Electrolyte combination, secondary liquid injection method and lithium ion battery

Through the electrolyte combination and secondary injection method, the elastic SEI film is formed by using lithium difluorosulfonimide and fluorovinyl carbonate, which solves the problem of changes in the volume of silicon negative electrode and the side reaction of fluorovinyl carbonate in lithium-ion batteries. , improves battery capacity and cycle performance.

CN119009124AActive Publication Date: 2024-11-22REPT BATTERO ENERGY CO LTD +1

Patent Information

Application Number
CN202411098804.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The volume change of the silicon negative electrode in lithium-ion batteries during charging and discharging leads to damage to the electrode material and decomposition of the electrolyte. Fluorovinyl carbonate, as the SEI film additive, has problems such as battery gas production, positive electrode corrosion and insufficient interface stability.

Method used

A combination of electrolytes is adopted, including a first electrolyte and a second electrolyte. The first electrolyte is composed of lithium difluorosulfonimide, fluorovinyl carbonate and fluorogenic lithium salt additives. The second electrolyte contains inhibitors Gas-producing additives form elastic SEI films through synergistic action to improve interface stability and cycling performance.

Benefits of technology

It effectively suppresses gas production of the battery, reduces the dissolution of the positive electrode metal ions, improves the battery capacity and circulation performance, and enhances the interface stability of the positive and negative electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009124A_ABST
    Figure CN119009124A_ABST
Patent Text Reader

Abstract

The invention relates to an electrolyte composition, a secondary liquid injection method and a lithium ion battery. The electrode liquid combination is used for secondary liquid injection of the lithium ion battery and comprises a first electrolyte, the first electrolyte is used for primary liquid injection in the secondary liquid injection, the first electrolyte comprises a first lithium salt, a first solvent and a first additive, the first lithium salt is lithium bis (fluorosulfonyl) imide, the first solvent comprises fluoroethylene carbonate, and the first additive comprises a second lithium salt and a second solvent; the first additive comprises a fluorine-containing lithium salt additive and a positive electrode film-forming additive; and the second electrolyte is used for secondary liquid injection in the secondary liquid injection, the second electrolyte comprises a second lithium salt, a second solvent and a second additive, the second lithium salt is lithium hexafluorophosphate, and the second additive comprises a gas production inhibition additive. According to the electrolyte composition provided by the invention, gas production of the battery is inhibited, dissolution of positive electrode metal ions is inhibited, an elastic SEI film rich in LiF is formed, the interface stability is improved, and the capacity performance and the cycle performance of the battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of batteries, in particular to an electrolyte, a secondary liquid injection method and a lithium ion battery. Background Art

[0002] As the energy density of lithium-ion batteries continues to increase, the application of high-capacity silicon-based negative electrodes has become increasingly common. However, during the charge and discharge process, the silicon negative electrode undergoes a huge volume change, causing damage to the electrode material and decomposition of the electrolyte, thereby reducing its electrochemical performance; in addition, silicon is a semiconductor with low electrical conductivity. Among them, the irreversible capacity loss of the silicon negative electrode is mainly due to the film consumption of the SEI film and the "lithium consumption" of silicon (forming Li5Si4 crystals).

[0003] At present, fluoroethylene carbonate, as an important negative electrode film-forming additive for silicon system, forms a LiF-containing SEI film on the surface of silicon particles, thereby inhibiting the "lithium eating" phenomenon.

[0004] However, fluoroethylene carbonate has the following problems as a negative electrode film-forming additive: (1) Based on the demand for high capacity, the silicon content needs to be increased, thereby increasing the content of FEC or DFEC. However, a high content of fluoroethylene carbonate will aggravate the gas production problem of the battery and also cause the battery cycle life to decay; (2) At high temperatures, fluoroethylene carbonate is easily decomposed to produce HF, which corrodes the positive electrode and causes the dissolution of positive electrode metal ions, resulting in a decrease in battery capacity and cycle performance; (3) The SEI film formed solely by fluoroethylene carbonate is rich in a certain amount of Li2CO3 and rigid polyolefins, and cannot maintain good interface stability during the lithium insertion and extraction process of the silicon negative electrode. Summary of the invention

[0005] Based on this, it is necessary to provide an electrolyte combination, a secondary injection method and a lithium-ion battery to inhibit battery gas production, reduce the side reaction of fluoroethylene carbonate with the positive electrode, inhibit the dissolution of positive electrode metal ions, inhibit the "lithium eating" phenomenon, form an elastic SEI film, improve interface stability, and improve the capacity performance and cycle performance of the battery.

