Method for producing rotationally symmetrical magnetic sheet, magnetic sheet, laminated core and electric machine

CN119013109APending Publication Date: 2024-11-22SIEMENS AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032441.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-03-02
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the punched and sintered magnetic sheets have high hysteresis loss at low frequencies and insufficient coercive strength, making it difficult to meet the demand for soft magnetic characteristics of modern high-power motors.

Method used

The magnetic sheet is manufactured by screen printing. The magnetic sheet with high iron content is formed by multiple heat treatment and uniaxial extrusion. The anisotropic texture structure is formed by recrystallization annealing, which improves the soft magnetic characteristics and coercivity of the magnetic sheet.

Benefits of technology

The magnetic sheet is achieved with low hysteresis loss and high coercive strength at low frequency, which improves the efficiency and energy efficiency of the motor, and the eddy current loss caused by the reduction of the thickness of the magnetic sheet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013109A_ABST
    Figure CN119013109A_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a rotationally symmetrical magnetic sheet (2) of a laminated core (4) of an electric machine (6), having a plurality of radially extending winding teeth (8), comprising the following steps:-applying a printing paste (12) to a substrate (14) by means of a screen printing method (16) in order to produce a green body (10), the printing paste (12) comprising a binder and iron particles, the invention relates to a method for producing a magnetic sheet (2), comprising the following steps:-a green body (10) comprising a binder and iron particles comprising more than 95% by weight of iron,-a first heat treatment (18) wherein the binder is removed from the green body (10) and thereby a preform (20) is formed,-a second heat treatment (22) of the preform (20) in the form of a sintering process for producing the magnetic sheet (2), subsequently, the magnetic sheet (2) is uniaxially pressed on the magnetic sheet plane (26) of the magnetic sheet (2) by means of a pressing punch (28) having a pressure of more than 5 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for producing a magnet sheet according to claim 1 , a magnet sheet according to claim 11 and a laminated core according to claim 12 and an electric machine according to claim 13 .

[0002] An electric motor, in particular an electric motor, has a rotor mounted on a shaft, which has a lamination stack with corresponding windings. The lamination stack mainly consists of or includes individual soft magnetic magnetic sheets, which in conventional electric motors are usually produced by punching out metal strips and stacked to form a lamination stack. For modern high-power electric motors, additively manufactured magnetic sheets, such as those produced by screen printing, are sintered and also stacked to form a lamination stack. The advantage of such printed magnetic sheets is that favorable soft magnetic materials can be used for material pairing to produce very good soft magnetic properties. However, the sintering process used for this purpose leads to isotropic crystal growth, which in turn has a negative impact on the coercive strength in the preferred direction along the plane of the magnetic sheet. For low frequencies, the magnetic sheets must have as low hysteresis losses as possible and therefore have a lower coercive strength in the direction of the magnetic flux. The technical problem to be solved by the present invention is to provide a method for manufacturing magnetic sheets, as well as the magnetic sheets themselves, a lamination group and a motor composed of the magnetic sheets. Compared with the prior art, especially punched magnetic sheets and printed and sintered magnetic sheets, the above-mentioned method, magnetic sheets, lamination group and motor have very good soft magnetic properties, and have a particularly high coercive strength, especially in the area where magnetic flux occurs.

[0003] This object is achieved according to the invention by a method for producing a magnet lamination according to claim 1 , a magnet lamination having the features of claim 11 , a laminated core having the features of claim 12 , and an electric machine having the features of claim 13 .

[0004] The method for manufacturing a rotationally symmetrical magnetic sheet according to claim 1 is used to manufacture a magnetic sheet of a lamination stack of an electric machine. The magnetic sheet has a plurality of radially extending winding teeth, and the method comprises the following steps:

[0005] - applying a printing paste onto a substrate by screen printing to produce a green body, wherein the printing paste comprises a binder and iron particles, and the iron particles comprise more than 95% by weight of iron,

[0006] - followed by a first heat treatment, in which the binder is removed from the green body and a preform is formed therefrom,

[0007] - the second heat treatment of the preform is then in the form of a sintering process to produce magnetic sheets,

[0008] - Then, the magnetic sheet is uniaxially pressed on the magnetic sheet plane by means of an extrusion punch with a pressure exceeding 5 MPa.

