Silicon-carbon composite material as well as preparation method and application thereof
By introducing a composite structure of mesoporous carbon, nano-silicon, metal, and fast ion conductor into silicon-carbon materials, the problems of low electronic conductivity and fast charging performance of silicon-carbon materials are solved, achieving efficient electron and ion transport and improving the charge-discharge performance and safety of lithium-ion batteries.
Patent Information
- Application Number
- CN202411031601.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing silicon-carbon materials have low electronic conductivity and fast-charging performance, resulting in high interface impedance, which affects the charging and discharging efficiency and stability of lithium-ion batteries.
Mesoporous carbon is used as the main material, doped with nano-silicon and metal, and the surface is covered with amorphous carbon and fast ion conductors. Silicon-carbon composite materials are formed through co-deposition and cyclic deposition to enhance electron and ion transport and reduce interfacial impedance.
It improves the electronic conductivity and lithium-ion migration rate of the material, enhances the structural stability and charge/discharge rate of the material, reduces the interface impedance, and improves the power performance and safety of lithium-ion batteries.
Smart Images

Figure CN119008879A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery material preparation, and in particular to a silicon-carbon composite material and a preparation method and application thereof. Background Art
[0002] As a silicon-based negative electrode material, silicon-carbon material is used in high energy density lithium-ion batteries due to its high specific capacity (1800-2200 mAh / g), high first efficiency (90%-92%), low expansion and good cycle performance.
[0003] Silicon-carbon material is composed of porous carbon and nanosilicon deposited in the pores thereof. However, due to the poor electronic conductivity of the porous carbon itself and the poor contact between the porous carbon and nanosilicon, the interface impedance is large, resulting in low electronic conductivity and fast charging performance of the silicon-carbon material.
[0004] In the prior art, attempts have been made to improve the power performance of silicon-carbon materials by means of doping, coating, etc., but the effect is not obvious. Summary of the invention
[0005] The main purpose of the present invention is to propose a silicon-carbon composite material and a preparation method and application thereof, aiming to solve the problems of low electronic conductivity and fast charging performance of silicon-carbon materials in the prior art.
[0006] To achieve the above object, the present invention provides a silicon-carbon composite material, characterized in that it includes a main body material, and a first shell layer and an outer shell sequentially covering the surface of the main body material;
[0007] Wherein, the main material comprises mesoporous carbon, and the mesoporous carbon is doped with heteroatoms, nano-silicon and metal;
[0008] The first shell layer includes amorphous carbon; and the outer shell includes a fast ion conductor.
[0009] In one embodiment, the heteroatom includes any one of a nitrogen atom and a sulfur atom; and / or,
[0010] The metal includes any one of magnesium, zinc and sodium; and / or,
[0011] The fast ion conductor includes LiAlSiO4, LiNbO3, Li7La3Zr2O 12 , Li 0.5 La 0.5 TiO3、Li 1.4 Al 0.4 Ti 1.6 Any of (PO4)3.
[0012] In one embodiment, in the silicon-carbon composite material, the mass ratio of silicon, carbon, metal, heteroatom, and fast ion conductor is (40-45): (40-45): (1-2.5): (1-2.5): (8-15).
[0013] The present invention also provides a method for preparing a silicon-carbon composite material, comprising the following steps:
[0014] S10, obtaining mesoporous carbon doped with heteroatoms, and transferring it to a fluidized bed, and introducing silane gas and metal gas for co-deposition under an inert atmosphere, so that nano-silicon and metal are deposited in the pores of the mesoporous carbon; and then introducing carbon source gas for carbon deposition to obtain a silicon-carbon precursor material;
[0015] S20, subjecting the silicon-carbon precursor material to fast ion conductor cyclic deposition to obtain the silicon-carbon composite material.
[0016] In one embodiment, in step S10, obtaining mesoporous carbon doped with heteroatoms comprises the following steps:
[0017] After the carbon source, the hard template agent and the heteroatom compound are dispersed in an organic solvent, a hydrothermal synthesis reaction is carried out, sintering is carried out, and washing is carried out to obtain the mesoporous carbon doped with the heteroatom.
[0018] In one embodiment, the mass ratio of the carbon source, the hard template, the heteroatom compound and the organic solvent is 100:(1-10):(1-5):(500-1500); and / or,
[0019] The carbon source comprises aliphatic polyurethane acrylate; and / or,
[0020] The hard template comprises at least one of silica microspheres, calcium carbonate microspheres, and zinc oxide microspheres, and the particle size of the hard template is 100 to 500 nm; and / or,
[0021] The heteroatom compound includes at least one of dopamine, pyrrole, thiophene, urea and melamine; and / or,
[0022] The organic solvent comprises at least one of xylene, acetone, ethyl acetate and benzene; and / or,
[0023] The temperature of the hydrothermal synthesis reaction is 100-200° C.; and / or,
[0024] The pressure of the hydrothermal synthesis reaction is 1-5 MPa; and / or,
[0025] The hydrothermal synthesis reaction time is 1 to 6 hours; and / or,
[0026] The sintering temperature is 600-1000° C.; and / or,
[0027] The sintering time is 1 to 6 hours; and / or,
[0028] The cleaning includes cleaning with hydrochloric acid, and the molar concentration of the hydrochloric acid is 1 to 5 mol / L.