[0006] The first aspect of the present application provides an electrolyte combination, which is used for secondary injection of a lithium-ion battery, and the electrolyte combination includes: a first electrolyte, the first electrolyte is used for the first injection in the secondary injection, the first electrolyte includes a first lithium salt, a first solvent and a first additive, the first lithium salt is lithium bis(fluorosulfonyl)imide, the first solvent includes fluoroethylene carbonate, and the first additive includes a fluorine-containing lithium salt additive and a positive electrode film-forming additive; a second electrolyte, the second electrolyte is used for the second injection in the secondary injection, the second electrolyte includes a second lithium salt, a second solvent and a second additive, the second lithium salt is lithium hexafluorophosphate, and the second additive includes a gas production inhibitor.

[0007] In some embodiments, the mass percentage of fluoroethylene carbonate in the first electrolyte is 18% to 45%; and / or the second additive further includes fluoroethylene carbonate, and the mass percentage of fluoroethylene carbonate in the second electrolyte is 0.01% to 5%.

[0008] In some embodiments, the mass percentage of lithium bis(fluorosulfonyl)imide in the first electrolyte is 3% to 7%.

[0009] In some embodiments, the mass percentage of the fluorine-containing lithium salt additive in the first electrolyte is 1% to 3%.

[0010] In some embodiments, the mass percentage of the gas generation inhibiting additive in the second electrolyte is 0.1% to 1%.

[0011] In some embodiments, a lithium-ion battery includes a negative electrode, the negative electrode includes a current collector and a negative electrode coating, the negative electrode coating includes a silicon-containing material, and the mass percentage a% of fluoroethylene carbonate in the electrolyte combination and the mass percentage x% of the silicon-containing material in the negative electrode satisfy: 0.5≤a / x≤0.7.

[0012] In some embodiments, the mass percentage of the first electrolyte in the electrolyte combination is 20% to 40%; and / or the mass percentage of the second electrolyte in the electrolyte combination is 60% to 80%.

[0013] The second aspect of the present application provides a secondary liquid injection method, which uses the electrolyte combination provided by the first aspect to perform secondary liquid injection on a lithium-ion battery. The secondary liquid injection method includes the following steps: using a first electrolyte to perform a first liquid injection on the lithium-ion battery in the secondary liquid injection; sequentially allowing the lithium-ion battery after the first liquid injection to stand and form; using a second electrolyte to perform a second liquid injection on the formed lithium-ion battery in the secondary liquid injection; and sequentially aging and capacity separation of the lithium-ion battery after the second liquid injection.

[0014] In some embodiments, the formation includes multiple formation stages, and the current density of a subsequent formation stage is less than the current density of a previous formation stage.

[0015] The third aspect of the present application provides a lithium-ion battery, which includes the electrolyte combination provided by the first aspect above; or, the lithium-ion battery is prepared by the secondary injection method provided by the second aspect above.

[0016] Compared with the traditional technology, this application has at least the following beneficial effects:

[0017] The electrolyte combination provided in the present application, the first electrolyte is used for the first injection, and the synergistic effect of lithium bis(fluorosulfonyl)imide, fluoroethylene carbonate and fluorine-containing lithium salt additive promotes the formation of an elastic, high-LiF-rich, low-impedance SEI film, thereby improving the battery charge and discharge performance and cycle performance. The lithium bis(fluorosulfonyl)imide salt in the first electrolyte can not only improve the stability of the electrolyte itself, but also the large anion FSI in the lithium bis(fluorosulfonyl)imide can improve the stability of the electrolyte. - The reducibility is good, which is also conducive to promoting the formation of LiF in the SEI film; the fluorine-containing lithium salt additive itself is easily reduced at the positive and negative electrodes to form an interface film rich in LiF components, inhibiting the "lithium eating" phenomenon and improving the cycle performance of the battery; the fluorine-containing lithium salt additive induces direct defluorination of fluoroethylene carbonate, increases the content of LiF in the formed SEI film, inhibits the "lithium eating" phenomenon, and direct defluorination maintains the ring structure of fluoroethylene carbonate, prompting the defluorinated fluoroethylene carbonate to be easily polymerized to form polyvinylene carbonate, thereby improving the elasticity of the formed SEI film, thereby improving the interface stability and the cycle stability of the battery.

[0018] In addition, the second electrolyte is used for the second injection. The gas production inhibitor additive in the second electrolyte reacts with the surface of the positive and negative electrodes at high temperature, repairs the interface film, ensures the interface stability of the positive and negative electrodes, inhibits battery gas production, and improves the battery's capacity performance and cycle performance.

[0019] In summary, the use of the electrolyte combination of the present application for secondary injection of lithium-ion batteries improves the interface stability of the positive and negative electrodes of the battery, and takes into account the capacity performance and cycle performance of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a flow chart of a secondary liquid injection method in one embodiment of the present application. DETAILED DESCRIPTION

[0021] References to embodiments of the present application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.

