Preparation method of negative electrode material, negative electrode material prepared by preparation method and battery containing negative electrode material
By using one-step fluidized bed vapor phase coating and carbonization technology, the problems of poor uniformity and high cost of anode material coating modification have been solved, realizing efficient and low-cost anode material preparation and improving the electrochemical performance of the battery.
Patent Information
- Application Number
- CN202411166765.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-22
AI Technical Summary
Existing coating modification of anode materials suffers from problems such as poor uniformity, high cost, and difficult processing.
Using anthracene oil as a carbon source, a one-step gas-phase coating and carbonization process is carried out through a fluidized bed reactor to achieve uniform coating of the anode material.
It improves coating uniformity, reduces costs, simplifies the process, and the prepared anode material has high residual carbon content, excellent capacity, first efficiency, rate capability and low temperature performance, long cycle life, and is suitable for industrial production.
Smart Images

Figure CN119008832A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and specifically discloses a method for preparing a negative electrode material, the negative electrode material prepared thereby, and a battery comprising the negative electrode material. Background Art
[0002] Lithium-ion batteries are widely used in electronic devices, electric vehicles and energy storage systems due to their high energy density, long cycle life and low self-discharge rate. Graphite is currently the most widely used negative electrode material for lithium-ion batteries, with the advantages of high capacity, low cost, long cycle life and safety and non-toxicity. At present, graphite is mainly artificial graphite and natural graphite. Mid-to-high-end graphite is often coated and modified due to performance requirements such as long cycle, high rate and low temperature resistance. Coating modification refers to using graphite-like carbon materials as the "core" and coating the surface with modified materials to form a structure similar to "core-shell". The current market mainstream is to coat and modify graphite with amorphous carbon.
[0003] CN101209837A discloses a method for modifying graphite and the modified graphite obtained. Specifically disclosed is a method for modifying graphite and the modified graphite obtained, which mainly dissolves a high molecular polymer into a corresponding organic solvent with a boiling point not exceeding the softening point of the high molecular polymer, and then fully mixes it with graphite, stirs and heats the mixture, fully impregnates the graphite, and then distills and granulates and continues to heat the high molecular polymer to completely solidify to obtain a graphite composite material with a surface coated with the high molecular polymer, and then cools it to room temperature and performs conventional carbonization treatment. The disadvantage of this method is that it is costly.
[0004] CN112830482A discloses a graphite coating agent, a coated modified graphite material, a battery, and its preparation and application. Specifically discloses a graphite coating agent, a coated modified graphite material, a battery, and its preparation and application. The preparation method of the graphite coating agent comprises the following steps: under a protective atmosphere, the aromatic fraction is subjected to reduced pressure heat treatment, pressurized heat treatment, and crushing. The disadvantages of this method are that the raw material source is small, the cost is high, and the process is complicated.
[0005] At present, the graphite coating modification method for EV / PHEV / power tools and most 3C applications in the market is still asphalt solid phase coating, that is, solid asphalt powder is used as the carbon source, and solid phase coated graphite is obtained through mechanical mixing and high-temperature carbonization process. The advantages of this process are low cost, simple process, and high efficiency. The disadvantages are poor coating uniformity and insufficient coating, which have a great impact on product compaction and energy density. Some 3C products require high energy density and high power density, so there is still a need for a better preparation method for negative electrode materials. Summary of the invention
[0006] The inventors of the present invention used anthracene oil as a carbon source and utilized a fluidized bed to perform one-step gas-phase coating and carbonization of negative electrode materials, and on this basis completed the present invention.
[0007] One purpose of the present invention is to solve the problems of poor uniformity, high cost and great process difficulty in coating and modifying negative electrode materials in the current industry.
[0008] According to one aspect of the present invention, a method for preparing a negative electrode material is provided.
[0009] According to another aspect of the present invention, a negative electrode material prepared by the preparation method is provided.
[0010] According to another aspect of the present invention, a battery comprising the negative electrode material is provided.
