Electrode bonding pad manufacturing method, light emitting diode and manufacturing method
Through the production method of electrode pads for vapor-depositing AuSn layer in two sections, the problem of poor welding stability of light emitting diode packaging is solved, ensuring the stable Au:Sn ratio and improving welding performance and reliability.
Patent Information
- Application Number
- CN202410892397.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-22
AI Technical Summary
The packaging welding stability of the light emitting diodes is poor, resulting in low reliability.
The electrode pad production method of two-stage evaporated AuSn layer is used to ensure that the Au:Sn ratio is stable at 8:2. Two AuSn crucibles are used for evaporation through the electron beam evaporation process to ensure the stable quality of the pad surface.
The welding stability and reliability of the light emitting diodes are improved, the proportional imbalance of gold-tin alloys is avoided during the evaporation process, and the welding performance between the pad and the packaging bracket is enhanced.
Smart Images

Figure CN119008807A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of light-emitting devices, and in particular to an electrode pad manufacturing method, a light-emitting diode and a manufacturing method thereof. Background Art
[0002] Light-emitting diodes are often used in display panels, lighting and other fields.
[0003] The related technology provides a light-emitting diode, which includes: a first semiconductor layer, an active layer and a second semiconductor layer stacked in sequence; an electrode connected to the semiconductor layer; a passivation layer covering the semiconductor layer and the electrode; and a pad penetrating the passivation layer and connected to the electrode structure.
[0004] However, the light emitting diode of the above structure has the problem of poor packaging welding stability, resulting in poor reliability of the light emitting diode. Summary of the invention
[0005] The embodiments of the present disclosure provide an electrode pad manufacturing method, a light emitting diode and a manufacturing method, which can improve the reliability of the light emitting diode. The technical solution is as follows:
[0006] In one aspect, a method for manufacturing an electrode pad is provided, the method comprising:
[0007] sequentially evaporating a metal stack and a protective layer;
[0008] The AuSn layer is deposited on the protective layer in two stages. The thickness of the first stage is The second stage evaporation thickness is
[0009] Optionally, the AuSn layer is evaporated on the protective layer in two stages, comprising:
[0010] Using the first crucible containing AuSn, electron beam evaporation was used to The first AuSn layer is evaporated at a deposition rate of
[0011] Using a second crucible containing AuSn, electron beam evaporation was performed to The second AuSn layer was evaporated at a deposition rate of .
[0012] Optionally, the sequentially evaporating and stacking the metal stack and the protective layer comprises:
[0013] sequentially evaporating a first Ti layer, a first Al layer, a second Ti layer, and a second Al layer as a metal stack;
[0014] A third Ti layer and a Pt layer are sequentially deposited on the metal stack as a protective layer.
[0015] Optionally, the sequentially evaporated stacked first Ti layer, first Al layer, second Ti layer and second Al layer as a metal stack comprises:
[0016] Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The first Ti layer;
[0017] Using a crucible containing Al, electron beam evaporation was used to The evaporation rate, evaporation The first Al layer;
[0018] Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The second Ti layer;
[0019] Using a crucible containing Al, electron beam evaporation was used to The evaporation rate, evaporation The second Al layer.
[0020] Optionally, a third Ti layer and a Pt layer are sequentially deposited on the metal stack as a protective layer, comprising:
[0021] Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The third Ti layer;
[0022] Using a crucible containing Pt, electron beam evaporation was used to The evaporation rate, evaporation of Pt layer.
[0023] In another aspect, a light emitting diode is provided, the light emitting diode comprising:
[0024] A first semiconductor layer, an active layer, and a second semiconductor layer are sequentially stacked, wherein the first semiconductor layer, the active layer, and the second semiconductor layer form a step structure;
[0025] A silver mirror structure, wherein the silver mirror structure is located on the surface of the second semiconductor layer;
[0026] a first passivation layer, wherein the first passivation layer covers the step structure and the silver mirror structure;
[0027] a first electrode and a second electrode, the first electrode penetrating the first passivation layer and connected to the first semiconductor, and the second electrode penetrating the first passivation layer and connected to the silver mirror structure;
[0028] a second passivation layer, the second passivation layer covering the first passivation layer, the first electrode and the second electrode;
[0029] a first electrode pad and a second electrode pad, the first electrode pad passing through the second passivation layer and connected to the first electrode, and the second electrode pad passing through the second passivation layer and connected to the second electrode;
[0030] The first electrode pad and the second electrode pad each include a metal stack, a protective layer and an AuSn layer. The AuSn layer is evaporated in two stages. The thickness of the first stage is The second stage evaporation thickness is
[0031]
[0032] Optionally, the metal stack includes a first Ti layer, a first Al layer, a second Ti layer and a second Al layer stacked in sequence, and the protective layer includes a third Ti layer and a Pt layer stacked in sequence.
