Preparation method and application of poly (ethylene carbonate)-based polymer solid electrolyte

Polyvinyl carbonate-based polymer solid electrolytes were prepared by copolymerizing ethylene carbonate and isocyanate, which solved the problems of flammability and volatility of organic electrolytes and the processing difficulty of inorganic electrolytes. This method achieves high voltage tolerance and stability over a wide temperature range, making it suitable for lithium-ion and sodium-ion batteries.

CN119009101APending Publication Date: 2024-11-22NORTHEASTERN UNIV CHINA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411283995.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The organic electrolytes used in existing lithium-ion and sodium-ion batteries have problems such as flammability, volatility, and poor electrochemical stability, which limit the development of high-energy-density batteries. Furthermore, inorganic solid electrolytes are difficult to process and their brittle fracture characteristics limit their application.

Method used

A polyvinyl carbonate-based polymer solid electrolyte was prepared by copolymerizing ethylene carbonate and isocyanate, combined with conductive salt and chain carbonate plasticizer, through in-situ polymerization. The resulting liquid mixture served as a precursor solution, and the polymer solid electrolyte was formed by static polymerization.

Benefits of technology

It achieves high voltage tolerance, wide temperature range stability and cation transport capability, with an electrochemical stability window of ≥5.4V vs. Li+/Li, ionic conductivity >10-3S cm-1, good thermal stability and flexibility, and is suitable for working environments from -20 to 60℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009101A_ABST
    Figure CN119009101A_ABST
Patent Text Reader

Abstract

The invention relates to the field of polymer solid electrolytes for lithium ion and sodium ion batteries, in particular to a preparation method and application of a poly (ethylene carbonate)-based polymer solid electrolyte, and belongs to the field of energy conversion and storage. The polymer solid electrolyte comprises ethylene carbonate, isocyanate, conducting salt and a chain carbonate plasticizer before polymerization, an initiator or a catalyst is added, a liquid mixture is formed to serve as a polymer solid electrolyte precursor solution, a polymerization reaction process is conducted during standing, and the poly (ethylene carbonate)-based polymer (quasi) solid electrolyte is obtained. The polymer solid electrolyte not only realizes high-voltage (greater than or equal to 5.4 V vs.Li < + > / Li) tolerance, can be matched with a high-voltage positive electrode to stably work for a long time, but also has very strong cation transmission capability, and can stably operate for a long time in a wide temperature range of-20 to 60 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer solid electrolytes for lithium ion and sodium ion batteries, in particular to a preparation method and application of a polyvinyl carbonate-based polymer solid electrolyte, and belongs to the field of energy conversion and storage. Background Art

[0002] With the rapid development of electric vehicles and green energy, there is an increasing urgent demand for high-safety, high-energy-density batteries. The use of high-capacity or high-voltage cathode materials is the primary consideration for achieving high energy density. However, organic electrolytes commonly used in commercial batteries, such as ethylene carbonate, dimethyl carbonate, 1,3-dioxolane, ethylene glycol dimethyl ether, etc., generally have safety defects such as volatility and flammability. At the same time, they have poor electrochemical stability, are easily oxidized and decomposed when matched with high-voltage cathodes, and can only work at room temperature. These problems have seriously restricted the further development of energy storage batteries. Solid electrolytes can solve the safety problems of energy storage batteries because of their non-flammable and non-leaking properties. Among the categories of solid electrolytes, inorganic solid electrolytes generally have higher ionic conductivity than other types of solid electrolytes, but the high processing temperature of ceramics, insufficient contact with electrodes, and brittle fracture characteristics limit their application in large batteries. In contrast, polymer solid electrolytes are favored by researchers due to their good processability, good environmental stability, and low cost. At the same time, polymer electrolytes can be prepared using advanced in-situ polymerization technology, which eliminates the complex processes of traditional non-in-situ polymerization processes such as polymer dissolution, film drying and electrolyte expansion, and is compatible with the existing battery industry system and has good application prospects.

[0003] At present, in-situ polymerized polymer electrolytes use monomers that are easy to undergo ring-opening polymerization or free radical polymerization (polymerization reaction) (such as 1,3-dioxolane ether electrolytes), for example:

[0004] Patent publication number CN118315658A points out that the electrochemical stability window of 1,3-dioxolane after polymerization is only 4.3Vvs.Li + / Li, its electrochemical stability is poor, and the electrochemical stability window after polymerization is not significantly widened compared with that before polymerization. In addition, the monomers cannot be completely reacted during the in-situ polymerization process, and the residual monomers that are easily oxidized will limit the electrochemical stability window of the gel electrolyte.