[0011] According to one embodiment of the present invention, the preparation method comprises the following steps: S1, removing impurities from anthracene oil and preheating to 50-100°C, preferably 50-80°C; S2, adding the anthracene oil preheated in step S1 and high-purity nitrogen preheated to 50-100° C., preferably 50-80° C., into a gas-liquid mixer simultaneously or separately; S3, heating the nitrogen and anthracene oil added to the gas-liquid mixer in step S2 to 200-350° C.; preferably 200-300° C. to mix and gasify to serve as a carrier gas; S4, adding the carrier gas and negative electrode active material powder obtained in step S3 into a continuous fluidized bed reactor for reaction and carbonization to obtain a gas-phase carbon-coated modified negative electrode material.
[0012] According to one embodiment of the present invention, the anthracene oil in S1 is national standard anthracene oil, which complies with GB / T 2281 and has a content of ≥99%.
[0013] According to one embodiment of the present invention, the purity of the high-purity nitrogen in S2 is ≥99.9%.
[0014] According to one embodiment of the present invention, the mass ratio of nitrogen / anthracene oil in the gas-liquid mixer described in S3 is 1:(0.01-0.2), preferably 1:(0.05-0.15); the pressure in the gas-liquid mixer is 5-50MPa, preferably 10-30MPa; According to one embodiment of the present invention, the mass ratio of the carrier gas and the negative electrode active material powder described in S4 is (0.005-0.06):1, preferably (0.005-0.03):1; the carbonization temperature in the continuous fluidized bed reactor is 950-1300°C, preferably 950-1150°C; the flow rate of the carrier gas is 0.1-100L / min, preferably 5-30 L / min; the negative electrode active material powder is one or more of natural graphite, artificial graphite, silicon-based negative electrode, hard carbon, and soft carbon; the residual carbon content of the gas-phase carbon-coated modified negative electrode is 0.1%-3.5%.
[0015] The amount of residual carbon can be flexibly controlled by the mass ratio of the carrier gas to the negative electrode active material.
[0016] According to one embodiment of the present invention, a negative electrode material prepared by the preparation method is provided.
[0017] According to one embodiment of the present invention, a battery including the negative electrode material is provided.
[0018] According to one embodiment of the present invention, the battery includes a lithium battery and a supercapacitor.
[0019] Beneficial Effects The method of the present invention gasifies the carbon source and uses a fluidized bed to achieve coating and carbonization in one step, with higher coating uniformity, lower cost, fewer impurities, and simple process. The gas-phase carbon-coated modified negative electrode prepared by the present invention has the advantages of high residual carbon content, high capacity, high initial efficiency, excellent rate and low-temperature performance, long cycle life, good kinetic performance, etc., and has a wide range of raw material sources, low comprehensive cost, high purity, simple process, and is suitable for industrial production.
[0020] The negative electrode material of the present invention has more obvious improvement on defects, and the carbon coating layer can penetrate deep into the negative electrode material, thereby improving the co-embedding and interlayer destruction of the negative electrode material by the electrolyte to a greater extent, and further improving the cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a SEM picture of the finished product after the anthracene oil fluidized bed continuous one-step method of gas-phase coating of artificial graphite is used. DETAILED DESCRIPTION
[0022] In order to enable persons with ordinary knowledge in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and the scope of the patent application. Unless otherwise specified, all technical and scientific words used in the text have the common meanings understood by those skilled in the art for the present invention. In case of conflict, the definitions in this specification shall prevail.
[0023] As used herein, the terms "include", "comprising", "having", "containing" or any other similar terms are open-ended transitional phrases, which are intended to cover non-exclusive inclusions. For example, a composition or article containing multiple elements is not limited to the elements listed herein, but may also include other elements that are not explicitly listed but are generally inherent to the composition or article. In addition, unless otherwise expressly stated, the term "or" refers to an inclusive "or" rather than an exclusive "or". For example, any of the following situations satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and both A and B are true (or exist). In addition, as used herein, the terms "include", "comprising", "having", and "containing" should be interpreted as being specifically disclosed and simultaneously covering closed or semi-closed transitional phrases such as "consisting of" and "consisting essentially of".