[0029] In one embodiment, in step S10:
[0030] The silane gas includes at least one of tetrahydrosilane, trichlorosilane, dichlorosilane, monochlorosilane, disilane and dimethylsilane; and / or,
[0031] The metal gas includes metal gas generated by heating metal magnesium, metal zinc or metal sodium to 1000° C.; and / or,
[0032] The volume ratio of the silane gas to the metal gas is 10:(1-3); and / or,
[0033] The total gas flow rate of the co-deposition is 10 to 100 mL / min; and / or,
[0034] The co-deposition temperature is 500-800° C.; and / or,
[0035] The co-deposition time is 60 to 600 minutes; and / or,
[0036] The carbon source gas includes at least one of methane, ethane, ethylene, acetylene and propyne; and / or,
[0037] The gas flow rate of the carbon deposition is 100 to 500 mL / min; and / or,
[0038] The temperature of the carbon deposition is 800-1100° C.; and / or,
[0039] The carbon deposition time is 30 to 300 minutes.
[0040] In one embodiment, in step S30:
[0041] The temperature of the fast ion conductor cyclic deposition is 200-250° C.; and / or,
[0042] The number of cycles of the fast ion conductor cyclic deposition is 50 to 150 times; and / or,
[0043] Fast ion conductors include LiAlSiO4, LiNbO3, Li7La3Zr2O 12 , Li 0.5 La 0.5 TiO3、Li 1.4 Al 0.4 Ti 1.6Any of (PO4)3.
[0044] The present invention also provides an application, in which the aforementioned silicon-carbon composite material or the silicon-carbon composite material prepared by the aforementioned method for preparing the silicon-carbon composite material is used in a lithium-ion battery.
[0045] The present invention provides a silicon-carbon composite material and a preparation method and application thereof. The mesoporous carbon has a large pore volume and a high specific surface area, and its elastic structure buffers the volume expansion of nano-silicon during the charging and discharging process, while providing a good electron transmission path; the heteroatoms doped in the mesoporous carbon enhance the transmission efficiency of electrons in the material, thereby improving the electronic conductivity of the material; the deposited nano-silicon in the mesoporous carbon enhances the specific capacity of the material, the metal enhances the electronic conductivity of the material, and the direct contact between the metal and the nano-silicon enhances the electron and ion transmission at the interface on the one hand, helps to form a stable solid electrolyte interface film and reduce side reactions, and on the other hand reduces the probability of nano-silicon separating from the conductive network due to volume changes during the charging and discharging process, thereby reducing the interface impedance; in addition, the amorphous carbon in the first shell isolates the nano-silicon from the external environment, reduces gas production and improves safety; the fast ion conductor shell helps to accelerate the migration of lithium ions in the electrode material during the charging and discharging process, reduces the internal resistance of the material, and improves the charging and discharging rate and power performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0047] Figure 1 This is a scanning electron microscope image of the silicon-carbon composite material in Example 4 provided by the present invention.
[0048] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0049] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0050] As a silicon-based negative electrode material, silicon-carbon material is used in high energy density lithium-ion batteries due to its high specific capacity (1800-2200 mAh / g), high first efficiency (90%-92%), low expansion and good cycle performance.
[0051] Silicon-carbon materials are composed of porous carbon and nano-silicon deposited in the pores. When the contact between nano-silicon and the conductive carbon material is insufficient, the electron transmission path will be blocked, increasing the interface impedance. During the charge and discharge process, the volume of silicon will change, which may also cause the material to crack or separate from the conductive network, increasing the interface impedance. A large interface impedance will affect the thickness and stability of the solid electrolyte interface (SEI) film, limit the rapid insertion and extraction of lithium ions, and thus affect the fast charging performance.
[0052] In the prior art, attempts have been made to improve the power performance of silicon-carbon materials by means of doping, coating, etc., but the effect is not obvious.
[0053] In view of this, the present invention provides a silicon-carbon composite material, characterized in that it includes a main body material, and a first shell layer and an outer shell sequentially covering the surface of the main body material;
[0054] Wherein, the main material comprises mesoporous carbon, and the mesoporous carbon is doped with heteroatoms, nano-silicon and metal;
[0055] The first shell layer includes amorphous carbon; and the outer shell includes a fast ion conductor.
[0056] In the technical solution of the present invention, the mesoporous carbon has a large pore volume and a high specific surface area, and its elastic structure buffers the volume expansion of nano-silicon during the charging and discharging process, while providing a good electron transmission path; the heteroatoms doped in the mesoporous carbon form local defects, enhance the transmission efficiency of electrons in the material, thereby improving the electronic conductivity of the material; the nano-silicon deposited in the mesoporous carbon improves the specific capacity of the material, the metal improves the electronic conductivity of the material, and the direct contact between the metal and the nano-silicon on the one hand enhances the electron and ion transmission at the interface, helps to form a stable solid electrolyte interface film and reduce side reactions, and on the other hand reduces the probability of nano-silicon separating from the conductive network due to volume changes during the charging and discharging process, thereby reducing the interface impedance; in addition, the amorphous carbon in the first shell isolates the nano-silicon from the external environment, reduces gas production and improves safety; the fast ion conductor shell helps to accelerate the migration of lithium ions in the electrode material during the charging and discharging process, reduces the internal resistance of the material, and improves the charging and discharging rate and power performance of the material.
[0057] The pore volume of the mesoporous carbon is 0.8 to 1.1 cm 2 / g, specific surface area is 1000~1500m 2 / g.
[0058] In some embodiments of the present invention, the heteroatom includes any one of a nitrogen atom and a sulfur atom. The above heteroatoms can be selected to introduce point defects or line defects in the mesoporous carbon, which can serve as a source of additional electrons or holes, or act as a transmission channel for electrons / holes, thereby improving the conductivity of the material.