[0009] The advantage of the method is that, due to the screen printing process and the subsequent debonding or sintering process, the material used for the manufactured magnetic sheet has particularly good soft magnetic properties compared to the conventional punched magnetic sheets in the prior art, and has an iron content as high as possible, including at least 95% iron. Ideally, pure iron with only very few impurities is used for this purpose. Therefore, this printed and sintered magnetic sheet is different from the prior art in its soft magnetic properties. It has been surprisingly confirmed that uniaxial extrusion with a pressure of at least 5 MPa, preferably in a pressure range of not more than about 50 MPa, produces the following crystal structure in the radial direction, especially in the winding teeth, which has a positive effect on the magnetic flux in the radial direction of the winding teeth, and the hysteresis losses that occur there are very low, and therefore there is also a lower coercive strength. In addition, uniaxial extrusion improves the flatness of the magnetic sheet, which makes the density greater when stacked into a lamination group, and thus the iron content per unit volume of the magnetic sheet is also higher.

[0010] The green body should be understood here as a molded body for subsequent heat treatment, which usually contains a binder, which also includes a solvent for improving molding. The green body itself is usually mechanically self-supporting and can be mechanically loaded to a limited extent. The green body from which these binders and / or solvents have been removed is correspondingly referred to as a preform. The molded body only contains the functional components of the final body, which also effectively participate in the sintering process. Through heat treatment in the form of a sintering process, the preform is transformed into a sintered body. Unlike the melting process, the individual grains in the preform form a continuous, material-bonded structure through a diffusion process during the sintering process. After the sintering process, the resulting green body is correspondingly referred to as a magnetic sheet. However, this magnetic sheet can still be reprocessed in different ways.

[0011] The screen printing method is understood to be a process in which a printing paste is applied to a substrate, for example by means of a doctor blade, wherein a layer with a thickness generally in the range of 70 μm to 300 μm, in particular 150 μm to 250 μm, is produced. The paste is only printed on the substrate in specific, uncovered areas that are exposed by means of a screen. The paste is usually printed through a screen, but this is not necessary. Screen printing using a screen is referred to as a screen printing process, and therefore screen printing processes are included in the screen printing process.

[0012] It is also suitable to carry out a third heat treatment in the form of a recrystallization annealing after the above-mentioned pressing process. The third heat treatment is preferably carried out in a temperature range of 600° C. to 800° C. The recrystallization annealing process should be carried out at a constant temperature for at least 8 minutes to about 30 minutes. The recrystallization annealing is completed after 60 minutes at a constant temperature within this temperature window. This annealing process is conducive to the formation of a magnetically effective grain structure.

[0013] This preferably involves an anisotropic magnetic grain structure in the radial extension direction of the winding tooth. The radial extension direction of the winding tooth is also the magnetic flux path in which the magnetic flux is realized and in which soft magnetic properties with as little hysteresis losses as possible should be present. As the grain structure, the so-called Gaussian grain structure has been found to be particularly advantageous here. However, the so-called cubic grain structure is also suitable. The grains of the grain structure 34 advantageously have an average diameter of 80 μm to 400 μm in the image plane.

[0014] In crystallography, the grain structure refers to the overall orientation of the grains of a polycrystalline solid. The orientation of the crystal can be determined by the diffraction of an incident wave at a lattice plane. According to the Bragg equation, an angle can be set between the incident monochromatic beam and the lattice parameters of the lattice plane. For example, the grain structure can be seen in a Kerr microscope with the aid of polarized light. A micrograph of the surface of the magnetic disk is made and the micrograph is analyzed under a microscope with the aid of image processing software. For example, a Zeiss microscope and the software ZEN for this purpose can be used for image processing. In the grain structure described here, more than 50% of the effective magnetic domains have a preferred direction with a deviation of less than 36° from the radial direction.