[0022] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.

[0023] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0024] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0025] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0026] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0027] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, it is mentioned that the method may also include step (c), which means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0028] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0029] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0030] The first aspect of the present application provides an electrolyte combination, which is used for the secondary injection of a lithium-ion battery, and the electrolyte combination includes a first electrolyte and a second electrolyte. The first electrolyte is used for the first injection, and the first electrolyte includes a first lithium salt, a first solvent, and a first additive. The first lithium salt is lithium bis(fluorosulfonyl)imide, the first solvent includes fluoroethylene carbonate, and the first additive includes a fluorine-containing lithium salt additive and a positive electrode film-forming additive. The second electrolyte is used for the second injection, and the second electrolyte includes a second lithium salt, a second solvent, and a second additive. The second lithium salt is lithium hexafluorophosphate, and the second additive includes a gas production inhibitor.

[0031] The electrolyte combination provided in the present application, the first electrolyte is used for the first injection, through the synergistic effect of lithium bis(fluorosulfonyl)imide, fluoroethylene carbonate and fluorine-containing lithium salt additive, the lithium bis(fluorosulfonyl)imide in the first electrolyte can not only improve the stability of the electrolyte itself, but also the large anion FSI in the lithium bis(fluorosulfonyl)imide can be used to improve the stability of the electrolyte. - The reducibility is good, which is also conducive to promoting the formation of LiF in the SEI film; the fluorine-containing lithium salt additive itself is easily reduced at the positive and negative electrodes to form an interface film rich in LiF components, inhibiting the "lithium eating" phenomenon and improving the cycle performance of the battery; the fluorine-containing lithium salt additive induces direct defluorination of fluoroethylene carbonate, increases the content of LiF in the formed SEI film, inhibits the "lithium eating" phenomenon, and direct defluorination maintains the ring structure of fluoroethylene carbonate, prompting the defluorinated fluoroethylene carbonate to be easily polymerized to form polyvinylene carbonate, thereby improving the elasticity of the formed SEI film, thereby improving the interface stability and the cycle stability of the battery.

[0032] In addition, the second electrolyte is used for the second injection. The gas production inhibitor additive in the second electrolyte reacts with the surface of the positive and negative electrodes at high temperature, repairs the interface film, ensures the interface stability of the positive and negative electrodes, inhibits battery gas production, and improves the battery's capacity performance and cycle performance.

[0033] In summary, the use of the electrolyte combination of the present application for secondary injection of lithium-ion batteries improves the interface stability of the positive and negative electrodes of the battery, and takes into account the capacity performance and cycle performance of the lithium-ion battery.

[0034] It is understood that the selection of the first lithium salt and the second lithium salt is based on the following reasons:

[0035] (1) The first lithium salt of the first electrolyte is not LiPF6 but LiFSI.

[0036] PF6 -Although LiF can be generated by hydrolysis, the SEI film formed is small in quantity and grows unevenly. In addition, the fluoroethylene carbonate-based electrolyte will interact with the strong Lewis acid PF5 produced by the decomposition of LiPF6 under high temperature conditions, and then undergo a defluorination reaction to generate acidic products such as VC and HF, resulting in increased acidity of the electrolyte and corrosion of the positive electrode.

[0037] LiFSI due to FSI - The delocalized charge of ethylene carbonate is easily soluble in bipolar aprotic solvents (i.e., fluoroethylene carbonate), and can cooperate with fluoroethylene carbonate, which is more conducive to the formation of high-content LiF and uniformly grown SEI films during electrochemical reduction.

[0038] (2) LiFSI is not selected as the second lithium salt of the second electrolyte in order to allow LiFSI to fully participate in the film formation while minimizing the residue, thereby avoiding excessive LiFSI residue in the electrolyte during battery cycling and storage, leading to high-temperature gas production at the positive electrode and corrosion of the current collector.

[0039] In some embodiments, the fluoroethylene carbonate includes one or more of monofluoroethylene carbonate (FEC) and bisfluoroethylene carbonate (DFEC).

[0040] In some embodiments, the mass percentage of fluoroethylene carbonate in the first electrolyte is 18% to 45%, including but not limited to 18%, 20%, 25%, 30%, 35%, 40%, and 45%. Within the above mass percentage range, a high content of fluoroethylene carbonate is used in the first injection of the electrolyte, which can form a LiF-rich SEI film on the surface of silicon particles, inhibit the formation of Li5Si4, reduce silicon expansion and consumption of lithium ions, and the introduction of a high content of fluoroethylene carbonate during the first injection can reduce the addition of fluoroethylene carbonate in the second injection, reducing the high temperature deterioration caused by fluoroethylene carbonate.