[0005] Patent publications CN110734517A and CN116111186A both propose a polyvinyl carbonate (VC) in-situ polymerization, which is composed of vinyl carbonate, C=C double bond compound, conductive lithium salt, porous support material, organic solvent and initiator to prepare block polymer electrolyte, and the electrochemical stability window is 5V vs.Li + / Li. However, with the increase of VC content, the impedance of organic components on the negative electrode surface continues to increase, resulting in a significant decrease in the low-temperature charging performance of the battery cell. The electrolyte can only perform at room temperature, which limits the use of this type of electrolyte assembled battery. Summary of the invention

[0006] In view of the above problems, the purpose of the present invention is to provide a preparation method and application of a polyvinyl carbonate-based polymer solid electrolyte, which not only achieves high voltage (≥5.4V vs.Li + / Li) tolerance can match the high voltage positive electrode to work stably for a long time, and it has a strong cation transport ability, and can operate stably for a long time in a wide temperature range of -20 to 60°C.

[0007] The technical solution of the present invention is:

[0008] A method for preparing a polyvinyl carbonate-based polymer solid electrolyte. The polymer solid electrolyte is prepared by direct polymerization of a precursor solution, or the polymer solid electrolyte is prepared by in-situ polymerization of a precursor solution inside a battery. Before polymerization, the precursor solution includes vinyl carbonate, isocyanate, conductive salt, and chain carbonate plasticizer, and an initiator or catalyst is added to form a liquid mixture as a polymer solid electrolyte precursor solution; a polymerization reaction process is carried out while standing to obtain a polyvinyl carbonate-based polymer solid electrolyte.

[0009] In the preparation method of the polyvinyl carbonate-based polymer solid electrolyte, the amount of isocyanate added is 0.04 to 1 of the molar number of vinyl carbonate, the concentration of the conductive salt is 0.5 mol / L to 5 mol / L, the amount of plasticizer added is 0.2 to 1.5 of the molar number of vinyl carbonate, and the amount of initiator or catalyst added is 0.1 mmol / L to 1 mol / L.

[0010] The preparation method of the polyvinyl carbonate-based polymer solid electrolyte, the structure of vinyl carbonate is as follows:

[0011]

[0012] In the preparation method of the polyvinyl carbonate-based polymer solid electrolyte, the isocyanate is one or more of the following: toluene-2,4-diisocyanate, toluene-2,5-diisocyanate, toluene-2,6-diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, p-phenylene diisocyanate, 1,3-phenylene diisocyanate, diphenylmethane diisocyanate, m-phenylenediisocyanate, L-lysine diisocyanate, cyclohexane-1,4-diisocyanate, trimethylhexane diisocyanate, dicyclohexylmethane 4,4'-diisocyanate, 2,2'-methylene diphenyl diisocyanate, 4,4'-methylenebis(phenyl isocyanate), triphenylmethane triisocyanate, and thiophosphoric acid triphenyl isocyanate.

[0013] The preparation method of the polyvinyl carbonate-based polymer solid electrolyte, the conductive salt is one or more of the following: lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium difluorooxalatoborate (LiDFOB), lithium tetrafluoroborate (LiBF4), sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium difluorooxalatoborate (NaDFOB), sodium bis(trifluoromethylsulfonyl)imide (NaTFSI).

[0014] In the preparation method of the polyvinyl carbonate-based polymer solid electrolyte, the chain carbonate plasticizer is one or more of the following: dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate; the initiator or catalyst is one or more of the following: lithium borohydride, lithium amide, lithium hydroxide, lithium tetramethoxyborate, lithium methoxide.

[0015] The application of the polyester-based polymer solid electrolyte in a solid-state battery comprises the following steps: taking a corresponding number of moles of ethylene carbonate, a conductive salt, a chain carbonate plasticizer and an initiator or a catalyst to prepare an electrolyte, and stirring it evenly; adding a corresponding number of moles of isocyanate and stirring it evenly to obtain a polymer solid electrolyte; the polymerization process is completed before assembling the battery, or is completed inside the assembled battery.