[0015] A Gaussian grain structure is a special form of a magnetic sheet grain structure, wherein, for this grain structure, the cubic crystals of the iron lattice are located in the plane of the magnetic sheet along the (110) direction, wherein the cubic edges of the cubic lattice essentially follow the radial extension direction of the winding teeth as defined above. In an ideal case (not shown), the cubic edges are oriented along the radius of the magnetic sheet. Also suitable is a so-called cubic grain structure, wherein the cubic edges also extend in the radial direction in the ideal case, but are oriented in the (100) direction.

[0016] Furthermore, it has been found that the grain structure has an average diameter of 100 μm to 400 μm in the image plane. The grains have a preferred thickness of 40 to 80 μm, in particular approximately 60 μm.

[0017] The screen printing process can change the thickness of the green sheet to be manufactured by parameters such as the scraper pressure and the amount of slurry. The thickness of the green sheet is preferably 100μm to 400μm, so that after the second heat treatment, a magnetic sheet with a thickness of 100μm to 300μm is obtained. The thickness of the magnetic sheet is particularly preferably 150μm to 250μm. This makes the magnetic sheet significantly thinner than traditional punched magnetic sheets, which usually have a thickness of at least 330μm. It should be noted here that the eddy current losses in the operation of the motor decrease quadratically with the decrease in the thickness of the magnetic sheet. Therefore, thinner magnetic sheets result in lower eddy current losses in the motor. According to the prior art, punched magnetic sheets with a thickness of less than 330μm cannot achieve reproducible high quality.

[0018] In another embodiment of the present invention, the iron content in the iron particles is as high as possible. The iron content should be at least 95% by weight, preferably 97% by weight and preferably above 99% by weight. The higher the iron content, the better the magnetizability of the magnetic sheet. This increases the torque in the electric motor with lower eddy current losses, thereby improving the efficiency and energy efficiency of the electric motor or motor.

[0019] In another embodiment of the present invention, the extrusion punch is rotated during the pressing process at an angle α of less than 10°, in particular less than 3°, at least 0.5°. In addition to applying uniaxial pressure to the magnetic sheet, shearing forces are also applied, so that a texture structure is also generated along the circumference of the magnetic sheet in addition to the winding teeth and the surrounding yoke.

[0020] Another component of the present invention is a rotationally symmetrical magnetic sheet for a lamination stack of an electric motor. The magnetic sheet is characterized by having a thickness of 100 μm to 250 μm and a sintered metal phase having an iron content of at least 95% by weight. The magnetic sheet also has a plurality of radially extending winding teeth. In addition, a plurality of radially extending winding teeth are provided, and an anisotropic magnetic grain structure exists along the radial extension direction of the winding teeth. The magnetic sheet has the same advantages as those described for the magnetic sheet manufactured by the method according to claim 1. In particular, the anisotropic magnetic grain structure achieved by uniaxial extrusion of the magnetic sheet produces particularly good soft magnetic properties of the magnetic sheet.

[0021] Another component of the invention is a laminated core of an electric machine, which has a plurality of stacked magnetic sheets, which are produced by a method according to one of claims 1 to 10. Furthermore, a part of the invention is an electric machine, which comprises a laminated core according to claim 12, wherein the electric machine is preferably an electric motor.

[0022] Other designs and other features of the present invention are described in the following special description with the aid of the accompanying drawings. These are purely exemplary, schematically shown designs and do not represent a limitation of the scope of protection.

[0023] In the attached picture:

[0024] Figure 1 An exploded view of a conventional electric machine with a rotor and a lamination stack is shown,

[0025] Figure 2 A conventional lamination stack is shown, wherein the lamination stack is composed of a plurality of magnetic sheets having a plurality of winding teeth.