[0059] In some embodiments of the present invention, the metal includes any one of magnesium, zinc and sodium. The above metals are selected because they are low in cost and easy to obtain.
[0060] In some embodiments of the present invention, the fast ion conductor includes LiAlSiO4, LiNbO3, Li7La3Zr2O 12 , Li 0.5 La 0.5 TiO3、Li 1.4 Al 0.4 Ti 1.6 (PO4)3. The fast ion conductor has high lithium ion conductivity, which ensures the rapid transmission of lithium ions during the charging and discharging process, thereby improving the power density and response speed of the material.
[0061] In some embodiments of the present invention, in the silicon-carbon composite material, the mass ratio of silicon, carbon, metal, heteroatom, and fast ion conductor is (40-45): (40-45): (1-2.5): (1-2.5): (8-15). The mass ratio can be 40:40:2.5:2.5:15 or 45:45:1:1:8. The mass ratio within a suitable range can ensure that the material has a higher specific capacity and electronic / ionic conductivity, while maintaining better structural stability and cycle performance.
[0062] The present invention also provides a method for preparing a silicon-carbon composite material, comprising the following steps:
[0063] S10, obtaining mesoporous carbon doped with heteroatoms, and transferring it to a fluidized bed, and introducing silane gas and metal gas for co-deposition under an inert atmosphere, so that nano-silicon and metal are deposited in the pores of the mesoporous carbon; and then introducing carbon source gas for carbon deposition to obtain a silicon-carbon precursor material;
[0064] S20, subjecting the silicon-carbon precursor material to fast ion conductor cyclic deposition to obtain the silicon-carbon composite material.
[0065] In the technical solution of the present invention, the co-deposition of nano-silicon and metal increases the contact area between nano-silicon and metal, forming an effective electron transfer path, and the contact area means more active sites, which is conducive to forming a more stable SEI film and reducing the occurrence of side reactions; nano-silicon will undergo a large volume change during the charge and discharge process, and the mesoporous carbon near the nano-silicon can help alleviate the volume expansion of silicon, thereby improving the mechanical stability and cycle life of the final material, and the metal itself can store lithium ions, and synergizes with nano-silicon to improve the specific capacity and electronic conductivity of the material; carbon deposition is performed on the surface of the mesoporous carbon composite material, on the one hand Carbon deposition can construct a continuous electronic conductive network, promote the transmission of electrons in the electrode material, and improve the overall conductivity of the material. On the other hand, the carbon layer can also absorb and buffer the volume expansion and contraction of nano-silicon during the charging and discharging process, avoiding the breakage of silicon particles and falling off the electrode. In addition, the nano-silicon deposited in the mesoporous carbon is very active and will explode when encountering air or oxygen. Amorphous carbon is deposited on its surface for surface passivation, which is convenient for improving safety performance. The cyclic deposition of fast ion conductors can deposit fast ion conductors with higher density and better uniformity on the surface of the silicon-carbon precursor material, thereby improving the ionic conductivity and power performance of the material.
[0066] In the technical solution of the present invention, silane gas and metal gas are co-deposited, and carbon source gas is deposited, so that nano-silicon and metal are deposited in the mesoporous carbon to improve the electronic conductivity of the material, improve the interface impedance in the inner core mesopores, and deposit amorphous carbon on its surface, thereby reducing the specific surface area and the defects of the mesoporous carbon, thereby improving the first efficiency and its electronic conductivity.
[0067] In some embodiments of the present invention, in step S10, obtaining mesoporous carbon doped with heteroatoms comprises the following steps:
[0068] After the carbon source, the hard template agent and the heteroatom compound are dispersed in an organic solvent, a hydrothermal synthesis reaction is carried out, sintering is carried out, and washing is carried out to obtain the mesoporous carbon doped with the heteroatom.
[0069] In the technical solution of the present invention, under hydrothermal conditions, the carbon source undergoes polymerization and carbonization, the hard template guides the carbon source to form a mesoporous structure, and the heteroatom compound decomposes and is incorporated into the carbon skeleton. This step improves the electronic conductivity of the material and the pore volume of the carbon material, and helps to reduce the expansion of nanosilicon during charging and discharging; sintering is carried out in an inert atmosphere, the purpose of which is to remove residual hard templates, while stabilizing the material structure and improving the doping efficiency of heteroatoms; cleaning can further remove hard template residues and by-products.
[0070] In some embodiments of the present invention, the mass ratio of the carbon source, the hard template, the heteroatom compound and the organic solvent is 100:(1-10):(1-5):(500-1500). The mass ratio of the carbon source, the hard template, the heteroatom compound and the organic solvent can be 100:10:5:1500, 100:5:3:1000 or 100:1:1:500. The mass ratio can ensure the formation of the mesoporous structure and the high doping amount of heteroatoms within a suitable range while keeping the basic structure of the carbon material intact.
[0071] In some embodiments of the present invention, the carbon source includes aliphatic polyurethane acrylate. The aliphatic polyurethane acrylate is a polymer, and its molecule contains both the urethane bond of polyurethane and the carbon-carbon double bond of acrylate, so they can be cross-linked or cured by free radical polymerization. As a carbon source, aliphatic polyurethane acrylate has good mechanical properties and thermal stability, and can be cross-linked by free radical polymerization to form a more uniform pore structure.
