scanning electron microscope (SEM) image of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention at 1 μm.

[0039] Figure 7 This is a projection electron microscope (TEM) image of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0040] Figure 8 This is an X-ray photoelectron spectroscopy (XPS) graph of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0041] Fig. 9 This is a high-resolution spectrum of Zn 2p of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0042] Fig.10 This is a high-resolution spectrum of S2p of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0043] Fig.11 This is a high-resolution spectrum of Si 2p of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0044] Fig.12 This is a high-resolution spectrum of C1s of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0045] Fig.13 This is a high-resolution spectrum of N1s of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0046] Fig.14 This is an X-ray diffraction (XRD) diagram of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0047] Fig.15 This is an ultraviolet-visible (UV-Vis) absorption spectrum of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 of the present invention.

[0048] Fig.16 The current-time (It) response curves of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 of Test 1 of the present invention and the pure SiC nanowire array-based photoelectrochemical ultraviolet photodetector in Comparative Example 1 after applying a 0.6V bias voltage and ultraviolet light irradiation in a 0.5mol / LNa2SO4 solution.

[0049] Fig.17 The current-light power density curves of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 and the pure SiC nanowire array-based photoelectrochemical ultraviolet photodetector in Comparative Example 1 after applying a bias voltage of 0.6V and ultraviolet light irradiation in 0.5mol / LNa2SO4 solution in Test 1 of the present invention.

[0050] Fig.18 The response rates (R) of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 and the pure SiC nanowire array-based photoelectrochemical ultraviolet photodetector in Comparative Example 1 under different light power densities in 0.5 mol / L Na2SO4 solution were applied with a bias voltage of 0.6 V and irradiated with ultraviolet light. λ )curve.

[0051] Fig.19The detection rates (D) of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 and the pure SiC nanowire array-based photoelectrochemical ultraviolet photodetector in Comparative Example 1 under different light power densities in 0.5 mol / L Na2SO4 solution with a bias voltage of 0.6 V and UV irradiation are shown in Table 1. * )curve.

[0052] Fig. 20 External quantum efficiency (EQE) curves of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 of Test 1 of the present invention and the pure SiC nanowire array-based photoelectrochemical ultraviolet photodetector in Comparative Example 1 at different light power densities after applying a 0.6V bias voltage and ultraviolet light irradiation in a 0.5mol / LNa2SO4 solution.

[0053] Fig.21 The rise and fall times of the transient current measured by the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 in Test 1 of the present invention in a 0.5 mol / L Na2SO4 solution.

[0054] Fig. 22 The current-time (It) response curves of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 in Test 2 of the present invention at different light power densities after applying a 0.6V bias voltage and ultraviolet light irradiation in a 0.1mol / L Na2SO4 solution.

[0055] Fig.23 The current-time (It) response curves of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 in Test 2 of the present invention at different light power densities after applying a 0.6V bias voltage and ultraviolet light irradiation in a 0.3mol / L Na2SO4 solution.

[0056] Fig.24 The current-time (It) response curves of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 in Test 2 of the present invention at different light power densities after applying a 0.6V bias voltage and ultraviolet light irradiation in a 0.5mol / L Na2SO4 solution.

[0057] Fig.25 The current-time (It) response curves of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 in Test 2 of the present invention in 0.1 mol / L Na2SO4 solution under self-powered conditions and after ultraviolet light irradiation at different light power densities.

[0058] Fig.26The current-time (It) response curves of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 in Test 2 of the present invention in 0.3 mol / L Na2SO4 solution under self-powered conditions and after ultraviolet light irradiation at different light power densities.

[0059] Fig. 27 The current-time (It) response curves of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 in Test 2 of the present invention in 0.5 mol / L Na2SO4 solution under self-powered conditions and after ultraviolet light irradiation at different light power densities.

[0060] Fig.28 They are respectively the stability test curves of a fresh self-supporting SiC / ZnS heterojunction nanoarray material-based photoelectrochemical ultraviolet photodetector prepared in Application Example 1 of the present invention and a SiC / ZnS heterojunction material-based photoelectrochemical ultraviolet photodetector stored for one month in a 0.5 mol / L Na2SO4 solution with a bias voltage of 0.6 V applied and after ultraviolet light irradiation for 2800 s.