[0024] In this article, all features or conditions defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be deemed to have covered and specifically disclosed all possible secondary ranges and individual values within the range, especially integer values. For example, the range description of "1 to 8" should be deemed to have specifically disclosed all secondary ranges such as 1 to 7, 2 to 8, 2 to 6, 3 to 6, 4 to 8, 3 to 8, etc., especially secondary ranges defined by all integer values, and should be deemed to have specifically disclosed individual values such as 1, 2, 3, 4, 5, 6, 7, 8, etc. within the range. Unless otherwise specified, the above interpretation method applies to all contents of the entire present invention, regardless of whether the range is broad or not.
[0025] If the quantity or other numerical value or parameter is expressed as a range, a preferred range or a series of upper and lower limits, it should be understood that all ranges consisting of any upper limit or preferred value of the range and the lower limit or preferred value of the range have been specifically disclosed herein, regardless of whether these ranges are disclosed separately. In addition, if a numerical range is mentioned herein, unless otherwise specified, the range should include its endpoints and all integers and fractions within the range.
[0026] In this document, under the premise of achieving the purpose of the invention, numerical values should be understood to have the accuracy of the number of significant digits of the numerical value. For example, the number 40.0 should be understood to cover the range from 39.50 to 40.49.
[0027] The following detailed description is merely illustrative in nature and is not intended to limit the present invention and its use. In addition, this document is not limited by any theory described in the above prior art or invention summary or the following detailed description or examples.
[0028] In the following examples, unless otherwise stated, all starting materials used were purchased from commercial sources.
[0029] Among them, anthracene oil was purchased from Xingtai Xuyang Coal Chemical Co., Ltd.; artificial graphite AG came from Xingtai Xuyang New Energy Technology Co., Ltd.
[0030] Example Example 1: Preparation of negative electrode material by one-step coating and carbonization using fluidized bed method 1. The purchased GB / T 2281 anthracene oil is sequentially dehydrated and impurized through a raw oil dehydration tank, a liquid crusher, and an oil residue separator to obtain anthracene oil raw material; 2. Preheat the anthracene oil raw material to 80° C. via a raw oil preheater and enter the gas-liquid mixer via a secondary filter; 3. High-purity nitrogen (purity 99.99%) enters the gas-liquid mixer after being preheated to 80°C; 4. Nitrogen and anthracene oil are heated to 300° C. in a gas-liquid mixer for mixed gasification, wherein the mass ratio of nitrogen to anthracene oil is 1:0.1; and the pressure in the gas-liquid mixer is 20 MPa.
[0031] 5. The above-mentioned gasified high-temperature anthracene oil and the negative electrode artificial graphite AG are added into a continuous fluidized bed reactor at a mass ratio of 0.03:1 for carbonization reaction. The carbonization temperature inside the reactor is 1150°C, and the flow rate of the high-temperature gasified anthracene oil is 10L / min. The gas phase carbon-coated modified artificial graphite AG-B is obtained through a graded discharging device.
[0032] The obtained gas phase carbon coated modified artificial graphite AG-B was observed by scanning electron microscope. Figure 1 shown.
[0033] According to the anthracene oil addition mass ratio and the fixed carbon content, the residual carbon content of the obtained gas phase carbon coated modified artificial graphite AG-B is 2%.
[0034] Example 2: Preparation of negative electrode material by one-step coating and carbonization using fluidized bed method 1. The purchased GB / T 2281 anthracene oil is sequentially dehydrated and impurized through a raw oil dehydration tank, a liquid crusher, and an oil residue separator to obtain anthracene oil raw material; 2. Preheat the anthracene oil raw material to 50° C. via a raw oil preheater and enter the gas-liquid mixer via a secondary filter; 3. High-purity nitrogen (purity 99.99%) enters the gas-liquid mixer after being preheated to 50°C; 4. Nitrogen and anthracene oil are heated to 200° C. in a gas-liquid mixer for mixed gasification, wherein the mass ratio of nitrogen to anthracene oil is 1:0.1; and the pressure in the gas-liquid mixer is 20 MPa.