[0072] In some embodiments of the present invention, the hard template includes at least one of silica microspheres, calcium carbonate microspheres, and zinc oxide microspheres, and the particle size of the hard template is 100 to 500 nm. That is, the hard template can be any one of silica microspheres, calcium carbonate microspheres, and zinc oxide microspheres, or two or more of silica microspheres, calcium carbonate microspheres, and zinc oxide microspheres, all within the scope of protection of the present invention. The particle size of the hard template can be 100 nm, 300 nm, or 500 nm, and its particle size can form pores with good mechanical stability within a suitable range.
[0073] In some embodiments of the present invention, the heteroatom compound includes at least one of dopamine, pyrrole, thiophene, urea, and melamine. That is, the heteroatom compound can be any one of dopamine, pyrrole, thiophene, urea, and melamine, or two or more of dopamine, pyrrole, thiophene, urea, and melamine, all within the protection scope of the present invention. The above heteroatom compounds can effectively incorporate nitrogen into carbon materials to improve the electronic conductivity of carbon materials.
[0074] In some embodiments of the present invention, the organic solvent includes at least one of xylene, acetone, ethyl acetate, and benzene. That is, the organic solvent can be any one of xylene, acetone, ethyl acetate, and benzene, or two or more of xylene, acetone, ethyl acetate, and benzene, all within the scope of the present invention. The above organic solvent has good dissolving power and stability, can ensure the efficient reaction, and is not prone to side reactions.
[0075] In some embodiments of the present invention, the temperature of the hydrothermal synthesis reaction is 100-200° C. The temperature of the hydrothermal synthesis reaction can be 100° C., 140° C. or 200° C., and the temperature within a suitable range can ensure the preparation of heteroatom-doped mesoporous carbon with high quality and purity.
[0076] In some embodiments of the present invention, the pressure of the hydrothermal synthesis reaction is 1-5 MPa. The pressure of the hydrothermal synthesis reaction can be 1 MPa, 3 MPa or 5 MPa. The pressure within a suitable range can ensure the preparation of heteroatom-doped mesoporous carbon with high quality and purity.
[0077] In some embodiments of the present invention, the hydrothermal synthesis reaction time is 1 to 6 hours. The hydrothermal synthesis reaction time can be 1 hour, 3 hours or 6 hours. The time within a suitable range can ensure the preparation of heteroatom-doped mesoporous carbon with high quality and purity, and is helpful to control the pore size in the mesoporous carbon, and has sufficient time to remove the hard template.
[0078] In some embodiments of the present invention, the sintering temperature is 600-1000° C. The sintering temperature can be 600° C., 800° C. or 1000° C. The temperature within a suitable range can ensure the promotion of carbonization, removal of residual hard templates, and enhancement of the density of the material, thereby leaving a more stable mesoporous structure.
[0079] In some embodiments of the present invention, the sintering time is 1 to 6 hours. The sintering time can be 1 hour, 3 hours or 6 hours. The time within a suitable range can ensure sufficient time to remove the hard template and enhance the mechanical strength and mesoporous stability of the material.
[0080] In some embodiments of the present invention, the cleaning includes cleaning with hydrochloric acid, and the molar concentration of the hydrochloric acid is 1 to 5 mol / L. The molar concentration of the hydrochloric acid can be 1 mol / L, 3 mol / L or 5 mol / L, and its molar concentration within a suitable range can ensure effective dissolution of the hard template, thereby releasing the mesoporous structure.
[0081] In some embodiments of the present invention, the silane gas includes at least one of tetrahydrosilane, trichlorosilane, dichlorosilane, monochlorosilane, disilane, and dimethylsilane. After decomposition at high temperature, the above silane gas can efficiently deposit nano-silicon in the pores of the heteroatom-doped mesoporous carbon.
[0082] In some embodiments of the present invention, the metal gas includes metal gas generated by heating metal magnesium, metal zinc or metal sodium to 1000° C. The metal gas is metal vapor, which is composed of metal atoms or small atomic clusters. The above metal gas has low decomposition temperature, low energy consumption and low cost.
[0083] In some embodiments of the present invention, the volume ratio of the silane gas to the metal gas is 10:(1-3). The volume ratio of the silane gas to the metal gas can be 10:3, 10:2 or 10:1. The volume ratio within a suitable range can improve the electronic conductivity of the mesoporous carbon and deposit nano-silicon in the pores, thereby improving the specific capacity.
[0084] In some embodiments of the present invention, the total gas flow rate of the co-deposition is 10-100 mL / min. The total gas flow rate of the co-deposition can be 10 mL / min, 60 mL / min or 100 mL / min. The total gas flow rate within a suitable range can ensure a high deposition efficiency and a more uniform deposition layer.
[0085] In some embodiments of the present invention, the co-deposition temperature is 500-800° C. The co-deposition temperature may be 500° C., 700° C. or 800° C. When the temperature is within a suitable range, the deposition efficiency can be improved while ensuring the decomposition of the material.
[0086] In some embodiments of the present invention, the co-deposition time is 60 to 600 minutes. The co-deposition time can be 60 minutes, 400 minutes or 600 minutes. The co-deposition time can ensure that the deposition layer is relatively uniform within a suitable range.
[0087] In some embodiments of the present invention, the carbon source gas includes at least one of methane, ethane, ethylene, acetylene, and propyne. That is, the carbon source gas can be any one of methane, ethane, ethylene, acetylene, and propyne, or two or more of methane, ethane, ethylene, acetylene, and propyne, all within the scope of the present invention. The above carbon source gas can efficiently decompose and deposit a carbon layer.