[0061] Fig.29 They are respectively the stability test curves of a fresh self-supporting SiC / ZnS heterojunction nanoarray material-based photoelectrochemical ultraviolet photodetector prepared in Application Example 1 of the present invention and a SiC / ZnS heterojunction material-based photoelectrochemical ultraviolet photodetector stored for one month in a 0.5 mol / L Na2SO4 solution under self-powered conditions and after ultraviolet light irradiation for 2800 s.

[0062] Fig.30 This is a diagram of the self-powered energy band mechanism of the self-supporting SiC / ZnS heterojunction nanoarray material in Test 3 of the present invention. DETAILED DESCRIPTION

[0063] The technical scheme of the present invention is further described below by specific embodiments in conjunction with the accompanying drawings. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0064] Embodiment 1:

[0065] S1. Preparation of SiC / ZnO heterojunction materials: The preparation flow chart is as follows Figure 1As shown in Figure 2, the preparation of 4H-SiC nanowire arrays is based on the anodization method. First, the SiC sheet and the graphite plate are used as the anode and cathode, respectively. In a C2H5OH:HF:H2O2 electrolyte with a volume ratio of 6:3:1, the SiC sheet is anodized for 1 min at 17 V using a pulse power supply (SOYI-300-500-5M) with a cycle of 0.8 ms (T on =0.4ms, T off =0.4ms), so that a cap layer is formed on the top surface of the SiC sheet. Subsequently, the applied voltage is increased to 30V with a duty cycle of 100% for about 180 seconds, so that the previously formed cap layer is completely removed.

[0066] S2, performing a second anodization treatment in a C2H5OH:HF:H2O2 electrolyte having the same concentration volume ratio of 6:3:1 to obtain a single crystal integrated self-supporting SiC nanowire array, the anodization treatment is exactly the same as the anodization in step S1;

[0067] S3, 0.22 g of Zn(CH3COOH)2·2H2O and 0.15 g of polyvinylpyrrolidone (PVP) were mixed in a glass beaker containing 100 ml of deionized water and stirred for 5 min to obtain solution A;

[0068] Add 0.075 g of CH3CSNH2(TAA) into another beaker containing 50 ml of deionized water and stir for 10 min to obtain solution B;

[0069] While continuing to stir, quickly pour solution B into solution A to obtain a mixed solution;

[0070] S4. Place the anodized single crystal integrated self-supporting SiC nanowire array into the mixed solution of step S3, then place it in a 100° C. oil bath for 25 min, and finally wash it with deionized water for 3 times and dry it with nitrogen to obtain a self-supporting SiC / ZnS heterojunction nanoarray.

[0071] The structure of the self-supporting SiC / ZnS heterojunction nanoarray prepared above was characterized by scanning electron microscopy (FESEM, S-4800, Hitachi, Japan) and transmission electron microscopy (TEM, JEOL-2100F, JEOL, Japan). The surface SEM images are shown in Figure 2. Figure 2-7 As shown in the figure, it can be seen that after chemical bath deposition, the ZnS film grows around the SiC nanowires, forming the desired SiC / ZnS heterojunction structure. This structure effectively increases the contact area between the ZnS and SiC nanowires, thereby improving the transmission efficiency of electrons between the materials, which is crucial to improving the electronic conduction performance of the heterojunction.

[0072] The elemental analysis of the self-supporting SiC / ZnS heterojunction nanoarray prepared above was performed using an X-ray photoelectron spectroscopy analyzer (XPS, Thermo Scientific K-Alpha). The XPS graph is shown in FIG. Figure 8-13 As shown, the results confirm that the SiC / ZnS heterojunction sample is composed of five elements: Si, C, Zn, S and N, which is consistent with the expected composition of the composite material.

[0073] X-ray diffraction was used to characterize the structure of the prepared self-supporting SiC / ZnS heterojunction nanoarray. Fig.14 As shown in the figure, it is not difficult to see that the relevant diffraction peaks of 4H-SiC and ZnS appear simultaneously in the spectrum of SiC / ZnS heterojunction material, confirming the coexistence of ZnS and 4H-SiC in the composite material. The absence of any additional impurity peaks further confirms the high purity of the synthesized product.

[0074] The absorption characteristics of the prepared self-supporting SiC / ZnS heterojunction nanoarrays in the UV-Vis wavelength range were measured using UV-vis absorption spectroscopy (UV-vis, U-3900, Hitachi, Japan). Fig.15 As shown, it can be seen that the SiC / ZnS heterojunction material exhibits a high absorption characteristic for ultraviolet light with a wavelength below 400nm.