[0041] In some embodiments, the first solvent also includes a linear carbonate, and the mass ratio of fluoroethylene carbonate and linear carbonate in the first solvent is 1:1 to 1:5, including but not limited to 1:1, 2:3, 3:7, 1:3, 1:4, 1:5. Within the above mass ratio range, the combination of fluoroethylene carbonate and linear carbonate is conducive to optimizing the formation of SEI film and improving the stability and elasticity of SEI film. A higher proportion of fluoroethylene carbonate ensures the formation of LiF-rich SEI film, thereby inhibiting the "lithium eating" phenomenon of silicon negative electrode and extending the cycle life of the battery. The addition of linear carbonate improves the stability of the electrolyte, and can reduce viscosity and improve electrolyte conductivity.

[0042] In some embodiments, the linear carbonate includes one or more of ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), propyl propionate (PP) and ethyl propionate (EP).

[0043] Furthermore, the mass percentage of lithium bis(fluorosulfonyl)imide in the first electrolyte is 3% to 7%, including but not limited to 3%, 4%, 5%, 6%, and 7%. Within the above mass percentage range, the content of LiFSI in the first electrolyte is relatively small. On the one hand, after the first injection, a small amount of LiFSI directly participates in the formation of the film, improving the low temperature and cycle performance of the battery. At the same time, an appropriate amount of LiFSI can reduce the high temperature gas production and current collector corrosion caused by excessive residual LiFSI in the battery cycle and electrolyte; on the other hand, the low content of LiFSI can effectively improve the infiltration. At the same time, the low concentration of the first lithium salt LiFSI can induce a high overpotential in the low current formation process, which is conducive to the formation of inorganic components such as LiF in the SEI layer formed by the highly fluorinated electrolyte.

[0044] In some embodiments, the fluorine-containing lithium salt additive includes one or more of lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium trifluoromethanesulfonate (LiFSA), lithium difluorooxalatoborate (LiODFB), lithium difluorodioxalatophosphate (LiODFP) and lithium tetrafluorooxalatoborate (LiOTFP).

[0045] In some embodiments, the mass percentage of the fluorine-containing lithium salt additive in the first electrolyte is 1% to 3%, including but not limited to 1%, 1.5%, 2%, 2.5%, and 3%. Within the above mass percentage range, it is beneficial for the fluorine-containing lithium salt additive to induce direct defluorination of fluoroethylene carbonate to form an inorganic elastic SEI film; if the content of the fluorine-containing lithium salt additive is too high, it will remain in the battery after capacity division, and the fluorine-containing lithium salt additive is unstable and easily reacts with the negative electrode to produce gas, affecting the electrochemical performance.

[0046] In some embodiments, the second electrolyte does not contain fluorine-containing lithium salt additives. If the second electrolyte also contains fluorine-containing lithium salt additives, the fluorine-containing lithium salt additives are highly reactive in the electrolyte and easily react and produce gas at high temperatures, which will lead to deterioration of high temperature performance.

[0047] In some embodiments, the second electrolyte further includes fluoroethylene carbonate, and the mass percentage of fluoroethylene carbonate in the second electrolyte is 0.01% to 5%, including but not limited to 0.01%, 0.5%, 1%, 2%, 3%, 4%, and 5%. Within the above mass percentage range, an appropriate amount of fluoroethylene carbonate is beneficial to repairing the SEI film in the later stage of battery cycling, while reducing gas production and side reactions, and improving the cycle performance and capacity performance of the battery.

[0048] In some embodiments, the gas generation suppressing additive includes one or more of vinyl sulfate (DTD), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), vinyl sulfite (ES), methylene methanedisulfonate (MMDS), 1,3-propane sultone (PS), propenyl-1,3-sultone (PST), tetravinylsilane (TVSI) and tripropynyl phosphate (TPP).

[0049] In some embodiments, the mass percentage of the gas production inhibitor additive in the second electrolyte is 0.1% to 1%, including but not limited to 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%. Within the above mass percentage range, it is beneficial to inhibit gas production and reduce battery impedance. If too much gas production inhibitor additive is added, it will gradually participate in film formation during the use of the battery, which will increase the battery impedance, deteriorate the battery dynamics, and be detrimental to the battery charge and discharge performance and cycle performance.

[0050] It is understandable that the gas generation inhibitor is added to the second electrolyte, but not to the first electrolyte. The gas generation inhibitor has a large impedance after film formation, so as not to make the initial impedance of the battery too large and affect the battery rate performance.