[0026] Figure 3 shows a laminated core with magnetic laminations in an alternative embodiment,

[0027] Figure 4 A top view of a magnetic sheet is shown,

[0028] Figure 5 A schematic diagram showing the manufacturing process of a magnetic sheet,

[0029] Figure 6 A diagram showing the magnetization when using different texture structures,

[0030] Figure 7 Schematic diagram of the microstructure showing the texture structure with directional indications for different magnetic domains.

[0031] Figure 1 An overview of a typical electric machine 6 in the form of an electric motor 46 is shown in an exploded view. This view serves to better organize the following description in detail. The electric machine 6 has a rotor 48 mounted on a shaft 50 . Figure 2 The lamination stack 4 is composed of a plurality of stacked magnetic sheets 2. Figure 1 A portion of a rotor 48 is shown. The individual magnet laminations 2 of the lamination stack 4 have winding teeth 8, around which an electrical wire (not shown here) is wound. The winding teeth 8 in the lamination stack 4 thus serve as a yoke for an electromagnet.

[0032] Another design scheme of the lamination pack 4 is as follows Figure 3 As shown, only four magnetic sheets 2 are stacked one on top of the other, but this is usually Figure 2 Shown are a further number of magnetic sheets 2 . Figure 3 The magnet disk 2 shown also has winding teeth 8 , wherein the magnet disk 2 also has a circumferential ring 9 into which the winding teeth 8 merge. Figure 3 The surrounding ring 9 is arranged in the area outside the magnetic disk 2. Figure 2 In the illustrated magnet disk 2 , a circumferential ring 9 is arranged in the interior of the magnet disk 2 .

[0033] Figure 4 A top view of a magnetic sheet 2 is shown. Figure 3 The radial extension 44 is shown here, which corresponds to the radius around the center of the rotationally symmetrical magnet piece 2. The winding teeth 8 are also arranged along a radial line. Figure 4 The magnet plane is also shown in dashed lines, which coincides with the image plane in this view. The second arrow in the surrounding ring 9 of the magnet 2 is labeled α, and this angle will be explained below.

[0034] Figure 5 Schematically shows the Figures 1 to 4 The manufacture of the magnetic sheet 2 and the lamination group 4 is described. The explanation starts from the first subview a on the upper left, which shows a screen printing method 16. The printing paste 12 is printed onto the substrate 14 by means of a scraper 52 through a screen 54, which is usually represented as a screen. A green body 10 is thus produced. The green body 10 usually has a thickness 40, which is about 250 μm to 300 μm in this state. The green body 10 has the components of the printing paste 12. These components are solvents, polymer binders and iron powder. The iron powder has an iron content as high as possible, which should be higher than 95% by weight. The iron content of the iron particles in the printing paste is especially higher than 99% by weight, so it can already be regarded as pure iron here.

[0035] Especially after the solvent is dried, the green body 10 itself has mechanical self-supporting properties, and can be Figure 5 The green body is now separated from the substrate 14, or, if the substrate 14 is a flexible substrate, the green body is directly subjected to a heat treatment on the substrate, i.e., a first heat treatment step 18. The first heat treatment step 18 is a debinding process, in which the green body 10 is dried, i.e., the solvent is removed, and then heated to such an extent that the organic binder is also thermally decomposed.

[0036] The process is schematically shown as a continuous process in a tunnel furnace 56. Figure 5 b. In principle, it is also possible to carry out the individual processes in individual batches in a batch furnace. However, in order to achieve the highest possible efficiency during production, it is appropriate to use a tunnel furnace as shown here. During the first heat treatment 18, i.e. during the debinding process, a temperature of, for example, about 250° C. is preferably applied in an inert gas. The second part of the continuous heating furnace 56 is characterized by a second heat treatment 22, which is carried out in the form of a sintering process 24. Compared with the first heat treatment, the temperature is significantly increased here, which is about 1000° C. to 1350° C. for sintering the iron particles.

