Negative current collector in negative-electrode-free lithium ion battery and modification method of negative current collector
By combining the metal foam material with zinc glutamate and calcining, the modified negative electrode current collector solves the problems of uneven lithium deposition and lithium dendrites in negative electrode-free lithium ion batteries, and improves the safety and circulation performance of the battery.
Patent Information
- Application Number
- CN202411304886.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-22
AI Technical Summary
The negative electrode-free lithium-ion battery has poor circulation stability and the generation of lithium dendrites due to uneven lithium deposition, which threatens battery safety.
The original negative electrode current collector is used to make a metal foam material, and it is soaked in zinc glutamate solution and then calcined to form zinc glutamate-metal material. The modified negative electrode current collector has its porous structure and zinc philtrum Lithium characteristics improve the deposition morphology of lithium and form a stable solid electrolyte interface film.
It improves the safety performance and cycling performance of the battery, prevents the vertical growth of lithium dendrites, reduces the local current density, and enhances the lithium+ transmission rate and deposition kinetics.
Smart Images

Figure CN119008960A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of negative electrode-free lithium ion batteries, and in particular to a negative electrode current collector in a negative electrode-free lithium ion battery and a modification method thereof. Background Art
[0002] The negative electrode of the negative electrode-free lithium battery directly uses the current collector copper foil as the negative electrode, and the positive electrode still uses the traditional positive electrode material. The battery of this structure can bring more excellent energy density, especially volume energy density, and greatly simplify the battery manufacturing process, reduce manufacturing costs, and improve battery safety. However, compared with traditional lithium-ion batteries, the negative electrode-free battery without the negative electrode active material still has some problems that hinder its practical application. One of the most important problems is the problem of cycle stability, which is manifested as a rapid decay of battery capacity; another problem is that lithium dendrites are easily generated, which threaten the safety of the battery. The main reasons for the above problems are: because the substrate is the current collector copper foil, lithium deposition is heterogeneous deposition, nucleation is more difficult, and a large polarization current will be generated, resulting in uneven deposition of lithium metal. This uneven deposition will cause lithium deposition to form lithium dendrites in the subsequent deposition process. At the same time, this lithium deposition morphology has a large specific surface area, and consumes more active lithium in the process of forming SEI film (solid electrolyte interface). During stripping, part of the active lithium will be wrapped by the SEI film and completely lose contact with other parts, and cannot participate in the subsequent electrochemical reaction to become dead lithium.
[0003] The Chinese invention patent with publication number CN113013417A discloses a method for preparing a negative electrode current collector for a negative electrode-free lithium metal battery, wherein a plurality of conductive layers, electronic conductor layers or ion-electronic mixed conductor layers are loaded on the negative electrode current collector, and the negative electrode current collector has good lithium affinity, or can alloy with lithium to have a lower nucleation barrier, or can form an ion conductor, forming a stable lithium affinity SEI layer, and effectively improving the lithium deposition morphology. However, the flat current collector used in this scheme is not suitable for preventing the vertical growth of Li dendrites and significant volume changes during the cycle, and a short circuit will occur inside the battery. Summary of the invention
[0004] In order to overcome the defects of the prior art, the technical problem to be solved by the present invention is to provide a negative electrode current collector in a negative electrode-free lithium ion battery and a modification method thereof which can improve the lithium deposition morphology and cycle performance.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for modifying a negative electrode current collector in a negative electrode-free lithium ion battery, comprising the following steps: using the original negative electrode current collector to make a metal foam material, soaking the metal foam material in a zinc glutamate solution, and then drying to obtain a zinc glutamate-metal material, and calcining the zinc glutamate-metal material to obtain a modified negative electrode current collector.
[0006] Another technical solution adopted by the present invention is: the negative electrode current collector in the negative electrode-free lithium ion battery is modified by the above-mentioned modification method.
