Positive plate and secondary battery
By setting a multifunctional coating between the current collector and active material layer of the lithium battery positive electrode sheet, the resistance and solid electrolyte content is regulated, the problem of degradation of battery cell performance caused by the safety coating is solved, and the low-temperature discharge and cycling performance is improved, ensuring that Battery safety and performance balance.
Patent Information
- Application Number
- CN202411111663.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The introduction of safety coatings for existing lithium batteries will lead to deterioration of the low-temperature discharge performance and cycling performance of the battery cell.
A multifunctional coating is provided between the current collector and active material layer of the positive electrode sheet. The multifunctional coating contains a solid electrolyte. By regulating the resistance, total thickness of the multifunctional coating and the resistance relationship of the positive electrode sheet (2≤R1*R2* d≤45) and the mass ratio and ionic conductivity of the solid electrolyte improve the low-temperature discharge performance and cycling performance of the battery.
The battery has been improved in low-temperature discharge performance and cycle performance, while taking into account the safety performance of the battery cell, ensuring that the acupuncture test pass rate is greater than 90%, the discharge capacity at -10℃ is not less than 79%, and after 800 weeks of cycle at 25℃, it is The capacity retention rate is not less than 89%.
Smart Images

Figure CN119008950A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, and in particular to a positive electrode sheet and a secondary battery. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, no memory effect, long cycle life, and environmental friendliness. They can adapt to various environments and are widely used in products such as 3C, electric vehicles, and power tools.
[0003] As competition in the lithium battery industry becomes increasingly fierce, customers have higher and higher requirements for lithium battery safety, and coating the positive electrode current collector with a safety coating is one of the common measures used to improve battery safety. Generally speaking, the safety coating contains a certain proportion of inorganic fillers, conductive agents and binders. The inorganic filler can be an inert substance such as alumina and boehmite, or an active substance such as lithium iron phosphate and lithium manganese iron phosphate that can provide a certain capacity and has good thermal stability.
[0004] The use of safety coatings can greatly improve the safety of batteries, but the introduction of safety coatings will also significantly increase the internal resistance of the battery cells, leading to deterioration of the low-temperature discharge performance and cycle performance of the battery cells. Summary of the invention
[0005] The main purpose of the present invention is to provide a positive electrode sheet and a secondary battery, aiming to solve the problem that the safety coating of the existing lithium battery will cause the low-temperature discharge performance and cycle performance of the battery cell to deteriorate.
[0006] To achieve the above object, the present invention provides a positive electrode sheet, the positive electrode sheet comprising:
[0007] current collector;
[0008] A multifunctional coating disposed on at least one side surface of the current collector;
[0009] A positive electrode active material layer disposed on a surface of the multifunctional coating layer away from the current collector;
[0010] The components of the multifunctional coating include a solid electrolyte, a first conductive agent and a first binder, and the resistance, total thickness of the multifunctional coating and the resistance of the positive electrode sheet satisfy the relationship: 2≤R 1 *R 2 *d≤45, where R 1 is the resistance of the multifunctional coating, R 2 is the resistance of the positive electrode sheet, and d is the total thickness of the multifunctional coating;
[0011] The mass ratio c of the solid electrolyte to the multifunctional coating is related to the ionic conductivity of the solid electrolyte at room temperature. Satisfies the relationship:
[0012] Preferably, the resistance, total thickness of the multifunctional coating and the resistance of the positive electrode sheet satisfy the relationship: 15≤R 1 *R 2 *d≤35.
[0013] Preferably, the mass ratio c of the solid electrolyte to the multifunctional coating is equal to the ionic conductivity of the solid electrolyte at room temperature. Satisfies the relationship:
[0014] Preferably, the total thickness d of the multifunctional coating is 1 μm to 20 μm; more preferably, the total thickness d of the multifunctional coating is 7.5 to 10.3 μm.
[0015] Preferably, when tested under a test pressure of 0.4t, the resistance R of the multifunctional coating is 1 It is 0.5Ω to 5Ω, and more preferably 1.2Ω to 1.9Ω.
[0016] Preferably, the mass ratio of the solid electrolyte, the first conductive agent and the first binder in the multifunctional coating is (1-95):(0.5-5):(0.5-10).
[0017] Preferably, the first conductive agent is selected from one or both of conductive carbon black and carbon nanotubes.
[0018] Preferably, the first binder is selected from at least one of polyvinylidene fluoride, styrene-butadiene rubber, sodium carboxymethyl cellulose and polyacrylate.
[0019] Preferably, the multifunctional coating further comprises at least one of a thermally stable active substance and an inert inorganic filler.
[0020] Preferably, the mass ratio of the solid electrolyte, the first conductive agent, the first binder, the thermally stable active substance, and the inert inorganic filler in the multifunctional coating is (1-95):(0.5-5):(0.5-10):(1-95):(1-95).
[0021] Preferably, the thermally stable active material is selected from one or both of lithium iron phosphate and lithium iron manganese phosphate; preferably, the inert inorganic filler is selected from one or both of alumina and boehmite.
[0022] Preferably, the double-sided coating density of the multifunctional coating is 2 mg / 1540.25 mm 2 ~35mg / 1540.25mm 2 .
[0023] Preferably, the solid electrolyte is selected from Li 1+x Al x M 2-x (PO 4 ) 3 , Li 7 La 3 N 2 O 12 , Li 3y La 2 / 3-y TiO 3 , Li 7- z La 3 Zr 2-z Ta z O 12 and Li 2+a-b ZrCl 6-a-b O a At least one of the following, wherein 0<x<0.5, M is selected from Ti and / or Ge, N is selected from at least one of Zr, Sn, and Ta, 0<y<0.16, 0<z<2, 0≤a≤2, and 0≤b≤0.75.