[0037] It should be noted that when entering the furnace 56 or during the first heat treatment, the green body 10 is still referred to as the green body 10, after the first heat treatment, the green body is referred to as the preform, the preform is input into the sintering process 24, and usually after leaving the continuous heating furnace or after the sintering process, the preform 20 is referred to as the magnetic sheet 2. The thickness 42 of the magnetic sheet 2 is 150 μm to 250 μm.

[0038] In addition, according to Figure 5 c, the magnetic sheet 2 is uniaxially extruded perpendicularly to the magnetic sheet plane 26. The effect of the uniaxial pressing process performed in the uniaxial press 30 with the aid of the extrusion punch 28 will be described below. It should be noted that the extrusion punch 28 is pressed on the magnetic sheet 2 by a force F, and the force F should be at least 5 MPa and generally does not need to exceed 50 MPa. It is appropriate to perform uniaxial extrusion multiple times, for example, repeating the extrusion process five times, in order to form the desired texture structure particularly well. It is also appropriate to regulate the temperature of the magnetic sheet 2 during uniaxial extrusion. This can be achieved, for example, by hot pressing at a temperature of, for example, 100°C to 300°C.

[0039] If necessary, the punch can be rotated by an angle α of less than 5°, for example 1°, so that shear forces are introduced into the magnet sheet 2 in addition to the uniaxial force F. It has been found that the effect of the force on the crystal structure of the magnet sheet is similar to that of a rolling process, which is unexpected due to the static nature of the force. It is particularly advantageous that the uniaxial pressing subjects the magnet sheet 2 to less shear forces than the rolling process.

[0040] In another optional step, according to Figure 5 d Recrystallization annealing is performed in the third heat treatment 32. The third heat treatment 32 is schematically shown here in the form of a batch furnace, which can also be Figure 5 b is carried out in a continuous heating furnace 56. For the recrystallization annealing 32, a temperature of 600°C to 800°C, for example 620°C or 720°C, can generally be kept constant for at least 8 minutes to 30 minutes. The temperature treatment in this area further strengthens the formation of the anisotropic grain structure of the magnetic sheet 2 in a certain material area. The temperature here is an influencing quantity on the size of the grains formed in the grain structure 34. The higher the recrystallization temperature, the larger the grains formed here. Advantageously, larger grains (80-150μm) are formed inside the magnetic sheet, while smaller grains (50-100μm) are formed on the surface (to suppress abnormal eddy current losses).

[0041] The heat-treated magnetic sheets 2 are now stacked to form a lamination stack 4, wherein the process is automated, for example, using a robot 60. The lamination stack 4 can be bonded to the extent that the individual magnetic sheets 2 are provided with an organic coating and, if necessary, immersed in a bath of an organic adhesive. This process will not be explained in more detail here.

[0042] As described above, an anisotropic grain structure 34 is produced in the winding tooth 8 by means of uniaxial pressing, in particular in the radial extension direction 44. This grain structure 34 is further strengthened by recrystallization annealing, ie, the third heat treatment 32. Figure 6 The losses P in the magnet plane 26 at 50 Hz are plotted according to the extension direction of the winding tooth 8. 1.5 The extension direction is along the radial extension direction 44 and transverse to the radial direction, ie, along the circumferential direction 64. The first grain structure 34 is a uniaxial Gaussian grain structure 36. If a second grain structure along a 90° direction is added, it is called a cubic grain structure 38. Figure 6 The circle 39 in the figure represents a purely isotropic grain structure 39. It can be seen here that the losses along the radial extension direction 44 are significantly lower than the losses in the case of isotropic materials for the Gaussian grain structure 36 and the cubic grain structure 38. It is therefore very advantageous to introduce these grain structures 34, 36, 38 into the magnetic sheet 2 by the uniaxial extrusion and to strengthen them by the third heat treatment 32, i.e., recrystallization annealing, if necessary.