[0035] 5. The above-mentioned gasified high-temperature anthracene oil and the negative electrode artificial graphite AG are added into a continuous fluidized bed reactor at a mass ratio of 0.03:1 for reaction and carbonization. The carbonization temperature inside the reactor is 1150°C, and the flow rate of the high-temperature gasified anthracene oil is 10L / min. The gas phase carbon-coated modified artificial graphite is obtained through a graded discharging device.
[0036] According to the calculation based on the mass ratio of anthracene oil addition and the fixed carbon content, the residual carbon content of the obtained gas phase carbon coated modified artificial graphite is 2%.
[0037] Example 3: Preparation of negative electrode material by one-step coating and carbonization using fluidized bed method 1. The purchased GB / T 2281 anthracene oil is sequentially dehydrated and impurized through a raw oil dehydration tank, a liquid crusher, and an oil residue separator to obtain anthracene oil raw material; 2. Preheat the anthracene oil raw material to 80° C. via a raw oil preheater and enter the gas-liquid mixer via a secondary filter; 3. High-purity nitrogen (purity 99.99%) enters the gas-liquid mixer after being preheated to 80°C; 4. Nitrogen and anthracene oil are heated to 300° C. in a gas-liquid mixer for mixed gasification, wherein the mass ratio of nitrogen to anthracene oil is 1:0.1; and the pressure in the gas-liquid mixer is 20 MPa.
[0038] 5. The above-mentioned gasified high-temperature anthracene oil and the negative electrode artificial graphite AG are added into a continuous fluidized bed reactor at a mass ratio of 0.005:1 for reaction and carbonization. The carbonization temperature inside the reactor is 1150°C, and the flow rate of the high-temperature gasified anthracene oil is 10L / min. The gas phase carbon-coated modified artificial graphite is obtained through a graded discharging device.
[0039] According to the calculation based on the mass ratio of anthracene oil addition and the fixed carbon content, the residual carbon content of the obtained gas phase carbon coated modified artificial graphite is 0.4%.
[0040] Example 4: Preparation of negative electrode material by one-step coating and carbonization using fluidized bed method 1. The purchased GB / T 2281 anthracene oil is sequentially dehydrated and impurized through a raw oil dehydration tank, a liquid crusher, and an oil residue separator to obtain anthracene oil raw material; 2. Preheat the anthracene oil raw material to 80° C. via a raw oil preheater and enter the gas-liquid mixer via a secondary filter; 3. High-purity nitrogen (purity 99.99%) enters the gas-liquid mixer after being preheated to 80°C; 4. Nitrogen and anthracene oil are heated to 300° C. in a gas-liquid mixer for mixed gasification, wherein the mass ratio of nitrogen to anthracene oil is 1:0.1; and the pressure in the gas-liquid mixer is 20 MPa.
[0041] 5. The above-mentioned gasified high-temperature anthracene oil and the negative electrode artificial graphite AG are added into a continuous fluidized bed reactor at a mass ratio of 0.03:1 for reaction and carbonization. The carbonization temperature inside the reactor is 950°C, and the flow rate of the high-temperature gasified anthracene oil is 10L / min. The gas phase carbon-coated modified artificial graphite AG-B is obtained through a graded discharging device.
[0042] According to the calculation based on the mass ratio of anthracene oil addition and the fixed carbon content, the residual carbon content of the obtained gas phase carbon coated modified artificial graphite is 2%.
[0043] Comparative Example 1: Comparative Example 1 uses original artificial graphite AG from Xingtai Xuyang New Energy Technology Co., Ltd. without modification or coating.