[0033] Optionally, the thickness of the first Ti layer is The thickness of the first Al layer is The thickness of the second Ti layer is The thickness of the second Al layer is The thickness of the third Ti layer is The thickness of the Pt layer is The thickness of the AuSn layer is
[0034] In another aspect, a method for manufacturing a light emitting diode is provided, the method comprising:
[0035] Sequentially manufacturing a first semiconductor layer, an active layer, and a second semiconductor layer, wherein the first semiconductor layer, the active layer, and the second semiconductor layer form a step structure;
[0036] Manufacturing a silver mirror structure, wherein the silver mirror structure is located on the surface of the second semiconductor layer;
[0037] Manufacturing a first passivation layer, wherein the first passivation layer covers the step structure and the silver mirror structure;
[0038] Manufacturing a first electrode and a second electrode, wherein the first electrode penetrates the first passivation layer and is connected to the first semiconductor, and the second electrode penetrates the first passivation layer and is connected to the silver mirror structure;
[0039] Manufacturing a second passivation layer, wherein the second passivation layer covers the first passivation layer, the first electrode and the second electrode;
[0040] A first electrode pad and a second electrode pad are manufactured, wherein the first electrode pad penetrates the second passivation layer and is connected to the first electrode, and the second electrode pad penetrates the second passivation layer and is connected to the second electrode; the first electrode pad and the second electrode pad are manufactured in the following manner: a metal stack and a protective layer are sequentially deposited; an AuSn layer is deposited on the protective layer in two stages, and the thickness of the first stage is The second stage evaporation thickness is
[0041] Optionally, the AuSn layer is evaporated on the protective layer in two stages, comprising:
[0042] Using the first crucible containing AuSn, electron beam evaporation was used to The first AuSn layer is evaporated at a deposition rate of
[0043] Using a second crucible containing AuSn, electron beam evaporation was performed to The second AuSn layer was evaporated at a deposition rate of .
[0044] The technical solution provided by the embodiments of the present disclosure has the following beneficial effects:
[0045] In the method for manufacturing an electrode pad for a light-emitting diode provided in the embodiment of the present disclosure, the AuSn layer is evaporated in two stages, wherein the first stage is the Second stage evaporation Since the thickness of the second stage of evaporation is relatively thin, the ratio of An and Sn in the second stage of evaporation can be ensured to be relatively stable, stable at the desired Au:Sn=8:2, thereby ensuring the stability of the quality of the surface of the AuSn layer, and making the welding between the pad surface and the packaging bracket have good stability, thereby improving the reliability of the light-emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0047] Figure 1 is a flow chart of a method for manufacturing an electrode pad provided by an embodiment of the present disclosure;
[0048] Figure 2 is a structural schematic diagram of a light emitting diode provided by an embodiment of the present disclosure;
[0049] Figure 3 is a structural schematic diagram of a welding pad provided by an embodiment of the present disclosure;
[0050] Figure 4 is a flow chart of a method for manufacturing a light emitting diode provided by an embodiment of the present disclosure;
[0051] Figure 5 This is a flow chart of another method for manufacturing a light emitting diode provided in an embodiment of the present disclosure.
[0052] The reference numerals are as follows:
[0053] 100: substrate; 101: first semiconductor layer; 102: active layer; 103: second semiconductor layer; 104: transparent conductive layer; 105: silver mirror structure; 106: first passivation layer; 107: first electrode; 108: second electrode; 109: second passivation layer; 110: first electrode pad; 111: second electrode pad; 112: first through hole; 113: second through hole; 114: third through hole; 115: fourth through hole; 201: metal stack; 202: protective layer; 203: AuSn layer. DETAILED DESCRIPTION
[0054] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.
[0055] Figure 1 is a flow chart of a method for manufacturing an electrode pad provided by an embodiment of the present disclosure. Figure 1 , the method comprising:
[0056] S10, sequentially evaporating a metal stack and a protective layer.
[0057] S20, vapor-depositing an AuSn (gold-tin alloy) layer on the protective layer in two stages.
[0058] Among them, the first stage evaporation thickness is The second stage evaporation thickness is
[0059] In the method for manufacturing an electrode pad for a light-emitting diode provided in the embodiment of the present disclosure, the AuSn layer is evaporated in two stages, wherein the first stage is the Second stage evaporation Since the thickness of the second stage of evaporation is relatively thin, the ratio of An and Sn in the second stage of evaporation can be ensured to be relatively stable, stable at the desired Au:Sn=8:2, thereby ensuring the stability of the quality of the surface of the AuSn layer, and making the welding between the pad surface and the packaging bracket have good stability, thereby improving the reliability of the light-emitting diode.
[0060] When the gold-tin alloy begins to be evaporated, the ratio of gold to tin is normal. If the thickness of the evaporated gold-tin is thicker, the evaporation time will be longer. The gold-tin alloy is in a liquid state during the evaporation process. The mass of gold is greater than the mass of tin. If it stays in the liquid state for a long time, the gold will sink to the bottom of the crucible, and the tin will be above the crucible due to its lighter mass. At this time, the ratio of gold to tin in the evaporated gold-tin film will be unbalanced. The segmented evaporation can improve the above problems in the second evaporation stage, thereby ensuring the stable quality of the AuSn layer surface.
[0061] In one example, step S10 may include:
[0062] sequentially evaporating a first Ti layer, a first Al layer, a second Ti layer, and a second Al layer as a metal stack;
[0063] A third Ti layer and a Pt layer are sequentially deposited on the metal stack as a protective layer.