[0024] Preferably, the particle size D of the solid electrolyte is v50 It is 0.2μm~1.5μm.
[0025] The present invention further provides a secondary battery, comprising a positive electrode sheet, a negative electrode sheet and a separator between the positive electrode sheet and the negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet as described above.
[0026] The beneficial effect of the technical solution of the present invention is that: the present invention arranges a multifunctional coating between the current collector and the active material layer of the positive electrode sheet, the multifunctional coating contains a solid electrolyte, and regulates 2≤R 1 *R 2 *d≤45 and It effectively improves the low-temperature discharge performance and cycle performance of the battery, while taking into account the safety performance of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of the positive electrode structure of an embodiment of the present invention. DETAILED DESCRIPTION
[0028] The scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] It should be noted that all directional indications in the embodiments of the present invention (such as up, down, left, right, front, back, top, bottom, side...) are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0030] It should also be noted that when an element is referred to as being "fixed on" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element at the same time. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0031] In addition, the descriptions involving "first", "second", etc. in the embodiments of the present invention are only for descriptive purposes and cannot be understood as indicating or suggesting their relative importance or implicitly indicating the number of the indicated technical features.
[0032] The internal short circuit of lithium-ion batteries can generally be divided into several types: 1) short circuit between positive and negative current collectors; 2) between positive and negative active materials; 3) between negative active materials and positive current collectors; 4) between positive active materials and negative current collectors. Among them, the impedance of the short circuit point between the negative active material and the positive current collector is small, and the trigger temperature of the negative exothermic reaction is low. Therefore, the short circuit between the negative active material and the Al foil is the most dangerous. By introducing a safety coating to the surface of the positive current collector, the probability of contact between the positive current collector and the negative active material can be reduced, which can effectively improve the safety performance of the battery cell. However, the introduction of the safety coating in the prior art will also significantly increase the internal resistance of the battery cell, resulting in the deterioration of the low-temperature discharge performance and cycle performance of the battery cell.
[0033] Based on the defects in the prior art, an embodiment of the present invention provides a positive electrode sheet, referring to Figure 1 , the positive electrode sheet 10 comprises:
[0034] Current collector 11;
[0035] A multifunctional coating 12 disposed on at least one side of the current collector 11;
[0036] A positive electrode active material layer 13 disposed on a surface of the multifunctional coating layer 12 away from the current collector 11;
[0037] The components of the multifunctional coating 13 include a solid electrolyte, a first conductive agent and a first binder, and the resistance, total thickness and resistance of the multifunctional coating and the positive electrode sheet satisfy the relationship: 2≤R 1 *R 2 *d≤45, where R 1 is the resistance of the multifunctional coating 13, R2 is the resistance of the positive electrode sheet 10, and d is the total thickness of the multifunctional coating 13;
[0038] The mass ratio c of the solid electrolyte to the multifunctional coating is related to the ionic conductivity of the solid electrolyte at room temperature. Satisfies the relationship:
[0039] In this embodiment, a multifunctional coating is provided between the current collector and the active material layer of the positive electrode sheet. The multifunctional coating contains a solid electrolyte. By utilizing its good ionic conductivity at low temperatures, the low-temperature discharge performance and cycle performance of the battery can be improved. Generally speaking, the effect of a solid electrolyte is related to its content and ionic conductivity. If the content or ionic conductivity is too low, it will not have a good effect. It can ensure that the solid electrolyte can play a better role. In addition, R 1 , d and R 2 These three parameters are positively correlated with the safety of the battery cell, but negatively correlated with the cycle performance of the battery cell. 1 *R 2 * When d≤2, the safety performance of the battery is poor, R 1 *R 2 * When d≥45, the cycle performance of the battery cell is poor. The present application makes the above-mentioned limitation on the parameters of the multifunctional coating, which can take into account the safety performance and cycle performance of the battery cell without changing the original process, so as to achieve a better balance between the safety performance and cycle performance.
[0040] Furthermore, the normal temperature in this embodiment is 25°C. The larger the value, the better the low-temperature discharge performance of the battery. The larger the value, the smaller c is when the same effect is achieved. In this embodiment, taking into account the marginal diminishing effect of the amount of solid electrolyte and its expensive price, when the above relationship is met, using less solid electrolyte can greatly improve the low-temperature discharge performance of the battery cell. When the parameters in the multifunctional coating simultaneously satisfy the above two relationship equations, the battery cell puncture pass rate can be greater than 90%, the 3.4V discharge capacity at -10°C is not less than 79%, and the capacity retention rate after 800 cycles at 25°C is not less than 89%.
[0041] Preferably, the resistance, total thickness of the multifunctional coating and the resistance of the positive electrode sheet satisfy the relationship: 15≤R 1 *R 2 *d≤35. Within this range, the performance of the sample is even better, the pass rate of the needle puncture test can reach 100%, and the capacity retention rate after 800 cycles at room temperature is >90%.
[0042] Preferably, the mass ratio c of the solid electrolyte to the multifunctional coating is equal to the ionic conductivity of the solid electrolyte at room temperature. Satisfies the relationship: Within this range, the amount of solid electrolyte used is relatively small, and the improvement in low-temperature discharge performance is obvious, so the overall benefits are better.
[0043] The choice of raw materials will affect the resistance R of the multifunctional coating. 1 and the total thickness d, and the resistance R of the positive electrode 2 , which in turn affects whether the parameters of the multifunctional coating can satisfy the above relationship. Therefore, the present invention also needs to make further limitations on the raw materials and dosage of the multifunctional coating.