[0007] The beneficial effects of the present invention are as follows: the modification method of the present invention firstly prepares a metal foam material by adopting the original negative electrode current collector, and the porous structure of the metal foam material can reduce the local current density and improve the safety performance and cycle performance of the battery; then the metal foam material is combined with zinc glutamate and calcined, and the presence of zinc can effectively improve the lithium deposition morphology, form a stable SEI film, and improve the cycle performance of the battery; the interaction between zinc glutamate and Li (lithium) can form an SEI film, which improves the Li+ transmission rate and deposition kinetics, and improves the cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 It is a schematic diagram showing the effect of the copper foil on lithium ions before modification in Example 1 of the present invention;
[0009] Figure 2 It is a schematic diagram showing the effect of the modified negative electrode current collector foil on lithium ions in Example 1 of the present invention;
[0010] Figure 3 It is a box diagram of the first performance test of preparing a negative electrode-free lithium ion battery using the modified negative electrode current collector and copper foil of Example 1 as the negative electrode current collector;
[0011] Figure 4 The figure shows the statistical graph of cycle test results of preparing negative electrode-free lithium ion batteries using the modified negative electrode current collector and copper foil of Example 1 as negative electrode current collectors respectively;
[0012] Description of labels:
[0013] 1. Copper foil; 2. Lithium dendrites; 3. Copper foam; 4. Zinc glutamate-copper foam alloy. DETAILED DESCRIPTION
[0014] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in combination with the implementation modes and the accompanying drawings.
[0015] Please refer to Figure 1 as well as Figure 2 , please refer to Figure 1 and Figure 2 A method for modifying a negative electrode current collector in a negative electrode-free lithium ion battery comprises the following steps: using the original negative electrode current collector to make a metal foam material, immersing the metal foam material in a zinc glutamate solution, and then drying to obtain a zinc glutamate-metal material, and calcining the zinc glutamate-metal material to obtain a modified negative electrode current collector.
[0016] From the above description, it can be seen that the beneficial effect of the present invention is that: the modification method of the present invention prepares a modified negative electrode current collector by using the original negative electrode current collector to make a metal foam material and combining the metal foam material with zinc glutamate and calcining it. The modified negative electrode current collector can improve the safety performance and cycle performance of the battery.
[0017] Among them, the metal foam material is a three-dimensional interconnected porous structure with a large number of internal pores, which can provide a "cage" for Li dendrites, so that the dendrites are preferentially deposited in the pore space rather than in the vertical direction facing the cathode, thereby preventing short circuits and related safety issues; at the same time, the metal foam material has a large surface area, which can effectively reduce the local concentrated current density, thereby reducing the overpotential of Li nucleation and improving the safety and cycle performance of the battery.
[0018] Zinc in zinc glutamate has good lithium affinity. When lithium nucleates, Li reacts with zinc metal to produce a solid solution buffer layer. Lithium is deposited on the solid solution buffer layer, which is easy for lithium nucleation and growth. Therefore, the alloyed material after calcination of zinc glutamate-metal material has a lower nucleation barrier and forms a stable lithium affinity SEI layer, which effectively improves the lithium deposition morphology and improves the first efficiency and cycle performance of the battery. Zinc glutamate has abundant -OH, which can promote the adsorption of lithium ions. Lithium ions can form transient Li-N bonds, which enhances the affinity with Li + The interaction forms the SEI film of Li3N (lithium nitride), which improves the Li + transfer rate and deposition kinetics, improving the cycling performance of the battery.
[0019] Furthermore, when the original negative electrode current collector is copper foil, the preparation step includes: connecting the copper foil as a working electrode to a counter electrode and placing it in an electrolyte for electrolysis to obtain foamed copper.
[0020] From the above description, it can be seen that the poor lithium affinity of commercial copper foil surface leads to moss-like lithium deposition, more side reactions between lithium and electrolyte, more active lithium consumption, and lower battery coulomb efficiency. The commonly used copper current collector is not conducive to lithium metal deposition because it has an FCC (face-centered cubic lattice) crystal structure and is difficult to form a lithium alloy solid solution with lithium metal. Therefore, copper foil is used for modification, and the modification effect is the best.
[0021] Furthermore, the surface oxide layer of the copper foil is polished before modification, and then cleaned with sulfuric acid solution, deionized water and anhydrous ethanol in sequence.
[0022] Furthermore, the electrolysis is specifically as follows: at a current density of 2 to 8 Acm -2 Electrolyze for 4 to 6 seconds under the same conditions.
[0023] From the above description, it can be seen that if the current density is too small and the time is too short, the pore size of the copper sheet will be insufficient, and lithium dendrites will easily deposit on the surface, causing the battery performance to decline. If the current density is too large and the time is too long, the pore size and specific surface area will be greatly increased, but the surface of the copper foil will become sharper, resulting in uneven Li deposition and a decline in battery cycle performance. Therefore, the current density is controlled to be 2-8Acm -2 .
[0024] Furthermore, the electrolyte includes 0.15-0.25 mol / L copper sulfate, 0.6-0.7 mol / L sulfuric acid, 1-1.4 mol / L ammonium sulfate and 0.3-0.5 mol / L 1,2,3-benzotriazole.