[0064] In this implementation, the metal stack and protective layer of the electrode pad are formed in the above-mentioned manner, wherein the Ti layer mainly plays an adhesion role; the Al layer plays a reflective and conductive role and has a low cost; the Pt layer blocks AuSn from forming an alloy with Al; the AuSn layer has high conductivity, and the packaging does not require solder paste, reducing the packaging cost.
[0065] In other examples, at least one of the metal stack and the protective layer may also be other film layer structures, which is not limited in the embodiments of the present disclosure.
[0066] The first Ti layer, the first Al layer, the second Ti layer and the second Al layer sequentially deposited and stacked as a metal stack may include:
[0067] Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The first Ti layer;
[0068] Using a crucible containing Al, electron beam evaporation was used to The evaporation rate, evaporation The first Al layer;
[0069] Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The second Ti layer;
[0070] Using a crucible containing Al, electron beam evaporation was used to The evaporation rate, evaporation The second Al layer.
[0071] In this implementation, each metal stack is manufactured with the above-mentioned evaporation rate and thickness, which can ensure the electrical conductivity and light reflection properties of the pad.
[0072] Wherein, a third Ti layer and a Pt layer are sequentially deposited on the metal stack as a protective layer, comprising:
[0073] Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The third Ti layer;
[0074] Using a crucible containing Pt, electron beam evaporation was used to The evaporation rate, evaporation of Pt layer.
[0075] In this implementation, each protective layer is manufactured using the above-mentioned evaporation rate and thickness, which can ensure the barrier effect of the protective layer and the adhesion effect with other film layers.
[0076] In one example, step S20 may include:
[0077] Using the first crucible containing AuSn, electron beam evaporation was used to The first AuSn layer is evaporated at a deposition rate of
[0078] Using a second crucible containing AuSn, electron beam evaporation was performed to The second AuSn layer was evaporated at a deposition rate of .
[0079] In this implementation, the above evaporation rate is adopted and two crucibles are used to produce the AuSn layer. On the one hand, the two-stage evaporation of AuSn can be ensured, and on the other hand, the second stage evaporation can obtain a thinner AuSn layer, thereby ensuring the stable quality of the AuSn layer surface.
[0080] In this implementation, two crucibles are used so that the gold has not sunk to the bottom of the crucible during the second stage of evaporation, thereby ensuring the stability of the quality of the surface of the AuSn layer.
[0081] In this implementation, the above-mentioned evaporation rate is used to avoid wasting machine production capacity due to a low rate, and at the same time avoid the problem that the evaporation power corresponding to the low rate is low, the gold-tin alloy is not fully melted, and gold-tin particles are generated, which affects the welding effect.
[0082] Exemplarily, the thickness of the first Ti layer is The thickness of the first Al layer is The thickness of the second Ti layer is The thickness of the second Al layer is The thickness of the third Ti layer is The thickness of the Pt layer is The thickness of the first AuSn layer 203 is The thickness of the second AuSn layer is
[0083] Exemplarily, the evaporation rate of the first Ti layer is The evaporation rate of the first Al layer is The evaporation rate of the second Ti layer is The evaporation rate of the second Al layer is The evaporation rate of the third Ti layer is The thickness of the Pt layer is 1.5×10 evaporation rate. The evaporation rate of the first AuSn layer is The evaporation rate of the second AuSn layer is
[0084] In the disclosed embodiment, when the electrode pad is evaporated, the vacuum degree in the metal evaporation chamber is 3.0E-7Pa and the temperature is 23°C-50°C.
[0085] Figure 2 is a schematic diagram of the structure of a light emitting diode provided by an embodiment of the present disclosure. Figure 2 The light emitting diode includes: a substrate 100, a first semiconductor layer 101, an active layer 102, a second semiconductor layer 103, a silver mirror structure 105, a first passivation layer 106, a first electrode 107, a second electrode 108, a second passivation layer 109, a first electrode pad 110 and a second electrode pad 111.
[0086] A first semiconductor layer 101 , an active layer 102 , and a second semiconductor layer 103 are sequentially stacked on the surface of the substrate 100 , and the first semiconductor layer 101 , the active layer 102 , and the second semiconductor layer 103 form a step structure.
[0087] The silver mirror structure 105 is located on the surface of the second semiconductor layer 103 .
[0088] A first passivation layer 106 , wherein the first passivation layer 106 covers the step structure and the silver mirror structure 105 .
[0089] A first electrode 107 and a second electrode 108 , wherein the first electrode 107 penetrates the first passivation layer 106 and is connected to the first semiconductor 101 , and the second electrode 108 penetrates the first passivation layer 106 and is connected to the silver mirror structure 105 .
[0090] The second passivation layer 109 covers the first passivation layer 106 , the first electrode 107 and the second electrode 108 .
[0091] A first electrode pad 110 and a second electrode pad 111 , wherein the first electrode pad 110 penetrates the second passivation layer 109 and is connected to the first electrode 107 , and the second electrode pad 111 penetrates the second passivation layer 109 and is connected to the second electrode 108 .