[0044] Based on this, in some embodiments, the total thickness d of the multifunctional coating is 1 μm to 20 μm; and / or, when tested under a test pressure of 0.4 t, the resistance R of the multifunctional coating is 1 0.5Ω~5Ω.
[0045] In this embodiment, the diaphragm resistance of the multifunctional coating is the primary factor affecting the safety performance of the battery cell. If the value is too small, the safety performance of the battery cell will deteriorate, while if it is too large, the cycle performance of the battery cell will deteriorate. The value is between 0.5Ω and 5Ω (the test pressure is 0.4t), which can take into account both safety performance and cycle performance, and is more preferably 1.2Ω to 1.9Ω.
[0046] In some embodiments, the mass ratio of the solid electrolyte, the first conductive agent, and the first binder in the multifunctional coating is (1-95):(0.5-5):(0.5-10); and / or the total thickness d of the multifunctional coating is 7.5-10.3 μm.
[0047] In this embodiment, the amount of the first conductive agent is 0.5% to 5% of the weight of the multifunctional coating, preferably 2% to 3.5%. If the content of the conductive agent is too low, the resistance of the multifunctional coating film will be too large, and the battery cell cycle performance will be poor. If the content is too high, the resistance of the multifunctional coating film will be too low, and the battery cell safety will be poor. When the content of the conductive agent is between 0.5% and 5%, both safety performance and cycle performance can be taken into account. The amount of the first binder is 0.5% to 10% of the weight of the multifunctional coating, preferably 4% to 6%. If the amount of the first binder is too low, the bonding force will be too low, and there is a risk of the coating falling off during use. If the amount of the first binder is too high, the bonding force can be improved, and the safety performance of the battery cell can be improved, but the cycle performance of the battery cell will also be poor.
[0048] In some embodiments, the first conductive agent is selected from one or both of conductive carbon black and carbon nanotubes; the first binder is selected from at least one of polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC) and polyacrylate (PAA).
[0049] In some embodiments, the multifunctional coating also includes at least one of a thermally stable active substance and an inert inorganic filler; and / or, the mass ratio of the solid electrolyte, the first conductive agent, the first binder, the thermally stable active substance, and the inert inorganic filler in the multifunctional coating is (1 to 95): (0.5 to 5): (0.5 to 10): (1 to 95): (1 to 95).
[0050] In this embodiment, the thermally stable active substance and the inert inorganic filler are non-essential components, but a certain amount of the thermally stable active substance and the inert inorganic filler can be added to the multifunctional coating in consideration of cost and processability.
[0051] In some embodiments, the thermally stable active material is selected from one or both of lithium iron phosphate and lithium iron manganese phosphate; and the inert inorganic filler is selected from one or both of alumina and boehmite.
[0052] In some embodiments, the double-sided coating density of the multifunctional coating is 2 mg / 1540.25 mm 2 ~35mg / 1540.25mm 2 .
[0053] In this embodiment, there is a positive correlation between the double-sided coating surface density of the multifunctional coating and its thickness. If the thickness is too low, the safety performance of the battery cell is poor, and if the thickness is too large, the energy density of the battery cell will be reduced.
[0054] In some embodiments, the solid electrolyte is selected from Li 1+x Al x M 2-x (PO 4 ) 3 , Li 7 La 3 N 2 O 12 , Li 3y La 2 / 3- y TiO 3 , Li 7-z La 3 Zr 2-z Ta z O 12 and Li 2+a-b ZrCl 6-a-b O aAt least one of the following, wherein 0<x<0.5, M is selected from Ti and / or Ge, N is selected from at least one of Zr, Sn, and Ta, 0<y<0.16, 0<z<2, 0≤a≤2, 0≤b≤0.75; and / or the particle size D of the solid electrolyte is v50 It is 0.2μm~1.5μm.
[0055] In this embodiment, the solid electrolyte selected has an ionic conductivity greater than 10 at room temperature. -5 S / cm, preferably, the solid electrolyte can be Li 1+x Al x Ti 2-x (PO 4 ) 3 (lithium aluminum titanium phosphate, LATP), Li 7 La 3 Zr 2 O 12 (lithium lanthanum zirconium oxide, LLZO) and Li 3x La 2 / 3-x TiO 3 (Lithium lanthanum titanate, 0<x<0.16, LLTO) neutralizes Li 2+a-b ZrCl 6-a-b O a (lithium zirconium oxychloride, LZCO, 0≤a≤2, 0≤b≤0.75) or more. The particle size D of the solid electrolyte v50 The particle size is between 0.2 and 1.5 μm. If the particles are too small, it will be difficult to disperse them in subsequent processing. If the particles are too large, the ion conduction path inside the electrolyte may become longer, thereby reducing the ion conduction efficiency. In addition, larger particles may not be able to form good contact with the electrode material, resulting in increased interface impedance and affecting the battery's charge and discharge performance. At the same time, larger particles may cause greater stress in the battery cell during the cycle process, thereby accelerating the aging of the material and reducing the battery's cycle life.
[0056] In some embodiments, the method for preparing the multifunctional coating comprises:
[0057] Mixing the raw material of the multifunctional coating with a solvent to obtain a multifunctional coating slurry;
[0058] The multifunctional coating slurry is transferred to at least one side surface of the current collector by gravure printing to obtain the multifunctional coating.
[0059] In this embodiment, the solvent can be N-methylpyrrolidone (NMP). Since the present application has strict requirements on the resistance and thickness of the multifunctional coating, the gravure printing method can achieve precise control of the multifunctional coating parameters. The temperature of the oven during gravure printing is 90°C to 110°C, and the printing speed is 10m / min to 50m / min. When the temperature of the oven is lower than 90°C, the production efficiency will be reduced, and when it is higher than 110°C, there may be problems such as cracking and migration of the conductive agent to the surface. If the printing speed is too low, the production efficiency will also be reduced. If it is too high, the multifunctional coating will be leaked, which will have a negative impact on the safety performance of the battery cell.