[0075] Application Example 1:

[0076] S1. The self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 was directly used as the working electrode, the Pt electrode was the counter electrode, and the Ag / AgCl (saturated KCl solution) electrode was the reference electrode, and assembled into a typical three-electrode system using an electrochemical workstation (CHI660D, Chenhua Instrument Co., Ltd., Shanghai, China).

[0077] S2. The electrolyte solution is arranged in the reaction container. The three-electrode system is detachably arranged on the container cover. The three electrodes are immersed in the electrolyte solution. The container cover is closed on the reaction container to form a SiC / ZnS-based photoelectrochemical ultraviolet photodetector. A light-transmitting window is fixedly arranged on the side wall of the reaction container for transmitting light.

[0078] Test 1: When the electrolyte solution is 0.5 mol / L Na2SO4 solution, a 0.6 V bias voltage and 375 nm light irradiation are applied in sequence to perform a performance test on the SiC / ZnS-based photoelectrochemical ultraviolet photodetector in Application Example 1.

[0079] Fig.16Pure SiC and the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 were directly used as photoanodes, and the photoelectric properties of the two were studied in Na2SO4 solution and at a light power density of 27.1 mW / cm 2 The results show that the photocurrent of the self-supporting SiC / ZnS heterojunction nanoarray is one order of magnitude higher than that of the pure SiC nanowire array, and the photocurrent value can reach 809.2μA / cm 2 The increase in photocurrent is mainly due to the formation of the heterojunction interface.

[0080] Fig.17 The photocurrent curves of the self-supporting SiC / ZnS heterojunction nanoarray prepared in Example 1 at different light power densities in Na2SO4 solution show that the photocurrent gradually increases with the increase of light power density. The specific data are shown in Table 1 below:

[0081] Table 1. Photocurrent data at different light power densities

[0082]

[0083] Figure 18-20 They are the response rates (R λ ), detection rate (D * ) and external quantum efficiency (EQE), it can be found that when the optical power density is fixed at level I, the SiC / ZnS-based photoelectrochemical UV photodetector shows excellent performance, and its R λ The value reaches 1226mA / W, D * The value can reach 2.52×10 11 The Jones,EQE value is 40.57%. The results show that the photodetector of Example 1 performs well in a low light power density environment. This is of great significance for application scenarios that require high sensitivity and high efficiency (such as nighttime monitoring in a low light environment).

[0084] Fig.21 The rise time and decay time of the transient current of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector prepared in Example 1 are shown in the curve. The millisecond response rate indicates that the SiC / ZnS-based photoelectrochemical ultraviolet photodetector has a rapid light response. This excellent performance is attributed to the structural characteristics of the SiC / ZnS heterojunction. The formation of the SiC / ZnS heterojunction introduces a new band structure and interface effect, which helps to absorb photons and separate carriers more efficiently. Due to the presence of the heterojunction, the photoexcited carriers can be separated and collected more quickly, thereby achieving a rapid response of the photodetector.

[0085] Figure 28-29 The long-term photocurrent-time response curve of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector freshly prepared and stored for one month in Example 1 is shown in Na2SO4 solution. It can be seen that the SiC / ZnS-based photoelectrochemical ultraviolet photodetector in Example 1 has good long-term stability and good anti-aging stability in Na2SO4 solution within 2800s.

[0086] Test 2: The electrolyte solution was 0.1 mol / L, 0.3 mol / L, and 0.5 mol / L Na2SO4 solution. The SiC / ZnS-based photoelectrochemical ultraviolet photodetector in Application Example 1 was placed therein, and a 0.6 V bias voltage and 375 nm light irradiation were applied in sequence to perform performance tests.

[0087] Figure 22-24 The photocurrent curves of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector in Application Example 1 at different light power densities in Na2SO4 solutions of different concentrations are shown. It has reliable ultraviolet light detection performance in Na2SO4 solutions of different concentrations. The photocurrent increases with the increase of light intensity, further revealing the high sensitivity of PD to light power density. In addition, the light response of the SiC / ZnS-based PEC UV PD decreases significantly with the decrease of the concentration of Na2SO4 solution, showing the high sensitivity of the device to the concentration of the solution. These sensitivities mainly come from the fact that the concentration and migration ability of ions in the solution greatly affect the size of the photocurrent. When the ion concentration in the solution is low, less charge is generated on the surface of the photoelectrode, resulting in less charge migration and smaller photocurrent.