[0016] The application of the polyester-based polymer solid electrolyte in solid-state batteries, the positive electrode active material is divided into a lithium battery positive electrode active material or a sodium battery positive electrode active material, the lithium battery positive electrode active material is one or more of the following: lithium nickel cobalt manganese oxide (NCM), lithium ferrous phosphate (LiFePO4), lithium cobalt oxide (LiCoO2), lithium nickel manganese oxide (LNMO), lithium nickel cobalt aluminum oxide (NCA), lithium-rich materials (LLOs), lithium manganese oxide (LiMn2O4), lithium nickel oxide (LiNiO2), sulfur; the sodium battery positive electrode active material is one of the following or two or more: sodium vanadium phosphate (NVP), sodium vanadium fluorophosphate (NVPF), sodium nickel manganate (NNMO), sodium nickel iron manganate (NaNiFeMnO4), sodium Prussian blue, sulfur; the negative electrode active material is divided into lithium battery negative electrode active material or sodium battery negative electrode active material, the lithium battery negative electrode active material is one or more of the following: metallic lithium, metallic lithium alloy, silicon or silicon-carbon composite material, lithium titanate, graphite, tin dioxide, lithium metal nitride; the sodium battery negative electrode active material is one or more of the following: metallic sodium, metallic sodium alloy, graphite;

[0017] The preparation process of the positive electrode comprises the following steps: grinding and mixing 60-98% by mass of a positive electrode active material, 1-30% by mass of a conductive additive, and 1-30% by mass of a binder to prepare a positive electrode slurry with a solid content of 15-70wt%, coating the positive electrode slurry evenly on the surface of a metal foil, and then drying to obtain a positive electrode;

[0018] The negative electrode directly selects metallic lithium, metallic lithium alloy; metallic sodium, metallic sodium alloy; or uses a prepared negative electrode, and the preparation process of the negative electrode includes the following steps: grinding and mixing 60-90% by mass of negative electrode active material, 5-30% by mass of conductive agent Super P, and 5-30% by mass of polyvinylidene fluoride (PVDF) evenly, adding N-methylpyrrolidone (NMP) to prepare a negative electrode slurry with a solid content of 15-70wt%, evenly coating the negative electrode slurry on the surface of the metal foil, and then drying to obtain the negative electrode.

[0019] The application of the polyester-based polymer solid electrolyte in solid-state batteries, the preparation process of the solid-state battery includes one of the following two methods: (1) non-in-situ polymerization process: the polymer solid electrolyte precursor solution is soaked on the diaphragm or directly coated on the flat plate, and is allowed to stand at 0-60°C for 0-24 hours. After it is solidified, it is assembled with the positive electrode and the negative electrode into a solid-state battery; (2) in-situ polymerization process: the polymer solid electrolyte precursor solution is injected into the system of the positive electrode, the diaphragm, and the negative electrode, and after standing at 0-60°C for 0-24 hours, the precursor solution is solidified in the battery system to obtain a solid-state battery.

[0020] The innovation and practicality of the present invention are:

[0021] The present invention is the first to copolymerize ethylene carbonate, which is widely used in commercial batteries, with isocyanate, and mix with plasticizers and conductive salts to prepare polymer solid electrolytes. The use of ethylene carbonate and isocyanate copolymerization can break through the thermodynamic limitations of the traditional ethylene carbonate homopolymerization process, so that ethylene carbonate can be ring-opened polymerized without harsh reaction conditions such as high temperature, and there are no unnecessary by-products in the reaction process. The prepared polymer solid electrolyte has a wide electrochemical stability window (≥5.4V vs.Li + / Li), cation conductivity comparable to that of liquid electrolytes (>10 -3 S cm -1 ), a lithium ion migration number close to that of a single ion conductor (>0.8) and good thermal stability. At the same time, the lithium-ion battery assembled with this solid electrolyte can not only work stably for a long time at a high temperature of 60°C, but also provide excellent performance at a low temperature of -20°C. The assembled soft-pack solid-state lithium-ion battery shows excellent safety and flexibility and can be applied to other metal battery systems.

[0022] The advantages and beneficial effects of the present invention are:

[0023] 1. The present invention develops a polyvinyl carbonate-based polymer solid electrolyte, which is prepared by polymerization reaction of ethylene carbonate with one or more of isocyanate, conductive salt, chain carbonate plasticizer, initiator, and catalyst. The polymer solid electrolyte not only achieves high voltage tolerance to match the high voltage positive electrode for long-term stable operation, but also has strong cation transport capacity, and can operate stably for a long time in a wide temperature range of -20 to 60°C. In addition, the polymer solid electrolyte exhibits intrinsic non-flammability, and the solid-state battery assembled in lithium batteries or sodium batteries has excellent safety and flexibility.