[0060] In some embodiments, the solid content of the multifunctional coating slurry is not less than 10%, and the viscosity is not less than 50 mPa·s. Too low a solid content will not only reduce the efficiency of production, but also make it difficult to obtain a multifunctional coating of a specified thickness and surface density, while too low a viscosity is not conducive to the gravure printing process. The multifunctional coating can firmly adhere to the surface of the current collector, which can not only reduce the surface contact resistance, but also reduce the generation of positive current collector burrs when the battery cell is safety tested, and reduce the contact short circuit between the positive current collector burrs and the unstable negative active material in the charging state, thereby improving the safety of the battery cell. At the same time, the solid electrolyte contained in the multifunctional coating can also conduct ions, reduce the interface impedance, and enable the battery cell to maintain good low-temperature discharge performance and cycle performance.
[0061] In this embodiment, the bonding force between the multifunctional coating 12 and the current collector 11 is not less than 100 N / m. When the bonding force is less than 100 N / m, the multifunctional coating has a risk of falling off during subsequent use. The current collector 11 can be one or both of aluminum foil and composite aluminum foil; the active material layer 13 includes a positive electrode active material, a second conductive agent, and a second binder.
[0062] In some embodiments, the positive electrode active material can be one or more of common lithium cobalt oxide, lithium iron phosphate and ternary materials, and its dosage is 90% to 98% of the total weight of the active material layer 13. Under the condition of ensuring that the active material has a certain conductivity and adhesion, the higher the content of the active material, the better, so that the battery cell has a higher energy density; the second conductive agent is a commonly used conductive agent, including one or two of conductive carbon black and carbon nanotubes. The dosage of the second conductive agent is 0.5% to 5% of the total weight of the active material layer 13, preferably 0.5% to 2%. If the content of the second conductive agent is too low, the resistance R of the positive electrode sheet will be increased. 2If it is too large, the cycle performance of the battery cell is not good. If it is too high, it is good for improving the cycle performance, but it will lead to poor safety performance of the battery cell. The second binder can be one or more of polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC), and polyacrylate (PAA), and the amount used is 0.5% to 5% of the total weight of the active material layer 13. The impact of the amount of the second binder is similar to that of the first binder, but considering that it does not directly contact the current collector, the upper limit of its amount can be appropriately reduced to ensure that the positive electrode active material does not fall off during the use of the battery cell. At the same time, a lower amount can also improve the cycle performance of the battery cell, increase the amount of positive electrode active material, and improve the energy density of the battery cell.
[0063] The present invention further provides a secondary battery, comprising a positive electrode sheet, a negative electrode sheet and a separator spaced between the positive electrode sheet and the negative electrode sheet, wherein the positive electrode sheet is the positive electrode sheet as described above.
[0064] In this embodiment, the positive electrode sheet includes the positive electrode current collector containing the multifunctional coating and a positive electrode active material layer coated on at least one surface of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, which is a positive electrode active material commonly used in lithium-ion batteries, including but not limited to a chemical formula such as Li x Ni h Co y M z O 2-d N d (wherein 0.95≤x≤1.2, h>0, y≥0, z≥0, and h+y+z=1, 0≤d≤1, M is selected from a combination of one or more of Mn and Al, and N is selected from a combination of one or more of F, P, and S) The positive electrode active material may also be, but is not limited to, LiCoO 2 、LiNiO 2 、LiVO 2 、LiCrO 2 、LiMn 2 O 4 、LiCoMnO 4 , Li 2 NiMn 3 O 8 、LiNi 0.5 Mn 1.5 O 4 、LiCoPO 4 、LiMnPO 4 、LiFePO 4 、LiNiPO 4 、LiCoFSO 4 , CuS 2 , FeS 2、MoS 2 、NiS、TiS 2 The positive electrode active material may also be subjected to a modification treatment. The method for modifying the positive electrode active material should be known to those skilled in the art. For example, the positive electrode active material may be modified by coating, doping, etc. The material used for the modification treatment may include but is not limited to a combination of one or more of Al, B, P, Zr, Si, Ti, Ge, Sn, Mg, Ce, W, etc.
[0065] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on at least one surface of the negative electrode current collector, and the negative electrode current collector is copper foil. The negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes a silicon-based material, which can be selected from one or more of elemental silicon, silicon oxide compounds, silicon carbon composites, and silicon alloys, or a mixture of silicon negative electrode materials and other commonly used negative electrode active materials. The other negative electrode active materials include but are not limited to one or more of graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, tin-based materials, lithium titanate, or other metals that can form alloys with lithium. Among them, the graphite can be selected from one or more of artificial graphite, natural graphite, and modified graphite; the tin-based material can be selected from one or more of elemental tin, tin oxide compounds, and tin alloys.
[0066] The separator can be any material suitable for lithium-ion battery separators in the art, for example, it can be a combination of one or more materials including but not limited to polyethylene, polypropylene, polyvinylidene fluoride, aramid, polyethylene terephthalate, polytetrafluoroethylene, polyacrylonitrile, polyimide, polyamide, polyester and natural fiber.