[0092] Figure 3 is a schematic diagram of the structure of the first electrode pad / second electrode pad provided by the embodiment of the present disclosure. Figure 3 The first electrode pad 110 and the second electrode pad 111 both include a metal stack 201, a protective layer 202 and an AuSn layer 203. The AuSn layer 203 is evaporated in two stages. The thickness of the first stage is The second stage evaporation thickness is Figure 3 The two parts on both sides of the dotted line in the AuSn layer 203 are formed by two-stage vapor deposition.
[0093] In the first electrode pad and the second electrode pad of the light-emitting diode provided in the embodiment of the present disclosure, the AuSn layer is evaporated in two stages, wherein the first stage is evaporated Second stage evaporation Since the thickness of the second stage of evaporation is relatively thin, the ratio of An and Sn in the second stage of evaporation can be ensured to be relatively stable, stable at the desired Au:Sn=8:2, thereby ensuring the stability of the quality of the surface of the AuSn layer, and making the welding between the pad surface and the packaging bracket have good stability, thereby improving the reliability of the light-emitting diode.
[0094] It should be noted that Figure 3 The diagram only shows the stacking diagram of the first electrode pad / the second electrode pad. The actual structure of the first electrode pad / the second electrode pad is related to the overall structure of the light emitting diode. Figure 2 In the light emitting diode, the edge of the first electrode pad / the second electrode pad may be located on the surface of the second passivation layer, and the middle of the first electrode pad / the second electrode pad is located above the through hole.
[0095] In the embodiment of the present disclosure, the substrate 100 may be any one of a sapphire substrate, a silicon substrate, etc., and the present disclosure does not limit the material of the substrate.
[0096] Exemplarily, the substrate 100 is a sapphire substrate.
[0097] In the embodiment of the present disclosure, the first semiconductor layer 101 may be an N-type semiconductor layer, the active layer 102 may be a multi-quantum well layer, and the second semiconductor layer 103 may be a P-type semiconductor layer.
[0098] Exemplarily, the first semiconductor layer 101 is an N-type GaN layer, the active layer 102 is an InGaN / GaN layer, and the second semiconductor layer 103 is a P-type GaN layer.
[0099] In another example, the first semiconductor layer 101 may be a P-type semiconductor layer, the active layer 102 may be a multi-quantum well layer, and the second semiconductor layer 103 may be an N-type semiconductor layer.
[0100] In the embodiment of the present disclosure, the silver mirror structure 105 includes a reflective layer and a barrier layer, wherein the barrier layer covers the surface and side surfaces of the reflective layer.
[0101] In the embodiment of the present disclosure, the reflective layer includes at least an Ag layer, and the barrier layer may include a combination of multiple layers of a Cr layer, an Al layer, a Ti layer, a Ni layer, a Pt layer, and an Au layer.
[0102] In the embodiment of the present disclosure, the reflective layer includes an Ag layer and a TiW layer stacked in sequence, and the barrier layer includes a Cr layer, an Al layer, a Ti layer, a Ni layer, a Pt layer and an Au layer stacked in sequence.
[0103] Optionally, the light emitting diode further includes: a transparent conductive layer 104 located between the second semiconductor layer 103 and the silver mirror structure 105 .
[0104] In the embodiment of the present disclosure, the transparent conductive layer 104 may be an indium tin oxide (ITO) layer.
[0105] In the embodiment of the present disclosure, the first passivation layer 106 and the second passivation layer 109 can be SiO2 layer, TiO2 layer, Al2O3, SiN x Any one or more of the above insulating films, x is greater than 0.
[0106] In the embodiments of the present disclosure, the passivation layer formed by the above materials has a good passivation effect. Wherein, when the passivation layer includes a single film layer, it can be any one or more of the above film layers; the passivation layer can also include multiple film layers, and the multiple film layers can be formed by different insulating materials. The passivation layer formed by stacking multiple film layers can further increase the film quality of the passivation layer, so that the passivation layer is not easily broken by metal particles.
[0107] In the embodiment of the present disclosure, the first passivation layer 106 has a first through hole 112 and a second through hole 113 . The first through hole 112 penetrates the first passivation layer 106 and communicates with the first semiconductor layer 101 . The second through hole 113 penetrates the first passivation layer 106 and communicates with the silver mirror structure 105 .
[0108] In the embodiment of the present disclosure, the second passivation layer 109 has a third through hole 114 and a fourth through hole 115 . The third through hole 114 penetrates the second passivation layer 109 and communicates with the first electrode 107 . The fourth through hole 115 penetrates the second passivation layer 109 and communicates with the second electrode 108 .
[0109] In the embodiment of the present disclosure, the first electrode 107 and the second electrode 108 include a Cr layer, an Al layer, a Ti layer, a Ni layer, a Pt layer, and an Au layer stacked in sequence.
[0110] In one example, when the first semiconductor layer 101 is an N-type semiconductor layer, the first electrode 107 is an N-electrode, and the first electrode pad 110 is an N-electrode pad; when the second semiconductor layer 103 is a P-type semiconductor layer, the second electrode 108 is a P-electrode, and the second electrode pad 111 is a P-electrode pad.