[0088] In some embodiments of the present invention, the gas flow rate of the carbon deposition is 100-500 mL / min. The gas flow rate of the carbon deposition can be 100 mL / min, 300 mL / min or 500 mL / min. The gas flow rate within a suitable range can ensure a high efficiency of depositing the carbon layer.
[0089] In some embodiments of the present invention, the temperature of the carbon deposition is 800-1100° C. The temperature of the carbon deposition can be 800° C., 950° C. or 1100° C. The temperature within a suitable range can ensure that the density of the deposited carbon layer is high while the carbon source is decomposed.
[0090] In some embodiments of the present invention, the carbon deposition time is 30 to 300 minutes. The carbon deposition time can be 30 minutes, 250 minutes or 300 minutes. The time within a suitable range can ensure that the thickness of the deposited carbon layer is more appropriate and the carbon layer is more uniform.
[0091] In some embodiments of the present invention, in step S30: the temperature of the fast ion conductor cyclic deposition is 200-250° C. The temperature of the fast ion conductor cyclic deposition can be 200° C., 220° C. or 250° C. The temperature within a suitable range can ensure that the uniformity, density and crystallinity of the fast ion conductor shell are good, and the interface bonding between the fast ion conductor and the substrate is good, thereby reducing the interface impedance.
[0092] In some embodiments of the present invention, in step S30: the number of cycles of the fast ion conductor cyclic deposition is 50 to 150. The number of cycles of the fast ion conductor cyclic deposition can be 50, 100 or 150. The number of cycles within a suitable range can ensure good uniformity and compactness of the shell, help form a stable and continuous SEI interface, and balance the ionic conductivity of the material and the activity of nano-silicon.
[0093] In some embodiments of the present invention, in step S30: the fast ion conductor includes LiAlSiO4, LiNbO3, Li7La3Zr2O 12 , Li 0.5 La 0.5 TiO3、Li 1.4 Al 0.4 Ti1.6 (PO4)3. The selection of the above fast ion conductors can ensure that the migration speed of lithium ions is fast, which is helpful to form a more stable SEI film, thereby improving the power density and charging speed of the battery.
[0094] The present invention also provides an application, using the aforementioned silicon-carbon composite material or the silicon-carbon composite material prepared by the aforementioned method for preparing the silicon-carbon composite material in a lithium-ion battery. The silicon-carbon composite material has all the above-mentioned beneficial effects, which will not be described one by one here.
[0095] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0096] Example 1
[0097] A silicon-carbon composite material comprises a main material and a shell, wherein the main material comprises mesoporous carbon, heteroatoms doped in the mesoporous carbon, nano-silicon, and metallic lithium; and a first shell layer and a shell layer sequentially covering the surface of the main material; the first shell layer comprises amorphous carbon; and the shell comprises a fast ion conductor.
[0098] The mass ratio of silicon, carbon, metallic lithium, heteroatoms and fast ion conductors in the silicon-carbon composite material is 43:43:2:2:10.
[0099] Example 2
[0100] Example 2 is similar to Example 1, except that:
[0101] The mass ratio of silicon, carbon, metallic lithium, heteroatoms and fast ion conductors in the silicon-carbon composite material is 45:40:1:1:8.
[0102] Example 3
[0103] Example 3 is similar to Example 1, except that:
[0104] The mass ratio of silicon, carbon, metallic lithium, heteroatoms and fast ion conductors in the silicon-carbon composite material is 40:45:2.5:2.5:15.
[0105] Example 4
[0106] A method for preparing a silicon-carbon composite material comprises the following steps:
[0107] S10, adding 100g of aliphatic polyurethane acrylate to 1000g of xylene organic solvent and dispersing evenly, then adding 5g of silica microspheres (particle size of 500nm) and 3g of dopamine, ultrasonically dispersing evenly, then transferring to a high-pressure reactor, reacting at a temperature of 150°C and a pressure of 3MPa for 3h, filtering, sintering the obtained filter residue at a temperature of 800°C for 3h, and then washing 3 times with 3mol / L hydrochloric acid to obtain heteroatom-doped mesoporous carbon;
[0108] The heteroatom-doped mesoporous carbon was transferred to a fluidized bed, and argon inert gas was first introduced to exhaust the air in the tube, and the temperature was heated to 650°C. Then, tetrahydrosilane gas and metal magnesium gas (the volume ratio of tetrahydrosilane gas to metal magnesium gas was 10:2) were introduced at the same time, and the gas flow rate was 50 mL / min for 300 min. Then, the temperature was raised to 950°C, and ethylene gas was introduced at a gas flow rate of 300 mL / min for 150 min. Then, the temperature was lowered to room temperature in an argon inert atmosphere to obtain a silicon-carbon precursor material.
[0109] S20. Place the silicon-carbon precursor material powder in a reaction chamber, evacuate the chamber to 0.1 torr, heat the temperature to 220°C, and deposit LiAlSiO4 according to the following procedure: (1) introduce LiAlSiO4 for 0.3 seconds; (2) purge with nitrogen for 60 seconds; (3) introduce an oxygen source for 5 seconds; (4) purge with nitrogen for 5 seconds; (5) introduce water for 0.03 seconds; (6) purge with nitrogen for 50 seconds; (7) repeat the process of step (1) for 100 cycles to form a LiAlSiO4 deposition layer of uniform thickness on the surface of the silicon-carbon precursor material layer by layer. After the cyclic deposition is completed, cool to room temperature to obtain a silicon-carbon composite material.