[0067] The secondary battery also includes an electrolyte, which includes an organic solvent, an electrolyte lithium salt and an additive. The electrolyte lithium salt can be LiPF used in high-temperature electrolytes. 6 and / or LiBOB; it can also be LiBF used in low temperature electrolytes 4 、LiBOB、LiPF 6 It can also be LiBF used in the overcharge-proof electrolyte 4 、LiBOB、LiPF 6 , LiTFSI; it can also be LiClO 4 、LiAsF 6 、LiCF 3 SO 3 、LiN(CF 3 SO 2 ) 2At least one of the above. The organic solvent may be a cyclic carbonate, including PC, EC; a chain carbonate, including DEC, DMC, or EMC; or a carboxylic acid ester, including PP, MA, EA, EP, etc. The additives include but are not limited to film-forming additives, conductive additives, flame retardant additives, overcharge prevention additives, and additives for controlling H in the electrolyte. 2 At least one of an additive for increasing the content of O and HF, an additive for improving low temperature performance, and a multifunctional additive.
[0068] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be further described in detail below in conjunction with specific implementation methods, but the implementation methods of the present invention are not limited thereto.
[0069] Example 1
[0070] A positive electrode sheet, comprising an active material layer, a multifunctional coating and an aluminum foil. The multifunctional coating can firmly adhere to the surface of the aluminum foil, which can not only reduce the surface contact resistance, but also reduce the generation of positive electrode collector burrs when the battery cell is subjected to safety testing, and reduce the contact short circuit between the positive electrode collector burrs and the negative electrode active material in an unstable charging state, thereby improving the safety of the battery cell. At the same time, the solid electrolyte contained in the multifunctional coating can also conduct ions, reduce the interface impedance, and enable the battery cell to maintain good low-temperature discharge performance and cycle performance.
[0071] Wherein, the multifunctional coating is arranged on the two surfaces of the aluminum foil, and the double-sided film resistance R 2 (Ω), double-sided film resistance R of the positive electrode multifunctional coating 1 (Ω) and its total thickness d (μm) should satisfy 2≤R 1 *R 2 *d≤45. In addition, the mass content of the solid electrolyte in the multifunctional coating accounts for c and the ionic conductivity of the solid electrolyte at room temperature (S / cm)Satisfy The multifunctional coating includes, in addition to the solid electrolyte, a first conductive agent, conductive carbon black Super P Li, a first binder, PVDF, and boehmite in a certain proportion. Specifically, the preparation method thereof is as follows:
[0072] Using NMP (N-methylpyrrolidone) as solvent, 76 parts of boehmite, 15 parts of solid electrolyte Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 (lithium aluminum titanium phosphate, LATP, ionic conductivity is 1.83×10 -4 S / cm, Dv 50 is 0.5μm), 6 parts of the first binder PVDF and 3 parts of the first conductive agent Super P Li are mixed evenly to obtain a multifunctional coating slurry with a solid content of 20% and a viscosity of 100mPa·s. The multifunctional coating slurry is coated on both sides of the aluminum foil by gravure printing. The oven temperature is set to 95°C during printing, and the printing speed is 30m / min. Finally, the double-sided coating surface density is 15mg / 1540.25mm 2 , the total double-sided thickness (referring to the sum of the thickness of the multifunctional coatings arranged on the two surfaces of the aluminum foil) is 8.1μm, the double-sided membrane resistance is 1.5Ω (the test pressure is 0.4t), and the adhesion between the multifunctional coating and the current collector is 215N / m for the aluminum foil containing the multifunctional coating.
[0073] The obtained aluminum foil containing the multifunctional coating is applied to a lithium ion battery. The preparation method of the lithium ion battery is as follows:
[0074] (1) Preparation of positive electrode sheet:
[0075] Lithium cobaltate, conductive agent (mixture of conductive carbon black and carbon nanotubes, mass ratio 6:5), PVDF binder and NMP are mixed evenly at a mass ratio of 97.6:1.1:1.3:35 to prepare a positive electrode slurry with a solid content of 75% and a viscosity of 7000mPa·s. The positive electrode slurry is coated on one side of the current collector aluminum foil containing the multifunctional coating, and after drying and rolling at 85°C, the positive electrode slurry is coated and dried on the other side of the current collector aluminum foil containing the multifunctional coating according to the above method, and then the positive electrode sheet coated with the positive electrode active material layer on both sides is cold pressed; then the edges are trimmed and stripped to prepare a lithium-ion battery positive electrode sheet (double-sided membrane sheet resistance is 1.7Ω, test pressure is 0.4t).
[0076] (2) Preparation of negative electrode sheet:
[0077] Using water as solvent, graphite, thickener and SBR binder are mixed evenly in a mass ratio of 97.7:1.1:1.2 to prepare a lithium ion battery negative electrode slurry with a solid content of 50% and a viscosity of 5000 mPa·s, which is coated on one side of the collector copper foil and dried and rolled up at 80°C. Then, the negative electrode slurry is coated and dried on the other side of the copper foil according to the above method to obtain a negative electrode sheet coated with active materials on both sides.
[0078] (3) Preparation of electrolyte:
[0079] LiPF 6 ) was dissolved in a mixed solvent of dimethyl carbonate (DMC), ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (the mass ratio of DMC, EC and EMC was 3:5:2) to obtain an electrolyte.
[0080] (4) Preparation of batteries:
[0081] The prepared positive electrode sheet, negative electrode sheet and separator are wound into a battery cell with a capacity of about 5Ah. The separator is located between adjacent positive and negative electrode sheets, the positive electrode is spot welded out with an aluminum tab, and the negative electrode is spot welded out with a nickel tab; the battery cell is then placed in an aluminum-plastic packaging bag, baked, and injected with the above electrolyte, and finally made into a lithium-ion battery through packaging, formation, capacity division and other processes.
[0082] Example 2
[0083] The difference from Example 1 is that the dosage of the components of the multifunctional coating is different, specifically: the dosage of LATP is 50 parts, and the dosage of boehmite is 41 parts.