[0111] In another example, when the first semiconductor layer 101 is a P-type semiconductor layer, the first electrode 107 is a P-electrode, and the first electrode pad 110 is a P-electrode pad; when the second semiconductor layer 103 is an N-type semiconductor layer, the second electrode 108 is an N-electrode, and the second electrode pad 111 is an N-electrode pad.
[0112] See again Figure 3 The metal stack 201 includes a first Ti layer ( Figure 3 Ti#1 in the middle), the first Al layer ( Figure 3 Al#1 in the middle), the second Ti layer ( Figure 3 Ti#2 in the middle) and the second Al layer ( Figure 3 The protective layer 202 includes a third Ti layer ( Figure 3 Ti#3) and Pt layers.
[0113] In the disclosed embodiment, the Ti layer mainly plays an adhesion role; the Al layer plays a reflective and conductive role and has a lower cost; the Pt layer blocks AuSn from forming an alloy with Al; the AuSn layer has high conductivity, and the packaging does not require solder paste, reducing the packaging cost.
[0114] In the embodiment of the present disclosure, the thickness of the first Ti layer is The thickness of the first Al layer is The thickness of the second Ti layer is The thickness of the second Al layer is The thickness of the third Ti layer is The thickness of the Pt layer is The thickness of the AuSn layer 203 in the first stage of evaporation is The second stage evaporation thickness is
[0115] By using the above-mentioned thickness to make each metal layer, the electrical conductivity and light reflection properties of the pad can be ensured.
[0116] Exemplarily, the thickness of the first Ti layer is The thickness of the first Al layer is The thickness of the second Ti layer is The thickness of the second Al layer is The thickness of the third Ti layer is The thickness of the Pt layer is The thickness of the first AuSn layer 203 is The thickness of the second AuSn layer 203 is The thickness given in this example is the thickness in the middle of each metal layer. Figure 3 It can be seen that the thickness of the edges of each metal layer changes gradually, for example, gradually decreases from the middle to the edge.
[0117] Figure 4 A method for manufacturing a light emitting diode is provided in an embodiment of the present disclosure. Figure 4 The method steps include:
[0118] S11, sequentially manufacturing a first semiconductor layer, an active layer, and a second semiconductor layer, wherein the first semiconductor layer, the active layer, and the second semiconductor layer form a step structure.
[0119] In the embodiment of the present disclosure, the first semiconductor layer may be an N-type semiconductor layer, the active layer may be a multi-quantum well layer, and the second semiconductor layer may be a P-type semiconductor layer.
[0120] Exemplarily, the first semiconductor layer is an N-type GaN layer, the active layer is an InGaN / GaN layer, and the second semiconductor layer is a P-type GaN layer.
[0121] S12, manufacturing a silver mirror structure, wherein the silver mirror structure is located on the surface of the second semiconductor layer.
[0122] S13, manufacturing a first passivation layer, wherein the first passivation layer covers the step structure and the silver mirror structure.
[0123] S14, manufacturing a first electrode and a second electrode, wherein the first electrode penetrates the first passivation layer and is connected to the first semiconductor, and the second electrode penetrates the first passivation layer and is connected to the silver mirror structure.
[0124] In the embodiment of the present disclosure, when the first semiconductor layer is an N-type semiconductor layer, the first electrode is an N-electrode, and when the second semiconductor layer is a P-type semiconductor layer, the second electrode is a P-electrode.
[0125] S15. Manufacturing a second passivation layer, wherein the second passivation layer covers the first passivation layer, the first electrode and the second electrode.
[0126] S16. Fabricate a first electrode pad and a second electrode pad, wherein the first electrode pad penetrates the second passivation layer and is connected to the first electrode, and the second electrode pad penetrates the second passivation layer and is connected to the second electrode.
[0127] The first electrode pad and the second electrode pad are both manufactured in the following manner: a metal stack and a protective layer are sequentially deposited; an AuSn layer is deposited on the protective layer in two stages, and the thickness of the first stage is The second stage evaporation thickness is
[0128] In the method for manufacturing an electrode pad for a light-emitting diode provided in the embodiment of the present disclosure, the AuSn layer is evaporated in two stages, wherein the first stage is the Second stage evaporation Since the thickness of the second stage of evaporation is relatively thin, the ratio of An and Sn in the second stage of evaporation can be ensured to be relatively stable, stable at the desired Au:Sn=8:2, thereby ensuring the stability of the quality of the surface of the AuSn layer, and making the welding between the pad surface and the packaging bracket have good stability, thereby improving the reliability of the light-emitting diode.
[0129] Figure 5 This is a flow chart of another method for manufacturing a light emitting diode provided in an embodiment of the present disclosure. Figure 5 The method steps include:
[0130] S21. A first semiconductor layer, an active layer, and a second semiconductor layer are sequentially formed on a surface of a substrate, wherein the first semiconductor layer, the active layer, and the second semiconductor layer form a step structure.
[0131] In the embodiment of the present disclosure, the first semiconductor layer is an N-type GaN layer, the active layer is an InGaN / GaN layer, and the second semiconductor layer is a P-type GaN layer.