[0110] Example 5
[0111] A method for preparing a silicon-carbon composite material comprises the following steps:
[0112] S10, adding 100g of aliphatic polyurethane acrylate to 500g of acetone organic solvent and dispersing evenly, then adding 1g of calcium carbonate microspheres (particle size of 500nm) and 1g of pyrrole, ultrasonically dispersing evenly, then transferring to a high-pressure reactor, reacting at a temperature of 100°C and a pressure of 5MPa for 6h, filtering, sintering the obtained filter residue at a temperature of 600°C for 6h, and then washing 3 times with 1mol / L hydrochloric acid to obtain heteroatom-doped mesoporous carbon;
[0113] The heteroatom-doped mesoporous carbon was transferred to a fluidized bed, and argon inert gas was first introduced to exhaust the air in the tube, and the temperature was heated to 500°C. Then, trichlorosilane gas and metal zinc gas (the volume ratio of trichlorosilane gas to metal zinc gas was 10:1) were introduced at the same time, and the introduction time was 600 minutes at a flow rate of 10 mL / min. Then, the temperature was raised to 800°C, and acetylene gas was introduced at a gas flow rate of 100 mL / min for 300 minutes. Then, the temperature was lowered to room temperature in an argon inert atmosphere to obtain a silicon-carbon precursor material.
[0114] S20. Place the powder of the silicon-carbon precursor material in a reaction chamber, evacuate the chamber to 0.1 torr, raise the temperature to 200°C, and deposit LiNbO3 according to the following procedure: (1) introduce LiNbO3 for 0.3 seconds; (2) purge with nitrogen for 60 seconds; (3) introduce an oxygen source for 5 seconds; (4) purge with nitrogen for 5 seconds; (5) introduce water for 0.03 seconds; (6) purge with nitrogen for 50 seconds; (7) repeat the process from step (1) for 50 cycles to form a LiNbO3 deposition layer of uniform thickness on the surface of the silicon-carbon precursor material layer by layer. After the cyclic deposition is completed, cool to room temperature to obtain a silicon-carbon composite material.
[0115] Example 6
[0116] A method for preparing a silicon-carbon composite material comprises the following steps:
[0117] S10, adding 100g of aliphatic polyurethane acrylate to 1500g of ethyl acetate organic solvent and dispersing evenly, then adding 10g of zinc oxide microspheres (particle size of 500nm) and 5g of urea, ultrasonically dispersing evenly, then transferring to a high-pressure reactor, reacting at a temperature of 200°C and a pressure of 1MPa for 1h, filtering, sintering the obtained filter residue at a temperature of 1000°C for 1h, and then washing 3 times with 5mol / L hydrochloric acid to obtain heteroatom-doped mesoporous carbon;
[0118] The heteroatom-doped mesoporous carbon was transferred to a fluidized bed, and argon inert gas was first introduced to exhaust the air in the tube, and the temperature was heated to 800°C. Then, dichlorosilane gas and metallic sodium gas (the volume ratio of dichlorosilane gas to metallic sodium gas was 10:3) were introduced at the same time, and the introduction time was 60 minutes at a gas flow rate of 100 mL / min. Then, the temperature was raised to 1100°C, and methane gas was introduced at a gas flow rate of 500 mL / min for 30 minutes. Then, the temperature was lowered to room temperature in an argon inert atmosphere to obtain a silicon-carbon precursor material.
[0119] S20, placing the silicon-carbon precursor material powder in a reaction chamber, evacuating the chamber to 0.1 torr, raising the temperature to 250° C., and adding Li7La3Zr2O 12 The deposition was carried out according to the following procedure: (1) Li7La3Zr2O12 0.3 seconds; (2) nitrogen purge for 60 seconds; (3) oxygen source for 5 seconds; (4) nitrogen purge for 5 seconds; (5) water for 0.03 seconds; (6) nitrogen purge for 50 seconds; (7) starting from step (1), the cycle is repeated for 150 times to form a uniform thickness of Li7La3Zr2O on the surface of the silicon-carbon precursor material layer by layer. 12 The deposition layer is cooled to room temperature after the cyclic deposition is completed to obtain a silicon-carbon composite material.
[0120] Comparative Example 1
[0121] Compared with Example 1, Comparative Example 1 is the same as Example 1 except that step S20 is not performed.
[0122] Comparative Example 2
[0123] Compared with Example 1, Comparative Example 2 is the same as Example 1 except that the metal magnesium gas is not introduced in step S10.
[0124] Performance Testing
[0125] The silicon-carbon composite material prepared in Example 4 was observed using a scanning electron microscope.
[0126] Depend on Figure 1 It can be seen that the silicon-carbon composite material presents a granular structure with a small amount of precipitated material on the surface. The particle size is between 5 and 10 μm and the size distribution is uniform.
[0127] Physical and chemical properties test:
[0128] According to the method in the national standard GB / T 38823-2020 "Silicon Carbon", the specific surface area and tap density of the silicon-carbon composite materials obtained in Examples 4 to 6 and Comparative Examples 1 to 2 were tested, and the resistivity of the silicon-carbon composite materials was tested using a powder resistance tester; and the gas production of the powder material was tested (45°C, 48h), and the results are shown in Table 1 below.
[0129] Table 1 Physical and chemical properties of silicon-carbon composite materials in Examples 4 to 6 and Comparative Examples 1 to 2
[0130]
[0131] It can be seen from Table 1 that the specific surface area and tap density of the silicon-carbon composite materials in Examples 4 to 6 are higher than those in Comparative Examples 1 to 2, while the resistivity and gas production are lower than those in Comparative Examples 1 to 2, which indicates that the silicon-carbon composite materials prepared by the present invention have a high specific surface area, high tap density, low resistivity and low gas production.