[0025] Furthermore, the zinc glutamate solution includes zinc glutamate, deionized water and hydrochloric acid solution.
[0026] Furthermore, the weight ratio of zinc glutamate, deionized water and hydrochloric acid in the hydrochloric acid solution is 1:200:0.65-0.67.
[0027] From the above description, it can be seen that zinc glutamate is a solid powder and has poor solubility in deionized water. Adding hydrochloric acid can provide an acidic environment to accelerate its dissolution. The content of zinc glutamate affects the formation of zinc-copper alloy. The content of hydrochloric acid should not be too high. Too high a hydrochloric acid content will cause porous copper to be etched by acid.
[0028] If the concentration of zinc glutamate is too low and the content is insufficient, zinc cannot form a good zinc-copper alloy with copper in the subsequent process, and the effect on the performance of the battery cell is small. If the concentration is too high, the porous structure formed may be aggregated by zinc ions, and the porous structure will lose its effect on the performance of the battery cell.
[0029] Furthermore, the concentration of the hydrochloric acid solution is 2.5-3.5M.
[0030] Furthermore, the soaking time is 10 to 14 hours.
[0031] From the above description, it can be seen that too long an immersion time will affect the production efficiency, and too short an immersion time cannot make zinc glutamate better infiltrate the porous copper; therefore, the immersion time is controlled to be 10 to 14 hours.
[0032] Furthermore, the drying temperature is 45-55°C.
[0033] Furthermore, the calcination is specifically as follows: heating to 400-600° C. at a heating rate of 5-10 min / ° C. for calcination for 4-8 hours under an inert gas atmosphere.
[0034] From the above description, it can be known that calcination is to make zinc and the metal foam material form an alloy better.
[0035] During calcination, the temperature of the present invention is low, and the zinc ions cannot be well fused with the copper to form an alloy. If the temperature is too high, the holes of the alloy porous copper will melt and close. A slow heating rate affects the production efficiency, but a too fast heating rate will cause the formed holes to collapse. If the calcination time is too long, it will cause the holes to collapse on the one hand, and the production efficiency is low on the other hand. If the time is too short, the zinc ions cannot be better fused with the copper. Therefore, during calcination, the temperature is raised to 400-600°C at a heating rate of 5-10min / °C in an inert gas atmosphere and calcined for 4-8h.
[0036] Another technical solution adopted by the present invention is: the negative electrode current collector in the negative electrode-free lithium ion battery is modified by the above-mentioned modification method.
[0037] It can be seen from the above description that the negative electrode current collector of the present invention can improve the safety performance and cycle performance of the battery.
[0038] Embodiment 1 of the present invention is: a method for modifying a negative electrode current collector in a negative electrode-free lithium ion battery, the steps are as follows:
[0039] S1: Use sandpaper to grind off the oxide layer of the copper foil, and then rinse the copper foil with 0.1 mol / L sulfuric acid solution, deionized water and anhydrous ethanol for 60 seconds in turn to remove impurities on the surface of the copper foil.
[0040] S2: Prepare electrolyte, which is composed of 0.2mol / L copper sulfate, 0.7mol / L sulfuric acid, 1.2mol / L ammonium sulfate, 0.4mol / L 1,2,3-benzotriazole and deionized water; connect copper foil as working electrode and platinum mesh as counter electrode, and place them in electrolyte at a current density of 6Acm -2 The electrolysis was carried out for 5s under the above conditions. During the electrolysis, a large number of hydrogen bubbles were generated on the copper foil to obtain foamed copper.
[0041] S3: Add 0.5 g of zinc glutamate powder into 100 mL of deionized water, and at the same time, add 3 mL of 3 M HCl using a rubber-tipped dropper and ultrasonicate at 25°C for 30 min to obtain a transparent glutamate solution; soak the foamed copper in the zinc glutamate solution for 12 h, and then dry at 50°C to obtain zinc glutamate-copper.
[0042] S4: zinc glutamate-copper is placed in a CVD furnace for calcination. The temperature is raised to 500° C. at a heating rate of 8 min / ° C. in a nitrogen atmosphere and calcined for 6 h to obtain a modified negative electrode current collector.
[0043] Embodiment 2 of the present invention is: a method for modifying a negative electrode current collector in a negative electrode-free lithium ion battery, the steps are as follows:
[0044] S1: Use sandpaper to grind off the oxide layer of the copper foil, and then rinse the copper foil with 0.1 mol / L sulfuric acid solution, deionized water and anhydrous ethanol for 60 seconds in turn to remove impurities on the surface of the copper foil.