[0051] In some embodiments, the second solvent includes cyclic carbonate and linear carbonate. Cyclic carbonate includes one or more of ethylene carbonate (EC) and propylene carbonate (PC); linear carbonate includes one or more of ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), propyl propionate (PP) and ethyl propionate (EP). The use of cyclic carbonate and linear carbonate together is conducive to promoting the full dissolution of the second lithium salt and the second additive, promoting the role of each component in the electrolyte, and improving the improvement effect of the electrolyte on battery performance.

[0052] In some embodiments, the second lithium salt includes one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium difluorooxalatoborate, and lithium bis(trifluoromethanesulfonyl)imide.

[0053] In some embodiments, the mass percentage of the second lithium salt in the second electrolyte is 13% to 18%.

[0054] In some embodiments, the mass percentage of the first electrolyte in the electrolyte combination is 20% to 40%, including but not limited to 20%, 25%, 30%, 35%, and 40%. Controlling the proportion of the first electrolyte in the electrolyte combination within the above range is conducive to forming a good SEI film in the early stage and stabilizing the positive and negative electrode interfaces.

[0055] In some embodiments, the mass percentage of the second electrolyte in the electrolyte combination is 60% to 80%, including but not limited to 60%, 65%, 70%, 75%, and 80%. Controlling the proportion of the second electrolyte in the electrolyte combination within the above range is conducive to continuing to optimize the SEI film in the later stage of the battery cycle and improving the long cycle performance and capacity performance of the battery.

[0056] In some embodiments, the lithium-ion battery includes a negative electrode, the negative electrode includes a current collector and a negative electrode coating, the negative electrode coating includes a silicon-containing material, and the mass percentage a% of fluoroethylene carbonate in the electrolyte composition and the mass percentage x% of the silicon-containing material in the negative electrode satisfy: 0.5≤a / x≤0.7. Within the above ratio range, the amount of fluoroethylene carbonate matches the content of silicon in the negative electrode, so that the formed SEI film can better inhibit the "lithium consumption" phenomenon.

[0057] In some embodiments, the silicon-containing material includes one or more of a silicon-carbon material, a silicon-oxygen material, and a pre-lithiation silicon material.

[0058] The second aspect of the present application provides a secondary injection method, such as Figure 1 As shown, the secondary injection method uses the electrolyte combination provided in the first aspect to perform secondary injection on the lithium-ion battery, and the secondary injection method comprises the following steps:

[0059] S1. Filling the lithium-ion battery with the first electrolyte for the first time.

[0060] S2. After the first injection, the lithium-ion battery is left to stand and formed in sequence.

[0061] S3, using the second electrolyte to inject the formed lithium-ion battery for the second time.

[0062] S4. The lithium-ion batteries after the second injection are aged and divided in turn.

[0063] In some embodiments, the formation includes multiple formation stages, and the current density of a subsequent formation stage is smaller than the current density of a previous formation stage.

[0064] The liquid injection formation method of the present application first adopts a high overpotential formation method, through the potential difference generated by uneven infiltration and the high polarization generated by large current, the interface is synergistically induced to generate a high overpotential, promoting the large growth of inorganic LiF in the SEI film, and then further through a small current formation method, a uniform and stable inorganic and organic alternating SEI film is formed. The SEI film formed by this method contains a large number of large particles of LiF, and the inner layer is loose and porous, which is conducive to lithium ion transmission.

[0065] The third aspect of the present application provides a lithium-ion battery, which includes the electrolyte combination provided by the first aspect above; or, the lithium-ion battery is prepared by the secondary injection method provided by the second aspect above.

[0066] In some embodiments, the lithium-ion battery further includes a positive electrode sheet and a negative electrode sheet.

[0067] The present application will be further described below with reference to specific embodiments and comparative examples.

[0068] Example 1

[0069] This embodiment provides a secondary liquid injection method for a lithium ion battery, the method comprising the following steps:

[0070] S1. Filling the lithium-ion battery with the first electrolyte for the first time.

[0071] The first electrolyte includes a first lithium salt, a first solvent and a first additive; based on the mass of the first electrolyte being 100%, the first lithium salt is 5wt% of LiFSI; the first solvent is 23.0wt% of FEC and 69.5wt% of EMC, and the mass ratio of FEC to EMC is 1:3; the first additive includes 1wt% of LiPO2F2, 1.0wt% of LiODFB and 0.5wt% of TMSP. The mass percentage of the first electrolyte in the electrolyte combination for secondary injection of lithium-ion batteries is 30%.

[0072] S2. After the first injection, the lithium-ion battery is left to stand at 45°C for 24 hours, then charged to 3.0V at 0.5C, charged to 3.4V at 0.2C, and then charged to 3.75V at 0.05C.

[0073] S3, using the second electrolyte to inject the formed lithium-ion battery for the second time.