[0132] Button cell battery test:
[0133] The silicon-carbon composite materials obtained in Examples 4 to 6 and Comparative Examples 1 to 2 were used as active materials for the negative electrode plates of the battery and were respectively prepared and assembled into five button batteries; wherein the specific preparation process of each button battery is as follows:
[0134] Preparation of negative electrode sheets for batteries: Add a binder, a conductive agent and a solvent to the silicon-carbon composite materials (as active materials of negative electrode sheets for batteries) corresponding to Examples 4 to 6 and Comparative Examples 1 to 2, stir to make pulp, apply on copper foil, dry and roll to obtain negative electrode sheets for batteries; wherein the binder is LA132 binder, the conductive agent is SP (conductive carbon black), and the solvent is NMP, and the ratio is: silicon-carbon composite material: SP: LA132: NMP = 95g: 1g: 4g: 220mL; Preparation of button batteries: electrolyte A LiPF6 solution was used, wherein the concentration of LiPF6 was 1 mol / L, and the solvent used was a mixed solution of ethylene carbonate and diethyl carbonate in a weight ratio of 1:1; a metal lithium sheet was used as the counter electrode, and a polypropylene (PP) film was used as the diaphragm. The simulated battery assembly was carried out in an argon-filled glove box, and the electrochemical performance was carried out on a Wuhan Blue Electric CT2001A battery tester. The test conditions were: the charge and discharge voltage range was 0.005V to 2.0V, and the charge and discharge rate was 0.1C; and its rate performance (1C / 0.1C) was tested. A full-charge expansion test was also carried out: the thickness D1 of the negative electrode sheet of the button battery after rolling was tested, and then the negative electrode sheet of the button battery was dissected when it was fully charged to 100% SOC, and the thickness D2 of the negative electrode sheet was tested, and then the full-charge expansion rate was calculated = (D2-D1) / D1*100%. The results are shown in Table 2 below.
[0135] Table 2 Performance characteristics of button batteries corresponding to Examples 4 to 6 and Comparative Examples 1 to 2
[0136]
[0137] It can be seen from Table 2 above that the button cells made using the silicon-carbon composite materials provided in Examples 4 to 6 of the present application are significantly better than those in Comparative Examples 1 to 2 in terms of first discharge specific capacity and first efficiency. The reason may be that the material of the present application uses magnesium doping to form magnesium silicate to improve the structural stability of the material and reduce its irreversible capacity, and coats its surface with a lithium fast ion conductor to improve the ionic conductivity of the material, reduce defects, and improve rate performance and first efficiency.
[0138] Soft pack battery test:
[0139] The silicon-carbon composite materials obtained in Examples 4 to 6 and Comparative Examples 1 to 2 were doped with 90% artificial graphite as negative electrode materials (i.e., negative electrode plates), and the ternary material LiNi 1 / 3 Co 1 / 3 Mn1 / 3 O2 is used as the positive electrode material, the electrolyte and the separator are assembled into a 5Ah soft pack battery; the separator of the soft pack battery is Celegard2400, the electrolyte is LiPF6 solution, the solvent of the LiPF6 solution is a mixed solution of EC and DEC with a volume ratio of 1:1, and the concentration of LiPF6 is 1.3mol / L. The following performance tests were carried out on each soft pack battery:
[0140] Liquid absorption capacity test: Use a 1mL burette and absorb 1mL of electrolyte, add a drop of electrolyte on the surface of the negative electrode, and time until the electrolyte is completely absorbed. Record the time t. The results are shown in Table 3 below;
[0141] Electrode surface resistance test: Use the electrode surface resistance tester to test the electrode (100cm 2 ) was placed on a test bench and its resistance was tested under a pressure of 500 kg. The results are shown in Table 3 below;
[0142] Rate and cycle performance: Cycle performance test and rate test were carried out on each soft pack battery; the test conditions of the cycle performance test were: charge and discharge voltage range was 2.5-4.2V, temperature was 25±3.0℃, charge and discharge rate was 1.0C / 1.0C, and the number of cycles was 500 times; the test conditions of the rate test were: test the charge constant current ratio at different charge rates (0.5C, 1C, 2C and 3C), and the test results are shown in Table 4 below.
[0143] Table 3 Liquid absorption speed and electrode sheet surface resistance of the soft battery corresponding to Examples 4 to 6 and Comparative Examples 1 to 2
[0144] Liquid suction speed (S) Electrode sheet surface resistance (Ω·cm) Example 4 87 11.23 Example 5 98 13.23 Example 6 75 9.25 Comparative Example 1 132 17.34 Comparative Example 2 113 14.25
[0145] It can be seen from Table 3 above that the liquid absorption and electrode sheet surface resistance of the silicon-carbon composite materials provided in Examples 4 to 6 of the present application are significantly better than those in Comparative Examples 1 to 3. The reason is that the materials of Examples 4 to 6 have a high specific surface area that improves the liquid absorption capacity of the material and a low powder resistivity that reduces the electrode sheet surface resistance.
[0146] Table 4 Rate and cycle performance of button cells corresponding to Examples 4 to 6 and Comparative Examples 1 to 2
[0147]
[0148] It can be seen from Table 4 above that the rate performance and cycle performance of the soft-pack lithium-ion batteries prepared using the silicon-carbon composite materials of Examples 4 to 6 of the present application are better than those of Comparative Examples 1 to 2. The main reason may be that the silicon-carbon composite materials provided in the embodiments of the present application have high powder conductivity and low electrode sheet surface resistance, which improves the rate performance of the material, and its low expansion and high specific surface area improve the liquid retention performance and cycle performance of the material.