[0088] Test 3: The electrolyte solution was 0.1 mol / L, 0.3 mol / L, and 0.5 mol / L Na2SO4 solution, and the SiC / ZnS-based photoelectrochemical ultraviolet photodetector in Example 2 was placed therein, and the performance was tested under self-powered conditions and 375 nm light irradiation.

[0089] Figure 25-27 The self-powered photocurrent curves of the SiC / ZnS-based photoelectrochemical UV photodetector in Example 1 at different light power densities in Na2SO4 solutions of different concentrations are shown. It can be seen that even under self-powered conditions, the SiC / ZnS-based PEC UV PD still has good light response performance. Its maximum photocurrent can reach 190.6μA / cm 2 .

[0090] This is because Fig.30As shown in the figure, since ZnS and SiC have different lattice structures and energy band structures, a heterojunction interface is formed at the contact point. When the SiC / ZnS heterojunction interface is formed, charge transfer occurs due to the difference in electron affinity and bandgap width between the two materials, resulting in the formation of a built-in electric field near the interface. This built-in electric field helps to separate photogenerated electrons and holes. At the same time, the separated electrons and holes move to the platinum electrode and the SiC / ZnS electrode respectively, and participate in the redox reaction at the electrolyte interface to generate H2 and O2, ultimately completing the charge exchange of the entire circuit.

[0091] Comparative Example 1:

[0092] The only difference from Example 1 is that in Comparative Example 1, the SiC nanowire array is not subjected to chemical bath deposition, and the anodized pure SiC nanowire array is directly made into a photoanode using the same preparation method as Example 1, and used as a working electrode to assemble a photoelectrochemical ultraviolet photodetector.

[0093] Fig.16 The current-time (It) response curve after applying a 0.6V bias voltage and ultraviolet light irradiation in a 0.5mol / L Na2SO4 solution. It can be clearly observed that the photocurrent of the SiC / ZnS heterojunction nanoarray prepared in Example 1 is one order of magnitude higher than that of the SiC nanowire array prepared in Comparative Example 1. The increase in photocurrent is mainly due to the formation of the heterojunction interface. First, the formation of the heterojunction interface leads to an enhanced charge separation effect. In the SiC / ZnS heterojunction material, due to the different electron affinities and energy gap sizes of the two materials, an energy level shift is formed at the interface after light excitation, thereby forming a coupling region of electrons and holes. This coupling region makes the separation of photogenerated carriers more efficient. Secondly, the heterojunction changes the transport and diffusion characteristics of carriers in the material. The formation of the SiC / ZnS heterojunction increases the mobility and diffusion length of carriers in the material, thereby increasing the collection efficiency of photogenerated carriers. At the same time, the formation of SiC / ZnS heterojunction leads to the enhancement of the surface reaction activity of the material, changes the chemical properties of the material surface, and improves the surface light absorption and photoelectric conversion efficiency. Some additional interface states will also be formed on the heterojunction interface. These interface states have an important influence on the transport and recombination of carriers, which can further improve the efficiency of photocurrent generation. The synergistic effect of these factors enables SiC / ZnS heterojunction materials to generate photogenerated carriers more efficiently, which undoubtedly shows that heterojunction materials have a significant enhancement effect in photocurrent generation.

[0094] Comparative Example 2:

[0095] The only difference from Example 1 is that in Comparative Example 2, SiC is not subjected to anodization treatment, but is directly prepared by chemical bath deposition, and then prepared as a photoanode using the same preparation method as Example 1, and used as a working electrode to assemble a photoelectrochemical ultraviolet photodetector.

[0096] In Comparative Example 2, the SiC wafer that has not undergone the anodization process cannot form a nanowire array structure on its surface, so that the light absorption capacity is greatly reduced compared to the SiC wafer that has formed an array structure, ultimately resulting in poor photoelectric performance.

[0097] Comparative Example 3:

[0098] The only difference from Example 1 is that the anodization is performed once, and the secondary anodization in step S2 is not performed to obtain the array. Then, the same preparation method as in Example 1 is used to make the photoanode, and the working electrode is used to assemble the photoelectrochemical ultraviolet photodetector.

[0099] In Comparative Example 3, the SiC wafer that has not undergone secondary anodization cannot form a complete nanowire array structure because the total anodization time is short, resulting in a lower light absorption capacity than the SiC wafer with a complete array structure, ultimately leading to poor photoelectric performance.