[0024] 2. The present invention adopts an in-situ polymerization process to prepare solid electrolytes, eliminating the complex processes of polymer dissolution, film drying and electrolyte expansion in the preparation process of non-in-situ polymerization process, greatly reducing environmental pollution and safety hazards. It integrates the synthesis of polymer solid electrolytes and the battery assembly process, effectively reducing costs, and is compatible with the existing battery industrial system, with good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 .Optical photographs of electrolyte before and after polymerization.

[0026] Figure 2 .Electrochemical impedance spectrum of polymer solid electrolyte. In the figure, the horizontal axis Z′ is the real part of the impedance (Ω), and the vertical axis -Z″ is the imaginary part of the impedance (Ω).

[0027] Figure 3.Linear sweep voltammetry curve of polymer solid electrolyte. In the figure, the horizontal axis Voltage is the voltage (V), and the vertical axis Current is the current (mA).

[0028] Figure 4 .Electrochemical impedance spectrum (inset) of lithium-lithium symmetric battery assembled with polymer solid electrolyte and the current variation curve over time. In the electrochemical impedance spectrum, the horizontal axis Z′ is the real part of the impedance (Ω), the vertical axis -Z″ is the imaginary part of the impedance (Ω), Before polarization is before polarization, and After polarization is after polarization. In the current variation curve over time, the horizontal axis Time is time (s), and the vertical axis Current is the current (μA).

[0029] Figure 5 .Charge and discharge curves of nickel cobalt manganese oxide lithium battery assembled with polymer solid electrolyte at 25℃ and 1C charge and discharge conditions. In the figure, the horizontal axis Specific capacity is the specific capacity (mAh·g -1 ), the vertical axis Voltage is voltage (V).

[0030] Figure 6 .Charge and discharge curves of nickel manganese oxide lithium battery assembled with polymer solid electrolyte at 25℃ and 1C. In the figure, the horizontal axis Specific capacity is the specific capacity (mAh·g -1 ), the vertical axis Voltage is voltage (V). DETAILED DESCRIPTION

[0031] In the specific implementation process, the present invention proposes a preparation method and application of a polyvinyl carbonate-based polymer solid electrolyte. The solid electrolyte is prepared by in-situ polymerization inside a battery. Before polymerization, it includes vinyl carbonate, isocyanate, conductive salt, and chain carbonate plasticizer, and an initiator or catalyst is added to form a liquid mixture as a solid electrolyte precursor solution; the electrolyte is directly formed into a film to prepare a polyvinyl carbonate-based polymer electrolyte, or it is used as an electrolyte or additive to directly assemble a battery, and a polymerization reaction process is carried out when the assembled battery is standing to obtain a polyvinyl carbonate-based polymer solid electrolyte. Among them, the added amount of isocyanate is 0.04 to 1 (preferably 0.1 to 0.4) of the molar number of ethylene carbonate, the concentration of the conductive salt is 0.5 mol / L to 5 mol / L (preferably 1 mol / L to 2 mol / L), the added amount of the plasticizer is 0.2 to 1.5 (preferably 0.6 to 1.2) of the molar number of ethylene carbonate, and the added amount of the initiator or catalyst is 0.1 mmol / L to 1 mol / L (preferably 10 mmol / L to 50 mmol / L).

[0032] The present invention is further described in detail below through examples and drawings.

[0033] Example 1

[0034] In this embodiment, the preparation process of the polyester-based polymer solid electrolyte is as follows:

[0035] In a glove box filled with argon, 1 mg of lithium borohydride was dissolved in 1 ml of electrolyte (1 M molar concentration of LiPF6 in ethylene carbonate (EC): dimethyl carbonate (DMC) = 1:1 (volume ratio), multiple reagents), stirred at room temperature for 2 hours to allow the initiator to fully dissolve in the electrolyte, and then 200 μL of toluene-2,4-diisocyanate was added and stirred for 10 minutes to obtain a precursor solution. The precursor solution was allowed to stand at room temperature for 24 hours to obtain a polymer solid electrolyte.

[0036] like Figure 1 As shown, the precursor solution is a flowable liquid before polymerization, and solidifies into a solid with a certain strength and cannot flow after standing for 24 hours.