[0084] The rest is the same as Example 1 and will not be described again here.
[0085] Example 3
[0086] The difference from Example 1 is that the components of the multifunctional coating are different, specifically: 15 parts of LATP are replaced by 15 parts of Li 7 La 3 Zr 2 O 12 (Lithium lanthanum zirconium oxide (LLZO), ionic conductivity is 1.87×10 -4 S / cm, D v50 0.5μm)
[0087] The rest is the same as Example 1 and will not be described again here.
[0088] Example 4
[0089] The difference from Example 1 is that the components and contents of the multifunctional coating are different, specifically: 15 parts of LATP are replaced by 30 parts of Li 0.33 La 0.57 TiO 3 (Lithium lanthanum titanate, LLTO, ionic conductivity is 2.29×10 -5 S / cm, D v50 0.5 μm), and the amount of boehmite used was 61 parts.
[0090] The rest is the same as Example 1 and will not be described again here.
[0091] Example 5
[0092] The difference from Example 1 is that the components and contents of the multifunctional coating are different, specifically: 15 parts of LATP are replaced by 60 parts of Li 0.33 La 0.57 TiO 3(Lithium lanthanum titanate, LLTO, ionic conductivity is 2.29×10 -5 S / cm, D v50 0.5 μm), and the amount of boehmite used was 31 parts.
[0093] The rest is the same as Example 1 and will not be described again here.
[0094] Example 6
[0095] The difference from Example 1 is that the components and contents of the multifunctional coating are different, specifically: 15 parts of LATP are replaced by 80 parts of Li 0.33 La 0.57 TiO 3 (Lithium lanthanum titanate, LLTO, ionic conductivity is 2.29×10 -5 S / cm, D v50 0.5 μm), and the amount of boehmite used was 11 parts.
[0096] The rest is the same as Example 1 and will not be described again here.
[0097] Example 7
[0098] The difference from Example 1 is that the LATP particle size of the multifunctional coating is different, specifically: the particle size D of LATP is v50 1μm.
[0099] The rest is the same as Example 1 and will not be described again here.
[0100] Example 8
[0101] The difference from Example 1 is that the LATP particle size of the multifunctional coating is different, specifically: the particle size D of LATP is v50 It is 1.3μm.
[0102] The rest is the same as Example 1 and will not be described again here.
[0103] Example 9
[0104] The difference from Example 1 is that the dosage of the components of the multifunctional coating is different, specifically: the dosage of the first conductive agent Super P Li is reduced from 3 parts to 2 parts, and the dosage of boehmite is increased from 76 parts to 77 parts.
[0105] The rest is the same as Example 1 and will not be described again here.
[0106] Example 10
[0107] The difference from Example 1 is that the solid content of the prepared multifunctional coating slurry is 23%, the viscosity is 157 mPa·s, the oven temperature is set to 95°C during gravure printing, the printing speed is 25 m / min, and the final multifunctional coating thickness is 10.3 μm.
[0108] The rest is the same as Example 1 and will not be described again here.
[0109] Embodiment 11
[0110] The difference from Example 1 is that the dosage of the components of the multifunctional coating is different, specifically: the dosage of the first conductive agent Super P Li is increased from 3 parts to 4 parts, and the dosage of boehmite is reduced from 76 parts to 75 parts.
[0111] The rest is the same as Example 1 and will not be described again here.
[0112] Example 12
[0113] The difference from Example 1 is that the dosage of the components of the multifunctional coating is different, specifically: the dosage of the first conductive agent Super P Li is increased from 3 parts to 4 parts, the dosage of boehmite is reduced from 76 parts to 75 parts, the prepared multifunctional coating slurry has a solid content of 12% and a viscosity of 81 mPa·s, and the final multifunctional coating thickness is 1 μm.
[0114] The rest is the same as Example 1 and will not be described again here.
[0115] Embodiment 13
[0116] The difference from Example 1 is that the amount of components of the multifunctional coating is different, specifically: the amount of the first conductive agent Super P Li is increased from 3 parts to 5 parts, the amount of boehmite is reduced from 76 parts to 74 parts, the solid content of the prepared multifunctional coating slurry is 38%, and the viscosity is 165mPa·s. When performing gravure printing, the oven temperature is set to 95°C, the printing speed is 25m / min, and the thickness of the final multifunctional coating is 20μm.
[0117] The rest is the same as Example 1 and will not be described again here.
[0118] Embodiment 14
[0119] The difference from Example 1 is that the dosage of the components of the multifunctional coating is different, specifically: the dosage of LATP is 11 parts, and the dosage of boehmite is 80 parts.
[0120] The rest is the same as Example 1 and will not be described again here.
[0121] Embodiment 15
[0122] The difference from Example 1 is that the components and dosage of the multifunctional coating are different, specifically: 15 parts of LATP are replaced by 91 parts of Li 1.75 ZrCl 4.75 O 0.5 (Lithium zirconium oxychloride, LZCO, ionic conductivity is 2.42×10 -3 S / cm, D v50 0.5 μm), and does not contain boehmite.
[0123] The rest is the same as Example 1 and will not be described again here.
[0124] Comparative Example 1
[0125] The current collector used in preparing the positive electrode sheet is a plain aluminum foil without a multifunctional coating.
[0126] The rest is the same as Example 1 and will not be described again here.
[0127] Comparative Example 2
[0128] The difference from Example 1 is that the amount of LATP used is 10 parts, and the amount of boehmite used is 81 parts.
[0129] The rest is the same as Example 1 and will not be described again here.