[0100] In summary, the SiC / ZnS-based photoelectrochemical ultraviolet photodetector of the present invention has excellent light response capability, which is one order of magnitude higher than the photocurrent of the pure SiC nanowire array-based photoelectrochemical ultraviolet photodetector, and has high sensitivity to solution concentration; it has fast response capability; it has excellent long-term operation stability and good anti-aging stability in Na2SO4 solution; it exhibits excellent sensitivity to light signals, detector response capability and input light signal capture capability at low light power density. In addition, the synthesis method of SiC / ZnS heterojunction material is simple, the production cost is low, and large-scale production can be achieved. The improvement of the SiC / ZnS-based photoelectrochemical ultraviolet photodetector of the present invention is mainly attributed to the effective synergistic effect of the heterojunction interface effect, cutoff wavelength and interface defects of the SiC / ZnS heterojunction material.

[0101] The parts of the embodiments herein that are not exhaustive of the midpoint values ​​of the technical scope claimed for protection by the present invention and the new technical solutions formed by equivalent replacement of single or multiple technical features in the technical solutions of the embodiments are also within the scope claimed for protection by the present invention; at the same time, in all the listed or unlisted embodiments of the scheme of the present invention, each parameter in the same embodiment merely represents an example of its technical solution (i.e., a feasible solution), and there is no strict coordination and limitation relationship between the parameters, wherein the parameters can be replaced with each other without violating the axioms and the claims of the present invention, unless otherwise stated.

[0102] The technical means disclosed in the scheme of the present invention are not limited to the technical means disclosed in the above technical means, but also include technical schemes composed of any combination of the above technical features. The above is a specific implementation of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also regarded as the protection scope of the present invention.

[0103] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A self-supporting SiC / ZnS heterojunction nanoarray, characterized in that: The nanoarray is grown on a SiC substrate by anodizing the SiC substrate and then performing chemical bath deposition on the SiC substrate.

2. A method for preparing the self-supporting SiC / ZnS heterojunction nanoarray according to claim 1, characterized in that: The method comprises the following steps: S1, placing SiC in an electrolyte for anodization to obtain a single crystal integrated self-supporting SiC nanowire array; S2. placing the single crystal integrated self-supporting SiC nanowire array in a Zn source solution in an oil bath, and finally washing and drying to obtain a self-supporting SiC / ZnS heterojunction nanoarray.

3. The method for preparing a self-supporting SiC / ZnS heterojunction nanoarray according to claim 1, characterized in that: The electrolyte is a mixture of C2H5OH, HF and H2O2 in a volume ratio of (5-8):(2-5):

1.

4. The method for preparing a self-supporting SiC / ZnS heterojunction nanoarray according to claim 2, characterized in that: The number of anodizations was 3 times, wherein each anodization step specifically included the following steps: first, anodization at 15-20 V for 0.5-2 min, with a cycle of 0.6-1.0 ms (T on =0.3-0.5ms, T off =0.3-0.5ms), then anodized at 25-35V for 150-250s, and after removing the surface cap layer, anodized again at 15-20V for 8-12min.

5. The method for preparing a self-supporting SiC / ZnS heterojunction nanoarray according to claim 2, characterized in that: The preparation method of the Zn source solution comprises the following steps: uniformly mixing Zn(CH3COOH)2·2H2O and polyvinyl pyrrolidone to obtain a mixed solution, and then pouring the mixed solution into an aqueous solution containing CH3CSNH2 to obtain a Zn source solution.

6. The method for preparing a self-supporting SiC / ZnS heterojunction nanoarray according to claim 5, characterized in that: The mass ratio of Zn(CH3COOH)2·2H2O, polyvinyl pyrrolidone and CH3CSNH2 is (2.5-3.5):(1-5):

1.

7. The method for preparing a self-supporting SiC / ZnS heterojunction nanoarray according to claim 1, characterized in that: The oil bath temperature in step S2 is 80-120°C and the time is 20-30 minutes.

8. The method for preparing a self-supporting SiC / ZnS heterojunction nanoarray according to claim 1, characterized in that: The wavelength range of the light source absorbed by the self-supporting SiC / ZnS heterojunction nanoarray is 200-480nm.

9. A photoelectrochemical ultraviolet photodetector, characterized in that: The working electrode of the photoelectrochemical ultraviolet photodetector is the self-supporting SiC / ZnS heterojunction nanoarray as described in claim 1.

10. The photoelectrochemical ultraviolet photodetector according to claim 9, characterized in that: The UV photodetector is biased at 0.6 V and 27.1 mW / cm 2 At low light power density, the photocurrent in 0.5 mol / L Na2SO4 solution can reach 750-850 μA / cm 2 .