[0132] In one example, step S21 includes:
[0133] The first step is to grow the first semiconductor layer.
[0134] Wherein, the first semiconductor layer is an N-type GaN layer.
[0135] An N-type GaN layer is grown on the surface of the substrate using MOCVD equipment.
[0136] In the disclosed embodiment, the growth of the semiconductor layer can be achieved by using VeecoK465i or C4 or RB metal organic chemical vapor deposition (MOCVD) equipment or AIXTRON metal organic chemical vapor deposition equipment. High purity H2 (hydrogen) or high purity N2 (nitrogen) or a mixture of high purity H2 and high purity N2 is used as a carrier gas, high purity NH3 is used as an N source, trimethyl gallium (TMGa) and triethyl gallium (TEGa) are used as gallium sources, trimethyl indium (TMIn) is used as an indium source, silane (SiH4) is used as an N-type dopant, trimethyl aluminum (TMAl) is used as an aluminum source, and bis(cyclopentadienyl) magnesium (CP2Mg) is used as a P-type dopant.
[0137] The second step is to grow the active layer.
[0138] Among them, the active layer is an InGaN / GaN layer.
[0139] Exemplarily, an MOCVD device is used to grow an InGaN / GaN layer on the surface of the N-type GaN layer.
[0140] The third step is to grow the second semiconductor layer.
[0141] Wherein, the second semiconductor layer is a P-type GaN layer.
[0142] Exemplarily, a P-type GaN layer is grown on the surface of the InGaN / GaN layer using MOCVD equipment.
[0143] In the fourth step, the first semiconductor layer, the active layer and the second semiconductor layer are patterned to form a step structure.
[0144] Exemplarily, an inductively coupled plasma (ICP) etching technique is used to pattern the first semiconductor layer, the active layer, and the second semiconductor layer stacked sequentially in the epitaxial structure to form a step structure.
[0145] S22, manufacturing a transparent conductive layer, wherein the transparent conductive layer is located on the surface of the second semiconductor layer.
[0146] In one example, step S22 includes:
[0147] A transparent conductive layer is formed on the surface of the second semiconductor layer by adopting magnetron sputtering technology and photolithography technology.
[0148] Wherein, the transparent conductive layer is an ITO layer.
[0149] S23, manufacturing a silver mirror structure, wherein the silver mirror structure is located on the surface of the second semiconductor layer and covers the transparent conductive layer.
[0150] In one example, step S23 includes:
[0151] A silver mirror structure is formed on the surface of the second semiconductor layer by using magnetron sputtering technology and photolithography technology.
[0152] The silver mirror structure includes a reflective layer and a barrier layer, and the barrier layer covers the surface and side surfaces of the reflective layer.
[0153] In the embodiment of the present disclosure, the reflective layer includes at least an Ag layer, and the barrier layer may include a combination of multiple layers of a Cr layer, an Al layer, a Ti layer, a Ni layer, a Pt layer, and an Au layer.
[0154] In the embodiment of the present disclosure, the reflective layer includes an Ag layer and a TiW layer stacked in sequence, and the barrier layer includes a Cr layer, an Al layer, a Ti layer, a Ni layer, a Pt layer and an Au layer stacked in sequence.
[0155] S24, manufacturing a first passivation layer, wherein the first passivation layer covers the step structure and the silver mirror structure.
[0156] In one example, the first passivation layer can be a SiO2 layer, a TiO2 layer, an Al2O3 layer, a SiN x Any one or more of the above insulating films, x is greater than 0.
[0157] S25, manufacturing a first electrode and a second electrode, wherein the first electrode penetrates the first passivation layer and is connected to the first semiconductor, and the second electrode penetrates the first passivation layer and is connected to the silver mirror structure.
[0158] In one example, step S25 includes:
[0159] The first electrode is manufactured in the first through hole by using electron beam evaporation technology and photolithography technology, and the second electrode is manufactured in the second through hole.
[0160] In the embodiment of the present disclosure, the first electrode and the second electrode include a Cr layer, an Al layer, a Ti layer, a Ni layer, a Pt layer, and an Au layer stacked in sequence.
[0161] S26. Fabricate a second passivation layer, wherein the second passivation layer covers the first passivation layer, the first electrode, and the second electrode, and the second passivation layer includes a plurality of alternately stacked dielectric layers and metal layers.
[0162] In one example, the second passivation layer can be a SiO2 layer, a TiO2 layer, an Al2O3 layer, a SiN x Any one or more of the above insulating films, x is greater than 0.
[0163] S27 . Make a first electrode pad and a second electrode pad, wherein the first electrode pad penetrates the second passivation layer and is connected to the first electrode, and the second electrode pad penetrates the second passivation layer and is connected to the second electrode.
[0164] In one example, step S27 includes:
[0165] A first electrode pad is manufactured in the third through hole, and a second electrode pad is manufactured in the fourth through hole by using photolithography technology and electron beam evaporation technology.
[0166] In the embodiment of the present disclosure, the first electrode pad and the second electrode pad each include a metal stack, a protective layer and an AuSn layer, and the AuSn layer is evaporated in two stages, and the thickness of the first stage is The second stage evaporation thickness is
[0167] In the embodiment of the present disclosure, the metal stack includes a first Ti layer, a first Al layer, a second Ti layer, and a second Al layer stacked in sequence, and the protective layer includes a third Ti layer and a Pt layer stacked in sequence.