[0130] Comparative Example 3
[0131] The difference from Example 1 is that the amount of the first conductive agent Super P Li is reduced from 3 parts to 0.3 parts, and the amount of boehmite is increased from 76 parts to 78.7 parts.
[0132] The rest is the same as Example 1 and will not be described again here.
[0133] Comparative Example 4
[0134] The difference from Example 1 is that the amount of the first conductive agent Super P Li is increased from 3 parts to 6 parts, and the amount of boehmite is reduced from 76 parts to 73 parts.
[0135] The rest is the same as Example 1 and will not be described again here.
[0136] Comparative Example 5
[0137] The difference from Example 1 is that the amount of the first binder PVDF is increased from 6 parts to 15 parts, and the amount of boehmite is reduced from 76 parts to 67 parts.
[0138] The rest is the same as Example 1 and will not be described again here.
[0139] Comparative Example 6
[0140] The difference from Example 1 is that the solid content of the prepared multifunctional coating slurry is 45%, the viscosity is 191 mPa·s, the oven temperature is set to 95°C during gravure printing, the printing speed is 25 m / min, and the final multifunctional coating thickness is 25 μm.
[0141] The rest is the same as Example 1 and will not be described again here.
[0142] The parameters in Examples 1-15 and Comparative Examples 1-6 are shown in Table 1.
[0143] Diaphragm resistance test method: The instrument used for the diaphragm resistance test is the ACCFILM diaphragm resistance test system (model TT-ACCF-G2A) of Hangzhou Chuanyuan Technology Co., Ltd. The pressure during the test is 0.4t and the pressure holding time is 10s.
[0144] Table 1 Parameters of Examples 1-15 and Comparative Examples 1 to 6
[0145]
[0146]
[0147] In order to verify the effect of the introduction of the multifunctional coating of the present invention on the performance of the battery cell, the safety performance (puncture test), low-temperature discharge performance and cycle performance of the battery cell were tested.
[0148] Acupuncture test method: Charge to 4.45V at 1.0C constant current and constant voltage at room temperature, with a cut-off rate of 0.05C. Then, the fully charged cell is subjected to acupuncture test. During the test, the deep pit side of the cell faces upward, and a steel nail with a diameter of 4.0mm is used to completely pierce the cell at a speed of 40mm / s. The nail piercing position is located at the left, middle, and right positions of the largest surface of the cell (5 cells are tested at each position). Keep for 1 hour. The cell passes the test if it does not catch fire or explode.
[0149] Low temperature discharge performance test method: discharge at 1C constant current to 3V, leave for 5 minutes; set the temperature box to 25℃, leave for 60 minutes; charge at 1.0C constant current and constant voltage to 4.45V, cut-off rate 0.02C; leave for 5 minutes, discharge at 0.2C constant current to 3V, and record the capacity when discharged at 0.2C to 3V as the initial capacity C 0 ; Set the incubator to 25℃ and leave for 60min; Charge to 4.45V at 1.0C constant current and constant voltage, with a cut-off rate of 0.02C; Leave for 5min, set the incubator to -10℃, leave for 120min, then discharge the cell at 0.2C to 3.0V, and record the capacity C when discharged to 3.4V and 3.0V 1 and C 2 , C 1 With C 0The ratio is the capacity retention rate when discharged to 3.4V at -10℃.
[0150] Cycling performance test method: Under the condition of ambient temperature of 25±2℃, discharge the battery cell to 3.0V at 0.2C constant current, then charge to 4.45V at 3C constant current and constant voltage, with a cut-off rate of 0.05C, and record the voltage, internal resistance, capacity, and thickness of the battery cell when it is fully charged for the first time (600gPPG is used for thickness measurement). The cycling process is in accordance with the following HFC format: discharge to 3V at 0.2C constant current; charge to 4.25V at 3.0C constant current; charge to 4.25V at 2.5C constant current; charge to 4.45V at 2.0C constant current; charge to 4.50V at 1.4C constant current and constant voltage, with a cut-off rate of 0.3C; charge to 4.45V at 2A constant current and constant voltage, with a cut-off rate of 0.05C; discharge to 3V at 1.0C constant current. Completing the above steps is one cycle. After 49 cycles, perform low current recovery according to the following format: charge to 4.25V at 3.0C constant current; charge to 4.25V at 2.5C constant current; charge to 4.45V at 2.0C constant current; charge to 4.50V at 1.4C constant current and constant voltage, with a cut-off rate of 0.3C; charge to 4.45V at 2A constant current and constant voltage, with a cut-off rate of 0.05C; discharge to 3V at 0.2C constant current; charge to 4.45V at 3.0C constant current and constant voltage, with a cut-off rate of 0.05C. Record the fully charged cell voltage, internal resistance, and thickness (600gPPG is used for thickness measurement) every 100 cycles.
[0151] The secondary batteries obtained in Examples 1 to 15 and Comparative Examples 1 to 6 were tested. The test results are shown in Table 2 below.
[0152] Table 2 Test results of Examples 1 to 15 and Comparative Examples 1 to 6
[0153]
[0154] From the comparison of the test results in the above table, it can be seen that compared with comparative example 1, after the multifunctional coating is introduced into Examples 1 to 15, the low-temperature discharge performance of the battery cell has been significantly improved by ~8%, and the capacity retention rate after 800cls of normal temperature cycling has also increased by ~2% (this value is a significant improvement in the field of lithium batteries). 1 *R 2 * For samples with d < 2, the safety performance of the embodiment is also significantly improved, and the pass rate of the needle puncture test is increased from 20% to > 90%; 1 *R 2 * For samples with d>45, the capacity retention rate after 800 cycles at room temperature in the embodiment is>89%. 1 *R 2 *d is in the preferred range, i.e.: 15≤R 1 *R 2*When d≤35, the performance of the sample is even better, the pass rate of the needle puncture test reaches 100%, and the capacity retention rate after 800 cycles at room temperature is greater than 90%.