[0045] S2: Prepare electrolyte, which is composed of 0.15mol / L copper sulfate, 0.6mol / L sulfuric acid, 1mol / L ammonium sulfate, 0.3mol / L 1,2,3-benzotriazole and deionized water; connect copper foil as working electrode and platinum mesh as counter electrode, and place them in electrolyte at a current density of 2Acm -2 The electrolysis was carried out for 6s under the above conditions. During the electrolysis, a large number of hydrogen bubbles were generated on the copper foil to obtain foamed copper.
[0046] S3: 0.5 g of zinc glutamate powder was added to 100 mL of deionized water, and 3.6 mL of 2.5 M HCl was added with a rubber-tipped dropper, and ultrasonicated at 25°C for 30 min to obtain a transparent glutamate solution; the foamed copper was immersed in the zinc glutamate solution for 10 h, and then dried at 45°C to obtain zinc glutamate-copper.
[0047] S4: zinc glutamate-copper is placed in a CVD furnace for calcination. The temperature is raised to 400° C. at a heating rate of 5 min / ° C. in a nitrogen atmosphere and calcined for 8 h to obtain a modified negative electrode current collector.
[0048] Embodiment 3 of the present invention is: a method for modifying a negative electrode current collector in a negative electrode-free lithium ion battery, the steps are as follows:
[0049] S1: Use sandpaper to grind off the oxide layer of the copper foil, and then rinse the copper foil with 0.1 mol / L sulfuric acid solution, deionized water and anhydrous ethanol for 60 seconds in turn to remove impurities on the surface of the copper foil.
[0050] S2: Prepare electrolyte, which is composed of 0.25mol / L copper sulfate, 0.65mol / L sulfuric acid, 1.4mol / L ammonium sulfate, 0.5mol / L 1,2,3-benzotriazole and deionized water; connect copper foil as working electrode and platinum mesh as counter electrode, and place them in electrolyte at a current density of 8Acm -2 The electrolysis was performed for 4 s under the above conditions. During the electrolysis, a large number of hydrogen bubbles were generated on the copper foil to obtain foamed copper.
[0051] S3: Add 0.5 g of zinc glutamate powder into 100 mL of deionized water, and at the same time, add 2.6 mL of 3.5 M HCl using a rubber-tipped dropper, and ultrasonicate for 30 min at 25°C to obtain a transparent glutamate solution; soak the foamed copper in the zinc glutamate solution for 14 h, and then dry it at 55°C to obtain zinc glutamate-copper.
[0052] S4: zinc glutamate-copper is placed in a CVD furnace for calcination. The temperature is raised to 600° C. at a heating rate of 10 min / ° C. in a nitrogen atmosphere and calcined for 4 h to obtain a modified negative electrode current collector.
[0053] Embodiment 4 of the present invention is: a negative electrode current collector in a negative electrode-free lithium ion battery obtained by the modification method of embodiment 1.
[0054] The modified negative electrode current collector and copper foil of Example 1 are respectively used as negative electrode current collectors to prepare negative electrode-free lithium ion batteries. The preparation method of the battery is as follows:
[0055] Step 1: The positive electrode slurry is prepared by mixing 3.5% PVDF (polyvinylidene fluoride) + 80% NMP (N-methylpyrrolidone) by mass fraction, 1.5% CNTs (carbon nanotubes), 1.0% carbon aerogel, 48.7% LFP (lithium iron phosphate) and the remaining NMP (N-methylpyrrolidone) for slurry, and NMP accounts for 26.7% of the slurry;
[0056] Lithium hexafluorophosphate (LiPF6) was dissolved in an amount of 1.2 mol / l in a solvent mixture of ethylene carbonate (EC), ethyl methyl carbonate (MEC) and diethyl carbonate (DEC) (mixing volume ratio: 40:40:20) to prepare an electrolyte;
[0057] Step 2: Apply the slurry on the aluminum foil → bake → roll to obtain the positive electrode; then die-cut the positive and negative current collectors → sweep the powder, and then stack the positive and negative current collectors and the separator in a Z-shape, spot weld, package, bake, inject liquid, form, degas once, bake, degas twice, separate the capacity, age, and seal twice to make the finished battery.