[0149] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A silicon-carbon composite material, It is characterized in that It comprises a main body material, and a first shell layer and an outer shell sequentially covering the surface of the main body material; Wherein, the main material comprises mesoporous carbon, and the mesoporous carbon is doped with heteroatoms, nano-silicon and metal; The first shell layer includes amorphous carbon; and the outer shell includes a fast ion conductor.
2. The silicon-carbon composite material according to claim 1, It is characterized in that The heteroatom includes any one of a nitrogen atom and a sulfur atom; and / or, The metal includes any one of magnesium, zinc and sodium; and / or, The fast ion conductor includes LiAlSiO 4 、LiNbO 3 , Li 7 La 3 Zr 2 O 12 , Li 0.5 La 0.5 TiO 3 , Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 Any of .
3. The silicon-carbon composite material according to claim 1, It is characterized in that In the silicon-carbon composite material, the mass ratio of silicon, carbon, metal, heteroatom and fast ion conductor is (40-45): (40-45): (1-2.5): (1-2.5): (8-15).
4. A method for preparing the silicon-carbon composite material according to any one of claims 1 to 3, It is characterized in that The following steps are involved: S10, obtaining mesoporous carbon doped with heteroatoms, and transferring it to a fluidized bed, and introducing silane gas and metal gas for co-deposition under an inert atmosphere, so that nano-silicon and metal are deposited in the pores of the mesoporous carbon; and then introducing carbon source gas for carbon deposition to obtain a silicon-carbon precursor material; S20, subjecting the silicon-carbon precursor material to fast ion conductor cyclic deposition to obtain the silicon-carbon composite material.
5. The method for preparing the silicon-carbon composite material according to claim 4, It is characterized in that In step S10, obtaining mesoporous carbon doped with heteroatoms comprises the following steps: After the carbon source, the hard template agent and the heteroatom compound are dispersed in an organic solvent, a hydrothermal synthesis reaction is carried out, sintering is carried out, and washing is carried out to obtain the mesoporous carbon doped with the heteroatom.
6. The method for preparing the silicon-carbon composite material according to claim 5, It is characterized in that The mass ratio of the carbon source, the hard template, the heteroatom compound and the organic solvent is 100:(1-10):(1-5):(500-1500); and / or, The carbon source comprises aliphatic polyurethane acrylate; and / or, The hard template comprises at least one of silica microspheres, calcium carbonate microspheres, and zinc oxide microspheres, and the particle size of the hard template is 100 to 500 nm; and / or, The heteroatom compound includes at least one of dopamine, pyrrole, thiophene, urea and melamine; and / or, The organic solvent comprises at least one of xylene, acetone, ethyl acetate and benzene; and / or, The temperature of the hydrothermal synthesis reaction is 100-200° C.; and / or, The pressure of the hydrothermal synthesis reaction is 1-5 MPa; and / or, The hydrothermal synthesis reaction time is 1 to 6 hours; and / or, The sintering temperature is 600-1000° C.; and / or, The sintering time is 1 to 6 hours; and / or, The cleaning includes cleaning with hydrochloric acid, and the molar concentration of the hydrochloric acid is 1 to 5 mol / L.
7. The method for preparing the silicon-carbon composite material according to claim 4, It is characterized in that In step S10: The silane gas includes at least one of tetrahydrosilane, trichlorosilane, dichlorosilane, monochlorosilane, disilane and dimethylsilane; and / or, The metal gas includes metal gas generated by heating metal magnesium, metal zinc or metal sodium to 1000° C.; and / or, The volume ratio of the silane gas to the metal gas is 10:(1-3); and / or, The total gas flow rate of the co-deposition is 10 to 100 mL / min; and / or, The co-deposition temperature is 500-800° C.; and / or, The co-deposition time is 60 to 600 minutes; and / or, The carbon source gas includes at least one of methane, ethane, ethylene, acetylene and propyne; and / or, The gas flow rate of the carbon deposition is 100 to 500 mL / min; and / or, The temperature of the carbon deposition is 800-1100° C.; and / or, The carbon deposition time is 30 to 300 minutes.
8. The method for preparing the silicon-carbon composite material according to claim 4, It is characterized in that In step S20: The temperature of the fast ion conductor cyclic deposition is 200-250° C.; and / or, The number of cycles of the fast ion conductor cyclic deposition is 50 to 150 times; and / or, Fast ion conductors include LiAlSiO 4 、LiNbO 3 , Li 7 La 3 Zr 2 O 12 , Li 0.5 La 0.5 TiO 3 , Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 Any of .
9. An application, It is characterized in that The silicon-carbon composite material as claimed in any one of claims 1 to 3 or the silicon-carbon composite material prepared by the method for preparing the silicon-carbon composite material as claimed in any one of claims 4 to 8 is used in a lithium-ion battery.
Citation Information
Patent Citations
Silicon negative electrode material with fluff structure and preparation method of silicon negative electrode material
CN111525121A
Metal-doped amorphous carbon coated silicon-carbon composite material, preparation method and application thereof
CN116137324A
Fluorine-nitrogen doped amorphous carbon coated silicon-carbon composite material and preparation method thereof
CN116314722A
Metal-doped silicon-carbon composite material as well as preparation method and application thereof
CN116779835A
Composite negative electrode material and preparation method and application thereof
CN117878283A