[0074] The second electrolyte includes a second lithium salt, a second solvent and a second additive; based on the mass of the second electrolyte being 100%, the second lithium salt is 15wt% of LiPF6; the second additive is 3.0wt% of FEC and 0.5wt% of VEC; the remainder is the second solvent, which is a mixed solvent of EC and EMC, and the volume ratio of EC to EMC is 3:7. The mass percentage of the second electrolyte in the electrolyte combination for secondary injection of lithium-ion batteries is 70%.

[0075] S4. The lithium-ion batteries after the second injection are aged and divided in turn.

[0076] Lithium-ion battery:

[0077] Prepared by the above-mentioned secondary liquid injection method, it includes a positive electrode sheet, a negative electrode sheet and an electrolyte combination injected by the above-mentioned secondary liquid injection method, wherein the mass percentage a% of FEC in the electrolyte combination and the mass percentage x% of the silicon-containing material in the negative electrode satisfy: a / x=0.6 (x%=15%).

[0078] The positive electrode sheet is prepared by the following preparation method:

[0079] Based on the total mass of the positive electrode material being 100 wt.%, the positive electrode material comprises 97.5 wt.% of LiNi 90 Co 5.5 Mn 3.5 Al1O2 positive electrode active material, 1.5wt.% Super P conductive agent and 1.0wt.% polyvinylidene fluoride binder; the above components are mixed, and then N-methylpyrrolidone solvent is added to mix evenly to obtain positive electrode slurry, the positive electrode slurry is coated on the surface of carbon-coated aluminum foil, and after drying, the positive electrode sheet is obtained by slicing;

[0080] The negative electrode sheet is prepared by the following preparation method:

[0081] Graphite, silicon-carbon composite material (purchased from Lanxi Zhide New Energy Materials Co., Ltd., model S0310), single-walled carbon nanotubes, Super P conductive agent, polyacrylic acid and styrene-butadiene latex are mixed in a mass ratio of 80.1:15:0.1:0.6:3.3:0.9, and then deionized water is added and stirred evenly to obtain a negative electrode slurry. The negative electrode slurry is coated on the surface of copper foil, and after drying, the negative electrode sheet is obtained by slicing.

[0082] Example 2

[0083] The secondary injection method and lithium ion battery of this embodiment are basically the same as those of embodiment 1, except that:

[0084] In step S1, the mass percentage of the first electrolyte in the electrolyte combination for secondary injection of lithium-ion batteries is 40%, and the mass percentage of FEC in the first electrolyte is 18wt%.

[0085] In step S3, the mass percentage of the second electrolyte in the electrolyte combination for secondary injection of lithium-ion batteries is 60%, and the mass percentage of FEC in the second electrolyte is 3wt%.

[0086] The mass percentage a% of FEC in the electrolyte composition and the mass percentage x% of the silicon-containing material in the negative electrode satisfy: a / x=0.6 (x%=15%).

[0087] Example 3

[0088] The secondary injection method and lithium ion battery of this embodiment are basically the same as those of embodiment 1, except that:

[0089] In step S1, the mass percentage of FEC in the first electrolyte is 18 wt %.

[0090] In step S3, the mass percentage of FEC in the second electrolyte is 3 wt %.

[0091] The mass percentage a% of FEC in the electrolyte composition and the mass percentage x% of the silicon-containing material in the negative electrode satisfy: a / x=0.5 (x%=15%).

[0092] Example 4

[0093] The secondary injection method and lithium ion battery of this embodiment are basically the same as those of embodiment 1, except that:

[0094] In step S1, the mass percentage of FEC in the first electrolyte is 40.5wt%, and the mass percentage of the first electrolyte in the electrolyte combination for secondary injection of lithium-ion batteries is 20%.

[0095] In step S3, the mass percentage of FEC in the second electrolyte is 3wt%, and the mass percentage of the second electrolyte in the electrolyte combination for secondary injection of lithium-ion batteries is 80%.

[0096] The mass percentage a% of FEC in the electrolyte composition and the mass percentage x% of the silicon-containing material in the negative electrode satisfy: a / x=0.7 (x%=15%).

[0097] Example 5

[0098] The secondary injection method and lithium ion battery of this embodiment are basically the same as those of embodiment 1, except that:

[0099] In step S1, the mass percentage of LiFSI in the first electrolyte is 3 wt%, and the mass percentage of EMC in the first electrolyte is 71.5 wt%.

[0100] Example 6

[0101] The secondary injection method and lithium ion battery of this embodiment are basically the same as those of embodiment 1, except that:

[0102] In step S1, the mass percentage of LiFSI in the first electrolyte is 7wt%, and the mass percentage of EMC in the first electrolyte is 67.5wt%.