[0037] Example 2

[0038] In this embodiment, the preparation process of the polyester-based polymer solid electrolyte is as follows:

[0039] In a glove box filled with argon, 2 mg of lithium methoxide was dissolved in 1 ml of electrolyte (1M LiPF6 in EC:DMC=1:1 (volume ratio), Duoduo reagent), stirred at room temperature for 2 hours to allow the initiator to fully dissolve in the electrolyte, and then 60 μL of toluene-2,4-diisocyanate was added and stirred for 10 minutes to obtain a precursor solution. The precursor solution was allowed to stand at room temperature for 24 hours to obtain a polymer solid electrolyte.

[0040] Example 3

[0041] In this embodiment, the preparation process of the polyester-based polymer solid electrolyte is as follows:

[0042] In a glove box filled with argon, 4 mg of lithium amide was dissolved in 1 ml of electrolyte (1M LiPF6 inEC:DMC=1:1 (volume ratio), Duoduo reagent), stirred at room temperature for 2 hours to allow the initiator to fully dissolve in the electrolyte, and then 200 μL of hexamethylene diisocyanate was added and stirred for 10 minutes to obtain a precursor solution. The precursor solution was allowed to stand at room temperature for 24 hours to obtain a polymer solid electrolyte.

[0043] Example 4

[0044] In this embodiment, the preparation process of the polyester-based polymer solid electrolyte is as follows:

[0045] In a glove box filled with argon, 8 mg of lithium hydroxide was dissolved in 1 ml of electrolyte (1.5 M LiPF6 inEC:DMC = 2:1 (volume ratio), Duoduo reagent), stirred at room temperature for 2 hours to allow the initiator to fully dissolve in the electrolyte, and then 400 μL of toluene-2,4-diisocyanate was added and stirred for 10 minutes to obtain a precursor solution. The precursor solution was allowed to stand at room temperature for 24 hours to obtain a polymer solid electrolyte.

[0046] Example 5

[0047] In this embodiment, the preparation process of the polyester-based polymer solid electrolyte is as follows:

[0048] In a glove box filled with argon, 8 mg of lithium hydroxide was dissolved in 1 ml of electrolyte (1M LiTFSI inEC:DMC=2:1 (volume ratio), Duoduo reagent), stirred at room temperature for 2 hours to allow the initiator to fully dissolve in the electrolyte, and then 400 μL of isophorone diisocyanate was added and stirred for 10 minutes to obtain a precursor solution. The precursor solution was allowed to stand at room temperature for 24 hours to obtain a polymer solid electrolyte.

[0049] Example 6

[0050] In this embodiment, the preparation process of the solid-state battery using a polyester-based polymer solid electrolyte is as follows: the above-mentioned unpolymerized precursor solution is used to assemble SS / / SS, SS / / Li, and Li / / Li batteries to test the lithium ion conductivity, electrochemical stability window, and lithium ion migration number of the polymer solid electrolyte. The solid-state batteries are all button batteries, and the assembly process follows the positive electrode shell → positive electrode → 30μL electrolyte → diaphragm → 30μL electrolyte → negative electrode → gasket → shrapnel → negative electrode shell. The above preparation processes are all completed in a glove box filled with argon.

[0051] like Figure 2 As shown in the figure, the impedance of the stainless steel symmetrical battery of the polymer solid electrolyte in Example 1 is 4.3Ω at 25°C, and the ionic conductivity is 1.79×10 -3 S cm -1 .

[0052] like Figure 3 As shown, the electrochemical stability window of SS / / Li battery assembled with polymer solid electrolyte reaches 5.4V.

[0053] like Figure 4 As shown, the lithium ion transfer number of the Li / / Li battery assembled with polymer solid electrolyte is 0.92.

[0054] Example 7

[0055] In this embodiment, 240 mg of lithium nickel cobalt manganese oxide (NCM811), 30 mg of conductive agent Super P and 30 mg of binder polyvinylidene fluoride (PVDF) were uniformly ground for 50 min, 180 mg of N-methylpyrrolidone (NMP) was added and uniformly ground for 10 min to prepare a positive electrode slurry, which was evenly coated on the surface of aluminum foil and dried in a vacuum drying oven at 100° C. for 12 h; the dried positive electrode sheet was cut into discs with a diameter of 1 cm, and a solid-state lithium-ion battery was assembled using the polymer solid electrolyte and lithium metal negative electrode in Example 2.