[0168] In the disclosed embodiment, the Ti layer mainly plays an adhesion role; the Al layer plays a reflective and conductive role and has a lower cost; the Pt layer blocks AuSn from forming an alloy with Al; the AuSn layer has high conductivity, and the packaging does not require solder paste, reducing the packaging cost.
[0169] In the embodiment of the present disclosure, the thickness of the first Ti layer is The thickness of the first Al layer is The thickness of the second Ti layer is The thickness of the second Al layer is The thickness of the third Ti layer is The thickness of the Pt layer is The thickness of the first stage of the AuSn layer evaporation is The second stage evaporation thickness is
[0170] By using the above-mentioned thickness to make each metal layer, the electrical conductivity and light reflection properties of the pad can be ensured.
[0171] Exemplarily, the thickness of the first Ti layer is The thickness of the first Al layer is The thickness of the second Ti layer is The thickness of the second Al layer is The thickness of the third Ti layer is The thickness of the Pt layer is The thickness of the first AuSn layer is The thickness of the second AuSn layer is The thickness given in this example is the thickness in the middle of each metal layer. Figure 3 It can be seen that the thickness of the edges of each metal layer changes gradually, for example, gradually decreases from the middle to the edge.
[0172] In the embodiment of the present disclosure, the manufacturing of the first electrode pad and the second electrode pad includes:
[0173] sequentially depositing the first Ti layer, the first Al layer, the second Ti layer, and the second Al layer;
[0174] sequentially evaporating a first Ti layer, a first Al layer, a second Ti layer, and a second Al layer as a metal stack;
[0175] Sequentially evaporating a third Ti layer and a Pt layer stacked on the metal stack as a protective layer;
[0176] The AuSn layer was evaporated in two stages. The thickness of the first stage was The second stage evaporation thickness is
[0177] In this implementation, the metal stack and protective layer of the electrode pad are formed in the above-mentioned manner, wherein the Ti layer mainly plays an adhesion role; the Al layer plays a reflective and conductive role and has a low cost; the Pt layer blocks AuSn from forming an alloy with Al; the AuSn layer has high conductivity, and the packaging does not require solder paste, reducing the packaging cost.
[0178] The first Ti layer, the first Al layer, the second Ti layer and the second Al layer sequentially deposited and stacked as a metal stack may include:
[0179] Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The first Ti layer;
[0180] Using a crucible containing Al, electron beam evaporation was used to The evaporation rate, evaporation The first Al layer;
[0181] Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The second Ti layer;
[0182] Using a crucible containing Al, electron beam evaporation was used to The evaporation rate, evaporation The second Al layer.
[0183] In this implementation, each metal stack is manufactured with the above-mentioned evaporation rate and thickness, which can ensure the electrical conductivity and light reflection properties of the pad.
[0184] Wherein, a third Ti layer and a Pt layer are sequentially deposited on the metal stack as a protective layer, comprising:
[0185] Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The third Ti layer;
[0186] Using a crucible containing Pt, electron beam evaporation was used to The evaporation rate, evaporation of Pt layer.
[0187] In this implementation, each protective layer is manufactured using the above-mentioned evaporation rate and thickness, which can ensure the barrier effect of the protective layer and the adhesion effect with other film layers.
[0188] In one example, evaporating the AuSn layer in two stages may include:
[0189] Using the first crucible containing AuSn, electron beam evaporation was used to The first AuSn layer is evaporated at a deposition rate of
[0190] Using a second crucible containing AuSn, electron beam evaporation was performed to The second AuSn layer was evaporated at a deposition rate of .
[0191] In this implementation, the above evaporation rate is adopted and two crucibles are used to produce the AuSn layer. On the one hand, the two-stage evaporation of AuSn can be ensured, and on the other hand, the second stage evaporation can obtain a thinner AuSn layer, thereby ensuring the stable quality of the AuSn layer surface.
[0192] Exemplarily, the thickness of the first Ti layer is The thickness of the first Al layer is The thickness of the second Ti layer is The thickness of the second Al layer is The thickness of the third Ti layer is The thickness of the Pt layer is The thickness of the first AuSn layer is The thickness of the second AuSn layer is
[0193] Exemplarily, the evaporation rate of the first Ti layer is The evaporation rate of the first Al layer is The evaporation rate of the second Ti layer is The evaporation rate of the second Al layer is The evaporation rate of the third Ti layer is The thickness of the Pt layer is 1.5×10 evaporation rate. The evaporation rate of the first AuSn layer is The evaporation rate of the second AuSn layer is
[0194] In the embodiments of the present disclosure, a film structure of multiple light-emitting diodes is usually manufactured on the surface of a substrate, and then the substrate is thinned, laser-cut and split to form multiple light-emitting diodes.
[0195] The above description is only an optional embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure shall be included in the protection scope of the present disclosure.