[0058] The battery is tested for initial efficiency and cycle testing. The test results are shown in Figure 3 and 4 ,Depend on Figure 3 and Figure 4 It can be seen that the negative electrode current collector modified by the modification method of the present invention is used to prepare a negative electrode-free lithium ion battery, which can improve the initial efficiency and cycle performance of the battery.
[0059] The test method for the first effect of the battery is:
[0060] (1) Charge the formed cell at 0.5C constant current and constant voltage to 3.65V and let it stand for 5 minutes;
[0061] (2) The battery cell is discharged at a constant current of 0.5C to 2.5V and left to stand for 5 minutes;
[0062] (3) 0.5C constant current and constant voltage charging to 3.65V, and let stand for 5 minutes;
[0063] (4) The battery cell is discharged at a constant current of 0.5C to 2.5V and left to stand for 5 minutes;
[0064] (5) 0.5C constant current and constant voltage charging to 3.65V, let stand for 5 minutes;
[0065] (6)Testing completed.
[0066] Battery cycle test method:
[0067] (1) Initial discharge of battery cells;
[0068] (2) The battery cells are charged at a constant power of 0.5×n×Prcn to a charge termination voltage of 3.65V and left to stand for 30 minutes;
[0069] (3) The battery cell is discharged at a constant power of 0.5×n'×Prdn' to a discharge end voltage of 2.5V and then left to stand for 30 minutes;
[0070] (4) Repeat steps (2) to (3) in a continuous cycle.
[0071] In summary, the negative electrode current collector in the negative electrode-free lithium ion battery and the modification method thereof provided by the present invention have the following advantages:
[0072] 1. Using foam metal material as the substrate, its three-dimensional interconnected porous structure can prevent safety problems such as short circuit caused by dendrites; the large surface area of the foam metal material can also effectively reduce the local concentrated current density, thereby reducing the overpotential of Li nucleation and improving the safety and cycle performance of the battery.
[0073] 2. The alloy formed by zinc glutamate and the surface of the foam metal material can form a stable lithium-philic SEI layer, which effectively improves the lithium deposition morphology and improves the initial efficiency and cycle performance of the battery. It can also improve the Li + transfer rate and deposition kinetics, further improving the battery's cycling performance.
[0074] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for modifying a negative electrode current collector in a negative electrode-free lithium ion battery, characterized in that: The following steps are involved: The original negative electrode current collector is used to make a metal foam material, which is immersed in a zinc glutamate solution and then dried to obtain a zinc glutamate-metal material. The zinc glutamate-metal material is calcined to obtain a modified negative electrode current collector.
2. The method for modifying the negative electrode current collector in a negative electrode-free lithium ion battery according to claim 1, characterized in that: When the original negative electrode current collector is copper foil, the preparation steps include: connecting the copper foil as a working electrode to a counter electrode and placing it in an electrolyte for electrolysis to obtain foamed copper.
3. The method for modifying the negative electrode current collector in a negative electrode-free lithium ion battery according to claim 2, characterized in that: The electrolysis is specifically: at a current density of 2 to 8 Acm -2 Electrolyze for 4 to 6 seconds under the same conditions.
4. The method for modifying the negative electrode current collector in a negative electrode-free lithium ion battery according to claim 2, characterized in that: The electrolyte includes 0.15-0.25 mol / L copper sulfate, 0.6-0.7 mol / L sulfuric acid, 1-1.4 mol / L ammonium sulfate and 0.3-0.5 mol / L 1,2,3-benzotriazole.
5. The method for modifying the negative electrode current collector in a negative electrode-free lithium ion battery according to claim 1, characterized in that: The zinc glutamate solution comprises zinc glutamate, deionized water and hydrochloric acid solution.
6. The method for modifying the negative electrode current collector in a negative electrode-free lithium ion battery according to claim 5, characterized in that: The concentration of the hydrochloric acid solution is 2.5-3.5M.
7. The method for modifying the negative electrode current collector in a negative electrode-free lithium ion battery according to claim 1, characterized in that: The soaking time is 10 to 14 hours.
8. The method for modifying the negative electrode current collector in a negative electrode-free lithium ion battery according to claim 1, characterized in that: The drying temperature is 45-55°C.
9. The method for modifying the negative electrode current collector in a negative electrode-free lithium ion battery according to claim 1, characterized in that: The calcination is specifically: heating to 400-600° C. at a heating rate of 5-10 min / ° C. and calcining for 4-8 hours in an inert gas atmosphere.
10. A negative electrode current collector in a negative electrode-free lithium ion battery obtained by modification using any modification method according to claims 1-9.