[0056] like Figure 5 As shown in the figure, the charge and discharge curves of the nickel cobalt manganese oxide lithium battery assembled with polymer solid electrolyte under 25℃ and 1C charge and discharge conditions. Figure 5 It can be seen that the assembled nickel cobalt manganese oxide lithium solid-state battery has a 175.9 mAh g -1 High discharge specific capacity and Coulomb efficiency of 99.3%.

[0057] Example 8

[0058] In this embodiment, 270 mg of lithium nickel manganese oxide (LNMO), 15 mg of conductive agent Super P and 15 mg of binder polyvinylidene fluoride (PVDF) were uniformly ground for 50 min, 150 mg of N-methylpyrrolidone (NMP) was added and uniformly ground for 10 min to prepare a positive electrode slurry, which was evenly coated on the surface of aluminum foil and dried in a vacuum drying oven at 100° C. for 12 h; the dried positive electrode sheet was cut into discs with a diameter of 1 cm, and a solid-state lithium-ion battery was assembled using the polymer solid electrolyte and lithium metal negative electrode in Example 3.

[0059] like Figure 6 As shown in the figure, the charge and discharge curves of the nickel manganese oxide lithium battery assembled with polymer solid electrolyte under 25℃ and 1C charge and discharge conditions. Figure 6 It can be seen that the assembled nickel manganese oxide lithium solid-state battery can work normally at a high charging cut-off voltage of 4.95V, showing a charge capacity of 103.1mAhg -1 The discharge specific capacity and high coulombic efficiency of 99.4% are achieved.

[0060] The results show that the preparation process of the polymer solid electrolyte is simple and easy to control, the reaction conditions are mild, and the cost is low; the room temperature ionic conductivity is greater than 10 -3 S cm -1, electrochemical stability window ≥5.4V; good interfacial compatibility and long cycle performance with high-voltage positive electrodes and alkali metal negative electrodes; solid-state batteries can work stably for a long time in a wide temperature range of -20 to 60°C. At the same time, the solid electrolyte has the characteristics of intrinsic non-flammability, and the assembled battery has good safety. In addition, the polymer solid electrolyte has good flexibility and is also suitable for flexible battery devices for wearable electronic devices.

Claims

1. A method for preparing a polyvinyl carbonate-based polymer solid electrolyte, characterized in that: The polymer solid electrolyte is prepared by direct polymerization of a precursor solution, or the polymer solid electrolyte is prepared by in-situ polymerization of a precursor solution inside a battery. Before polymerization, it includes ethylene carbonate, isocyanate, conductive salt, and chain carbonate plasticizer, and an initiator or catalyst is added to form a liquid mixture as a polymer solid electrolyte precursor solution; a polymerization reaction process is carried out when standing to obtain a polyethylene carbonate-based polymer solid electrolyte.

2. The method for preparing a polyvinyl carbonate-based polymer solid electrolyte according to claim 1, characterized in that: The amount of isocyanate added is 0.04 to 1 of the mole of ethylene carbonate, the concentration of the conductive salt is 0.5 mol / L to 5 mol / L, the amount of the plasticizer added is 0.2 to 1.5 of the mole of ethylene carbonate, and the amount of the initiator or catalyst added is 0.1 mmol / L to 1 mol / L.

3. The method for preparing a polyvinyl carbonate-based polymer solid electrolyte according to claim 1, characterized in that: The structure of ethylene carbonate is as follows:

4. The method for preparing a polyvinyl carbonate-based polymer solid electrolyte according to claim 1, characterized in that: The isocyanate is one or more of the following: toluene-2,4-diisocyanate, toluene-2,5-diisocyanate, toluene-2,6-diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, p-phenylene diisocyanate, 1,3-phenylene diisocyanate, diphenylmethane diisocyanate, m-phenylenediisocyanate, L-lysine diisocyanate, cyclohexane-1,4-diisocyanate, trimethylhexane diisocyanate, dicyclohexylmethane 4,4'-diisocyanate, 2,2'-methylenediphenyl diisocyanate, 4,4'-methylenebis(phenyl isocyanate), triphenylmethane triisocyanate, and thiophosphoric acid triphenyl isocyanate.