Claims
1. A method for manufacturing an electrode pad, characterized in that: The method comprises: Sequentially evaporating a metal stack (201) and a protective layer (202); The AuSn layer (203) is deposited on the protective layer (202) in two stages. The thickness of the first stage is The second stage evaporation thickness is 2. The method according to claim 1, characterized in that: The AuSn layer (203) is evaporated on the protective layer (202) in two stages, comprising: Using the first crucible containing AuSn, electron beam evaporation was used to The first AuSn layer is evaporated at a deposition rate of Using a second crucible containing AuSn, electron beam evaporation was performed to The second AuSn layer was evaporated at a deposition rate of .
3. The production method according to claim 1 or 2, characterized in that: The sequentially evaporating and stacking metal layers (201) and protective layers (202) comprises: Sequentially evaporating and stacking a first Ti layer, a first Al layer, a second Ti layer, and a second Al layer as a metal stack (201); A third Ti layer and a Pt layer are sequentially deposited on the metal stack (201) as a protective layer (202).
4. The method according to claim 3, characterized in that The first Ti layer, the first Al layer, the second Ti layer and the second Al layer sequentially deposited and stacked as a metal stack (201) include: Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The first Ti layer; Using a crucible containing Al, electron beam evaporation was used to The evaporation rate, evaporation The first Al layer; Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The second Ti layer; Using a crucible containing Al, electron beam evaporation was used to The evaporation rate, evaporation The second Al layer.
5. The method according to claim 3, characterized in that: A third Ti layer and a Pt layer are sequentially deposited on the metal stack (201) as a protective layer (202), comprising: Using a crucible containing Ti, electron beam evaporation was used to The evaporation rate, evaporation The third Ti layer; Using a crucible containing Pt, electron beam evaporation was used to The evaporation rate, evaporation of Pt layer.
6. A light emitting diode, characterized in that: The light emitting diode comprises: A first semiconductor layer (101), an active layer (102) and a second semiconductor layer (103) stacked in sequence, wherein the first semiconductor layer (101), the active layer (102) and the second semiconductor layer (103) form a step structure; A silver mirror structure (105), wherein the silver mirror structure (105) is located on the surface of the second semiconductor layer (103); A first passivation layer (106), the first passivation layer (106) covering the step structure and the silver mirror structure (105); a first electrode (107) and a second electrode (108), wherein the first electrode (107) penetrates the first passivation layer (106) and is connected to the first semiconductor (101), and the second electrode (108) penetrates the first passivation layer (106) and is connected to the silver mirror structure (105); A second passivation layer (109), wherein the second passivation layer (109) covers the first passivation layer (106), the first electrode (107) and the second electrode (108); A first electrode pad (110) and a second electrode pad (111), wherein the first electrode pad (110) penetrates the second passivation layer (109) and is connected to the first electrode (107), and the second electrode pad (111) penetrates the second passivation layer (109) and is connected to the second electrode (108); The first electrode pad (110) and the second electrode pad (111) both comprise a metal stack (201), a protective layer (202) and an AuSn layer (203). The AuSn layer (203) is evaporated in two stages. The thickness of the first stage is The second stage evaporation thickness is 7. The light emitting diode according to claim 6, characterized in that: The metal stack (201) comprises a first Ti layer, a first Al layer, a second Ti layer and a second Al layer stacked in sequence, and the protective layer (202) comprises a third Ti layer and a Pt layer stacked in sequence.
8. The light emitting diode according to claim 7, characterized in that: The thickness of the first Ti layer is The thickness of the first Al layer is The thickness of the second Ti layer is The thickness of the second Al layer is The thickness of the third Ti layer is The thickness of the Pt layer is 9. A method for manufacturing a light emitting diode, characterized in that: The method comprises: Sequentially manufacturing a first semiconductor layer, an active layer, and a second semiconductor layer, wherein the first semiconductor layer, the active layer, and the second semiconductor layer form a step structure; Manufacturing a silver mirror structure, wherein the silver mirror structure is located on the surface of the second semiconductor layer; Manufacturing a first passivation layer, wherein the first passivation layer covers the step structure and the silver mirror structure; Manufacturing a first electrode and a second electrode, wherein the first electrode penetrates the first passivation layer and is connected to the first semiconductor, and the second electrode penetrates the first passivation layer and is connected to the silver mirror structure; Manufacturing a second passivation layer, wherein the second passivation layer covers the first passivation layer, the first electrode and the second electrode; A first electrode pad and a second electrode pad are manufactured, wherein the first electrode pad penetrates the second passivation layer and is connected to the first electrode, and the second electrode pad penetrates the second passivation layer and is connected to the second electrode; the first electrode pad and the second electrode pad are manufactured in the following manner: a metal stack and a protective layer are sequentially deposited; an AuSn layer is deposited on the protective layer in two stages, and the thickness of the first stage is The second stage evaporation thickness is 10. The method according to claim 9, characterized in that The AuSn layer is evaporated on the protective layer in two stages, comprising: Using the first crucible containing AuSn, electron beam evaporation was used to The first AuSn layer is evaporated at a deposition rate of Using a second crucible containing AuSn, electron beam evaporation was performed to The second AuSn layer was evaporated at a deposition rate of .