[0044] Comparative Example 2: Preparation of negative electrode material by one-step coating and carbonization using a fluidized bed method 1. The purchased GB / T 2281 anthracene oil is sequentially dehydrated and impurized through a raw oil dehydration tank, a liquid crusher, and an oil residue separator to obtain anthracene oil raw material; 2. Preheat the anthracene oil raw material to 80° C. via a raw oil preheater and enter the gas-liquid mixer via a secondary filter; 3. High-purity nitrogen (purity 99.99%) enters the gas-liquid mixer after being preheated to 80°C; 4. Nitrogen and anthracene oil are heated to 300° C. in a gas-liquid mixer for mixed gasification, wherein the mass ratio of nitrogen to anthracene oil is 1:0.1; and the pressure in the gas-liquid mixer is 20 MPa.
[0045] 5. The above-mentioned gasified high-temperature anthracene oil and the negative electrode artificial graphite AG are added into a continuous fluidized bed reactor at a mass ratio of 0.03:1 for carbonization reaction. The carbonization temperature inside the reactor is 800°C, and the flow rate of the high-temperature gasified anthracene oil is 10L / min. The gas phase carbon-coated modified artificial graphite AG-B is obtained through a graded discharging device.
[0046] According to the anthracene oil addition mass ratio and the fixed carbon content, the residual carbon content of the obtained gas phase carbon coated modified artificial graphite AG-B is 2%.
[0047] Comparative Example 3: Conventional solid-phase coating carbonization to prepare negative electrode materials The artificial graphite AG from Xingtai Xuyang New Energy Technology Co., Ltd. was stirred and mixed with the coated asphalt at 30 Hz for 30 minutes using a VC mixer, and then carbonized at 1150° C. for 6 hours to obtain the solid-phase coated modified graphite; The coated asphalt has a softening point of 250°C, a coking value of 69%, and a crushed particle size of 3-5 mm; The artificial graphite AG and the coated asphalt are added in a ratio of 1:0.03.
[0048] Experimental Example 1 The negative electrode materials obtained in the above-mentioned embodiments and comparative embodiments were mixed with a water-based binder (styrene-butadiene rubber SBR) and a conductive agent (carbon black SP) at a mass ratio of 90:7:3, applied to a copper foil, and then dried at 90°C to 110°C. After rolling and drying, the original sheet was formed as a negative electrode sheet. The coating density of the mixture of the negative electrode material, the water-based binder and the conductive agent was 10 mg / cm 2 , compacted density 1.3g / cm 3 Metal lithium sheet was selected as the counter electrode, the separator was a PE material with a thickness of 13μm and a porosity of about 48%, the electrolyte was ethylene carbonate (EC) + propylene carbonate (PC) = 1:1, 5% of the total mass of fluoroacetate (FEC) and 1.0 mol·L-1 LIF6 were added, and a button cell model CR2032 was assembled to obtain a lithium-ion battery. The gram capacity, first coulomb efficiency, cell rate and cycle performance of the negative electrode material were tested.
[0049] Among them, the detection steps of gram capacity and first coulomb efficiency are as follows: Standstill → 0.6mA constant current discharge to 5mv → Standstill → 0.2mA constant current discharge to 5mv → Standstill → 0.05mA constant current discharge to 5mv → Standstill → 0.6mA constant current charge to 2V.
[0050] Record the discharge capacity and charge capacity of this process, calculate the mass of the active material on the electrode, and thus calculate its charge-discharge specific capacity in mAh / g. The charge capacity divided by the discharge capacity gives the first charge-discharge efficiency. m active material = (m pole piece - m copper foil) × active material % Discharge capacity in grams = C discharge / m active material Charge capacity in grams = Ccharge / m active material First discharge efficiency = charging gram capacity / discharging gram capacity × 100%; The detection method of battery fast charging is as follows: Standstill → 0.1C constant current discharge to 5mv → Standstill → 0.05C constant current discharge to 5mv → Standstill → 0.1C constant current charge to 2v → Standstill → 0.1C constant current discharge to 5mv → Standstill → 4C constant current charge to 2v; Record the discharge capacity and charge capacity of this process; 4C retention rate = 4C CC charging capacity / 0.1C CC charging capacity * 100%.