5. The method for preparing a polyvinyl carbonate-based polymer solid electrolyte according to claim 1, characterized in that: The conductive salt is one or more of the following: lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethylsulfonyl imide) (LiTFSI), lithium bis(fluorosulfonyl imide) (LiFSI), lithium difluorooxalatoborate (LiDFOB), lithium tetrafluoroborate (LiBF4), sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium difluorooxalatoborate (NaDFOB), sodium bis(trifluoromethylsulfonyl imide) (NaTFSI).

6. The method for preparing a polyvinyl carbonate-based polymer solid electrolyte according to claim 1, characterized in that: The chain carbonate plasticizer is one or more of the following: dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate; the initiator or catalyst is one or more of the following: lithium borohydride, lithium amide, lithium hydroxide, lithium tetramethoxyborate, lithium methoxide.

7. Use of the polyester-based polymer solid electrolyte according to any one of claims 1 to 6 in a solid-state battery, characterized in that: The method comprises the following steps: taking corresponding molar numbers of ethylene carbonate, conductive salt, chain carbonate plasticizer and initiator or catalyst to prepare electrolyte, and stirring the electrolyte evenly; adding corresponding molar numbers of isocyanate and stirring the electrolyte evenly to obtain a polymer solid electrolyte; the polymerization process is completed before assembling the battery, or is completed inside the assembled battery.

8. The use of the polyester-based polymer solid electrolyte in a solid-state battery according to claim 7, characterized in that: The positive electrode active materials are divided into lithium battery positive electrode active materials or sodium battery positive electrode active materials. The lithium battery positive electrode active materials are one or more of the following: lithium nickel cobalt manganese oxide (NCM), lithium ferrous phosphate (LiFePO4), lithium cobalt oxide (LiCoO2), lithium nickel manganese oxide (LNMO), lithium nickel cobalt aluminum oxide (NCA), lithium-rich materials (LLOs), lithium manganese oxide (LiMn2O4), lithium nickel oxide (LiNiO2), sulfur; the sodium battery positive electrode active materials are one or more of the following: sodium vanadium phosphate (N VP), sodium vanadium fluorophosphate (NVPF), sodium nickel manganate (NNMO), sodium nickel iron manganate (NaNiFeMnO4), sodium Prussian blue, sulfur; negative electrode active materials are divided into lithium battery negative electrode active materials or sodium battery negative electrode active materials, lithium battery negative electrode active materials are one or more of the following: metallic lithium, metallic lithium alloy, silicon or silicon-carbon composite material, lithium titanate, graphite, tin dioxide, lithium metal nitride; sodium battery negative electrode active materials are one or more of the following: metallic sodium, metallic sodium alloy, graphite; Positive electrode preparation process The method comprises the following steps: grinding and mixing 60-98% by mass of a positive electrode active material, 1-30% by mass of a conductive additive, and 1-30% by mass of a binder to prepare a positive electrode slurry with a solid content of 15-70wt%, coating the positive electrode slurry evenly on the surface of a metal foil, and then drying to obtain a positive electrode; The negative electrode directly selects metallic lithium, metallic lithium alloy; metallic sodium, metallic sodium alloy; or uses a prepared negative electrode, and the preparation process of the negative electrode includes the following steps: grinding and mixing 60-90% by mass of negative electrode active material, 5-30% by mass of conductive agent Super P, and 5-30% by mass of polyvinylidene fluoride (PVDF) evenly, adding N-methylpyrrolidone (NMP) to prepare a negative electrode slurry with a solid content of 15-70wt%, evenly coating the negative electrode slurry on the surface of the metal foil, and then drying to obtain the negative electrode.

9. The use of the polyester-based polymer solid electrolyte in a solid-state battery according to claim 8, characterized in that: The preparation process of solid-state batteries includes one of the following two methods: (1) non-in-situ polymerization process: the polymer solid electrolyte precursor solution is soaked on the diaphragm or directly coated on the flat plate, and then allowed to stand at 0-60°C for 0-24 hours. After it solidifies, it is assembled with the positive electrode and the negative electrode into a solid-state battery; (2) in-situ polymerization process: the polymer solid electrolyte precursor solution is injected into the system of positive electrode, diaphragm and negative electrode, and after standing at 0-60°C for 0-24 hours, the precursor solution solidifies in the battery system to obtain a solid-state battery.

Citation Information

Patent Citations

  • Preparation and application of polycarbonate-based block polymer electrolyte

    CN110734517A

  • Carbonate-based polymer electrolyte with wide electrochemical window

    CN116111186A

  • Flame-retardant copolymer solid electrolyte as well as preparation method and application thereof

    CN118315658A