[0103] Example 7

[0104] The secondary liquid injection method and the lithium ion battery in this embodiment are substantially the same as those in Embodiment 1, except that:

[0105] In step S1, the fluorine-containing lithium salt additives LiPO2F2 and LiODFB are replaced with 2.0 wt% of LiFSA.

[0106] Example 8

[0107] The secondary liquid injection method and the lithium ion battery in this embodiment are substantially the same as those in Embodiment 1, except that:

[0108] In step S1, the mass percentage of the first electrolyte in the electrolyte combination for secondary injection of the lithium-ion battery is 60%.

[0109] In step S3, the mass percentage of the second electrolyte in the electrolyte combination for secondary injection of the lithium-ion battery is 40%.

[0110] Example 9

[0111] The secondary injection method and lithium ion battery of this embodiment are basically the same as those of embodiment 1, except that:

[0112] In step S1, the mass percentage of the first electrolyte in the electrolyte combination for secondary injection of the lithium-ion battery is 10%.

[0113] In step S3, the mass percentage of the second electrolyte in the electrolyte combination for secondary injection of the lithium-ion battery is 90%.

[0114] Example 10

[0115] The secondary liquid injection method and the lithium ion battery in this embodiment are substantially the same as those in Embodiment 1, except that:

[0116] In step S1, the mass percentage of LiFSI in the first electrolyte is 12%, and the mass percentage of EMC in the first electrolyte is 62.5wt%.

[0117] Embodiment 11

[0118] The secondary liquid injection method and the lithium ion battery in this embodiment are substantially the same as those in Embodiment 1, except that:

[0119] In step S2, the voltage is set to 3.0V at 0.05C, then to 3.4V at 0.2C, and then to 3.75V at 0.5C.

[0120] Example 12

[0121] The secondary liquid injection method and the lithium ion battery in this embodiment are substantially the same as those in Embodiment 1, except that:

[0122] In step S3, the second electrolyte further includes 1 wt% of LiPO2F2 and 0.5 wt% of LiODFB.

[0123] Comparative Example 1

[0124] The secondary injection method and lithium ion battery of this comparative example are substantially the same as those of Example 1, except that:

[0125] In step S1, the first solvent does not include FEC, and the mass percentage of EMC in the first electrolyte is 92.7%.

[0126] Comparative Example 2

[0127] The secondary injection method and lithium ion battery of this comparative example are substantially the same as those of Example 1, except that:

[0128] In step S1, the first additive does not include LiPO2F2 and LiODFB, and the mass percentage of EMC in the first electrolyte is 71.5%.

[0129] Comparative Example 3

[0130] The secondary injection method and lithium ion battery of this comparative example are substantially the same as those of Example 1, except that:

[0131] In step S1, the first lithium salt is replaced by LiPF6.

[0132] Comparative Example 4

[0133] The secondary injection method and lithium ion battery of this comparative example are substantially the same as those of Example 1, except that:

[0134] In step S3, the second lithium salt is replaced with LiFSI.

[0135] Comparative Example 5

[0136] The secondary injection method and lithium ion battery of this comparative example are substantially the same as those of Example 1, except that:

[0137] In step S3, the second additive does not include VEC.

[0138] Performance Testing

[0139] (1) Discharge specific capacity test

[0140] The lithium ion batteries in the examples and comparative examples were tested for capacity, left to stand for 1 min, and discharged at a current of 0.1 C until the cut-off voltage was 2.5 V, and the first discharge capacity was recorded. The results are shown in Table 1 below.

[0141] (2) High temperature cycle performance test

[0142] The lithium-ion batteries in the embodiments and comparative examples were placed in a 45°C constant temperature box, charged to 4.2V at a constant current of 1C, charged to 0.05C at a constant voltage at 4.2V, and then discharged to 2.5V at a constant current of 1C. This was recorded as a charge and discharge cycle, and the initial discharge capacity was recorded; capacity retention rate = (remaining discharge capacity / initial discharge capacity) × 100%, and the number of cycles when the capacity retention rate of the secondary battery was 80% was recorded.

[0143] (3) High temperature storage performance:

[0144] The lithium ion batteries in the embodiment and the comparative example were charged to 4.2V at a constant current of 1C at 25°C, charged to 0.05C at a constant voltage at 4.2V, and then discharged to 2.5V at a constant current of 1C. This was recorded as a charge and discharge cycle process, and the initial discharge capacity C0 was recorded. After being fully charged again, the secondary battery was placed in a 60°C oven. After storage for 30 days, the secondary battery was left at room temperature for 2h and discharged to 2.5V at 1C. The remaining discharge capacity of the battery at this time was recorded and the final battery capacity retention rate was calculated. Battery capacity retention rate = (remaining discharge capacity / initial discharge capacity) × 100%;

[0145] (4) Gas production after high temperature storage:

[0146] Volume test method for lithium-ion batteries: Place a beaker filled with deionized water on an electronic balance, record the reading m1 of the electronic balance at this time, fix the lithium-ion battery in mid-air with the clamp of the iron stand, and slowly immerse it in the beaker filled with deionized water until the lithium-ion battery is completely immersed in the deionized water, record the reading m2 of the electronic balance at this time, according to the formula mg = ρ H2O VP, the battery volume V=(m2-m1)×g / (ρ H2O ×P). H2O is the density of deionized water, g is the gravity coefficient, P is one standard atmospheric pressure, and V is the volume of the secondary battery;

[0147] The volume test method is used to calculate the battery volume V1 of the secondary battery before high-temperature storage, and then the volume V2 of the secondary battery after high-temperature storage is calculated. The gas production of the battery after high-temperature storage = V2-V1;

[0148] The method of high temperature storage is the same as above (3).

[0149] Table 1

[0150]

[0151]

[0152] As shown in Table 1, by comparing Examples 1 to 12 and Comparative Examples 1 to 5, it can be seen that the electrolyte combination, secondary injection method and lithium-ion battery of the present application ensure the capacity performance while improving the high-temperature cycle performance and high-temperature storage performance of the battery and reducing the gas production of the battery.

[0153] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0154] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the technical concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. An electrolyte combination, characterized in that: For secondary injection of lithium-ion batteries, the electrolyte combination comprises: A first electrolyte, wherein the first electrolyte is used for the first injection in the secondary injection, the first electrolyte comprises a first lithium salt, a first solvent and a first additive, the first lithium salt is lithium bis(fluorosulfonyl)imide, the first solvent comprises fluoroethylene carbonate, and the first additive comprises a fluorine-containing lithium salt additive and a positive electrode film-forming additive; The second electrolyte is used for the second injection in the secondary injection, the second electrolyte comprises a second lithium salt, a second solvent and a second additive, the second lithium salt is lithium hexafluorophosphate, and the second additive comprises a gas generation inhibiting additive.

2. The electrolyte combination according to claim 1, characterized in that: The mass percentage of the fluoroethylene carbonate in the first electrolyte is 18% to 45%; and / or, The second additive further includes fluoroethylene carbonate, and the mass percentage of the fluoroethylene carbonate in the second electrolyte is 0.01% to 5%.

3. The electrolyte combination according to claim 1, characterized in that: The mass percentage of the lithium bis(fluorosulfonyl)imide in the first electrolyte is 3% to 7%.

4. The electrolyte combination according to claim 1, characterized in that: The mass percentage of the fluorine-containing lithium salt additive in the first electrolyte is 1% to 3%.

5. The electrolyte combination according to claim 1, characterized in that: The mass percentage of the gas generation inhibiting additive in the second electrolyte is 0.1% to 1%.

6. The electrolyte combination according to any one of claims 1 to 5, characterized in that: The lithium-ion battery includes a negative electrode, the negative electrode includes a current collector and a negative electrode coating, the negative electrode coating includes a silicon-containing material, and the mass percentage a% of the fluoroethylene carbonate in the electrolyte combination and the mass percentage x% of the silicon-containing material in the negative electrode coating satisfy: 0.5≤a / x≤0.

7.

7. The electrolyte combination according to any one of claims 1 to 5, characterized in that: The mass percentage of the first electrolyte in the electrolyte combination is 20% to 40%; and / or, The mass percentage of the second electrolyte in the electrolyte combination is 60% to 80%.

8. A secondary liquid injection method, characterized in that: A lithium-ion battery is subjected to secondary injection using the electrolyte combination according to any one of claims 1 to 7, wherein the secondary injection method comprises the following steps: Using the first electrolyte to inject the lithium ion battery for the first time; The lithium-ion battery after the first injection is sequentially left to stand and formed; Using the second electrolyte to inject the formed lithium-ion battery for a second time; The lithium-ion battery after the second injection is aged and divided in order.

9. The secondary liquid injection method according to claim 8, characterized in that: The formation includes multiple formation stages, and the current density of a later formation stage is smaller than the current density of a previous formation stage.

10. A lithium ion battery, characterized in that: comprising the electrolyte combination according to any one of claims 1 to 7; or, The lithium-ion battery is prepared by the secondary liquid injection method according to claim 8 or 9.

Citation Information

Patent Citations

  • Lithium ion battery and preparation method thereof

    CN117457993A

  • Combined electrolyte for secondary liquid injection, lithium ion battery and secondary liquid injection method of lithium ion battery

    CN117594874A

  • Electrolyte composition, method for secondary electrolyte filling, and lithium secondary battery

    WO2024114190A1

Cited By

  • Battery

    CN119208702A

  • Battery

    CN119208702B