[0051] The test method of cycle performance is as follows: Standstill → 0.1C constant current discharge to 5mv → Standstill → 0.05C constant current discharge to 5mv → Standstill → 0.5C constant current charge to 2v → Standstill → 0.5C constant current discharge to 5mv → Repeat 0.5C constant current charge & 0.5C constant current discharge; Record the discharge capacity and charge capacity of this process; 500-week cycle retention rate = 0.5C CC charge capacity at the 500th week / charge capacity at the 1st week.
[0052] Table 1 below lists various parameters of the batteries of various examples and comparative examples tested in Experimental Example 1.
[0053] Table 1
[0054] It can be seen from the results of the above embodiments and comparative embodiments that the negative electrode material prepared by the method of the present invention has the highest rate retention, and the material reversible capacity, first efficiency and cycle retention rate also maintain the best performance under the process conditions of the present invention.
[0055] It can be seen from the results of Comparative Example 2 that when the carbonization temperature is too low (800° C.), the first efficiency, capacity and rate performance of the material are poor.
[0056] Example 1 / Comparative Example 1 The results show that the negative electrode material prepared by the method of the present invention can significantly improve the rate performance.
[0057] The results of Example 1 / Comparative Example 3 show that the negative electrode material prepared by the method of the present invention can significantly improve the initial efficiency, capacity, cycle and rate performance of the material compared with the conventional solid phase coating modification process. Moreover, compared with the characteristics of the solid phase coating process, the efficiency and cost of the continuous production of the embodiment of the present invention are basically the same as those of the process of Comparative Example 3.
[0058] According to the test data of the negative electrode material prepared by the embodiment of the present invention and applied in the battery, the material prepared by the preparation method of the present invention has excellent electrochemical properties. Applying it in the battery can significantly improve the first coulombic efficiency and reversible capacity of the battery, and improve the rate and cycle performance of the battery cell.
Claims
1. A method for preparing a negative electrode material, the method comprising the following steps: S1, removing impurities from anthracene oil and preheating to 50-100°C, preferably 50-80°C; S2, adding the anthracene oil preheated in step S1 and high-purity nitrogen preheated to 50-100° C., preferably 50-80° C., into a gas-liquid mixer simultaneously or separately; S3, heating the nitrogen and anthracene oil added to the gas-liquid mixer in step S2 to 200-350° C.; preferably 200-300° C. to mix and gasify to serve as a carrier gas; S4, adding the carrier gas and negative electrode active material powder obtained in step S3 into a continuous fluidized bed reactor for reaction and carbonization to obtain a gas-phase carbon-coated modified negative electrode material.
2. The preparation method according to claim 1, wherein The anthracene oil described in S1 is national standard anthracene oil, which complies with GB / T 2281 and has a content of ≥99%.
3. The preparation method according to claim 1, wherein The purity of the high-purity nitrogen described in S2 is ≥99.9%.
4. The preparation method according to claim 1, wherein The mass ratio of nitrogen / anthracene oil in the gas-liquid mixer described in S3 is 1:(0.01-0.2), preferably 1:(0.05-0.15); the pressure in the gas-liquid mixer is 5-50 MPa, preferably 10-30 MPa.
5. The preparation method according to claim 1, wherein The mass ratio of the carrier gas and the negative electrode active material powder described in S4 is (0.005-0.06):1, preferably (0.005-0.03):1; the carbonization temperature in the continuous fluidized bed reactor is 950-1300°C, preferably 950-1150°C; the flow rate of the carrier gas is 0.1-100L / min, preferably 5-30 L / min; the negative electrode active material powder is one or more of natural graphite, artificial graphite, silicon-based negative electrode, hard carbon, and soft carbon; the residual carbon content of the gas-phase carbon-coated modified negative electrode is 0.1%-3.5%. 6 . A negative electrode material prepared by the preparation method according to claim 1 .
7. A battery comprising the negative electrode material according to claim 6. The battery according to claim 7 , which is a lithium battery or a supercapacitor.