[0155] In addition, it is also found from Comparative Example 2 that when When the ionic conductivity of the solid electrolyte deteriorates, the improvement of the low-temperature discharge performance of the battery cell becomes insignificant. Example 4 shows that when the ionic conductivity of the solid electrolyte deteriorates, in order to achieve the same effect, its dosage needs to be significantly increased (from 15% in Example 1 to 30%). However, from Examples 5-6 and 14-15, it can be seen that when the dosage of the solid electrolyte reaches a certain level, the improvement of the low-temperature performance of the battery cell is no longer obvious. When the amount of solid electrolyte is small, and the low-temperature discharge performance is significantly improved, the overall benefit is better.
[0156] In summary, it can be concluded that by introducing a solid electrolyte into the multifunctional coating and adjusting the double-sided film resistance R 1 and thickness d, double-sided film resistance R of the positive electrode 2 The relationship between the parameters is defined, and the content c of the solid electrolyte in the multifunctional coating and the ionic conductivity at room temperature are determined. The relationship between 2≤R is limited, thereby reducing the internal resistance of the battery, which not only maintains the safety performance of the coating, but also the solid electrolyte has excellent ionic conductivity at low temperatures, taking into account the low-temperature discharge performance and cycle performance of the battery. The battery cell provided by the present invention satisfies 2≤R 1 *R 2 *d≤45, and The puncture pass rate can be greater than 90%, the discharge capacity at -10°C is not less than 79%@3.4V, and the capacity retention rate after 800 cycles at 25°C is not less than 89%.
[0157] The above description is only a partial or preferred embodiment of the present invention. Neither the text nor the drawings can limit the scope of protection of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the overall concept of the present invention, or direct / indirect application in other related technical fields are included in the scope of protection of the present invention.
Claims
1. A positive electrode sheet, characterized in that: include: current collector; A multifunctional coating disposed on at least one side surface of the current collector; A positive electrode active material layer disposed on a surface of the multifunctional coating layer away from the current collector; The multifunctional coating includes a solid electrolyte, a first conductive agent and a first binder, and the resistance, total thickness of the multifunctional coating and the resistance of the positive electrode sheet satisfy the relationship: 2≤R1*R2*d≤45, wherein R1 is the resistance of the multifunctional coating, R2 is the resistance of the positive electrode sheet, and d is the total thickness of the multifunctional coating; The mass ratio c of the solid electrolyte to the multifunctional coating is related to the ionic conductivity of the solid electrolyte at room temperature. Satisfies the relationship:
2. The positive electrode sheet according to claim 1, characterized in that: The resistance and total thickness of the multifunctional coating and the resistance of the positive electrode sheet satisfy the relationship: 15≤R1*R2*d≤35.
3. The positive electrode sheet according to claim 1, characterized in that: The mass ratio c of the solid electrolyte to the multifunctional coating is related to the ionic conductivity of the solid electrolyte at room temperature. Satisfies the relationship:
4. The positive electrode sheet according to any one of claims 1 to 3, characterized in that: The total thickness d of the multifunctional coating is 1 μm to 20 μm; And / or, when tested under a test pressure of 0.4t, the resistance R1 of the multifunctional coating is 0.5Ω to 5Ω.
5. The positive electrode sheet according to claim 4, characterized in that: The mass ratio of the solid electrolyte, the first conductive agent, and the first binder in the multifunctional coating is (1-95): (0.5-5): (0.5-10); And / or, the total thickness d of the multifunctional coating is 7.5-10.3 μm.
6. The positive electrode sheet according to claim 5, characterized in that: The first conductive agent is selected from one or both of conductive carbon black and carbon nanotubes; and / or the first binder is selected from at least one of polyvinylidene fluoride, styrene-butadiene rubber, sodium carboxymethyl cellulose and polyacrylate.
7. The positive electrode sheet according to claim 1, characterized in that: The multifunctional coating further comprises at least one of a thermally stable active material and an inert inorganic filler; And / or, the mass ratio of the solid electrolyte, the first conductive agent, the first binder, the thermally stable active substance, and the inert inorganic filler in the multifunctional coating is (1-95): (0.5-5): (0.5-10): (1-95): (1-95).
8. The positive electrode sheet according to claim 7, characterized in that: The double-sided coating density of the multifunctional coating is 2 mg / 1540.25 mm 2 ~35mg / 1540.25mm 2 ; And / or, the thermally stable active material is selected from one or both of lithium iron phosphate and lithium iron manganese phosphate; the inert inorganic filler is selected from one or both of alumina and boehmite.
9. The positive electrode sheet according to claim 1, characterized in that: The solid electrolyte is selected from Li 1+x Al x M 2-x (PO4)3, Li7La3N2O 12 , Li 3y La 2 / 3-y TiO3、Li 7-z Ln3Z 2-z Ta z O 12 and Li 2+a-b ZrCl 6-a-b O a At least one of the following, wherein 0<x<0.5, M is selected from Ti and / or Ge, N is selected from at least one of Zr, Sn, and Ta, 0<y<0.16, 0<z<2, 0≤a≤2, 0≤b≤0.75; and / or the particle size D of the solid electrolyte is v50 It is 0.2μm~1.5μm.
10. A secondary battery, comprising a positive electrode sheet, a negative electrode sheet, and a separator between the positive electrode sheet and the negative electrode sheet, characterized in that: The positive electrode sheet is the positive electrode sheet as claimed in any one of claims 1 to 9.