[0043] The texture structure 34 does not usually naturally form precisely oriented magnetic domains, but rather involves Figure 7 The preferred directions shown are mostly oriented along the radial extension direction 44. Figure 7 As shown by the arrows and angle data in FIG. 4 , at least 50% of the grains in the individual grains should not deviate from the preferred direction by more than 36° in the radial and tangential directions 44. This is referred to herein as an isotropic grain structure, such as Figure 6 The texture structure shown produces higher magnetic losses for a preferred direction.

[0044] Reference numerals list

[0045] 2 Magnetic disk

[0046] 4 lamination pack

[0047] 6 Motor

[0048] 8 Winding teeth

[0049] 9 Ring around

[0050] 10 Green

[0051] 12 Printing paste

[0052] 14 substrate

[0053] 16 Screen printing process

[0054] 18 First heat treatment

[0055] 20 Preform

[0056] 22 Second heat treatment

[0057] 24 Sintering process

[0058] 26 Magnetic Plate Plane

[0059] 28 Extrusion Punch

[0060] 30 Uniaxial Press

[0061] 32 Third heat treatment

[0062] 34 Texture structure

[0063] 36 Gaussian texture structure

[0064] 38 Cube Texture Structure

[0065] 39 Isotropic grain structure

[0066] 40 Green thickness

[0067] 42 Thickness of magnetic sheet

[0068] α Angle

[0069] 44 Radial extension direction

[0070] 46 Electric Motor

[0071] 48 Rotor

[0072] 50 Axis

[0073] 52 Scraper

[0074] 54 Silk Screen

[0075] 56 Continuous Heating Furnace

[0076] 58 Conveyor belt

[0077] 60 Robotic Arm

[0078] 64 Circumferential

Claims

1. A method for producing a rotationally symmetrical magnetic segment (2) of a lamination stack (4) of an electric machine (6), the magnetic segment having a plurality of radially extending winding teeth (8), the method comprising the following steps: - applying a printing paste (12) to a substrate (14) by screen printing (16) to produce a green body (10), wherein the printing paste (12) comprises a binder and iron particles, and the iron particles comprise more than 95% by weight of iron, a first heat treatment (18), in which the binder is removed from the green body (10) and a preform (20) is formed therefrom, - a second heat treatment (22) of the preform (20) in the form of a sintering process to produce a magnetic sheet (2), - Then, the magnetic sheet (2) is uniaxially pressed on the magnetic sheet plane (26) by means of a pressing punch (28) with a pressure exceeding 5 MPa.

2. The method according to claim 1, characterized in that After the uniaxial pressing, a third heat treatment in the form of a recrystallization annealing is carried out.

3. The method according to claim 2, characterized in that During the recrystallization annealing, a temperature between 600° C. and 800° C. is kept constant for at least 8 minutes.

4. The method according to any one of claims 1 to 3, characterized in that An anisotropic magnetic texture structure (34) is generated along the radial extension direction of the winding teeth.

5. The method according to claim 4, characterized in that A Gaussian texture structure is generated along the radial extension direction of the winding teeth.

6. The method according to claim 4 or 5, characterized in that: The grains of the texture structure (34) have an average diameter of 80 μm to 400 μm in the image plane.

7. The method according to any one of the preceding claims, characterized in that The thickness of the green body (10) is adjusted in the range of 100 μm to 400 μm by screen printing (16), thereby producing a thickness of the magnetic sheet (2) in the range of 100 μm to 300 μm.

8. The method according to claim 7, characterized in that The thickness (42) of the magnetic sheet is adjusted between 150 μm and 250 μm.

9. The method according to any one of the preceding claims, characterized in that The iron particles have an iron content of more than 97% by weight, preferably more than 99% by weight.

10. The method according to any of the preceding claims, characterized in that The extrusion punch (28) is rotated during the extrusion process by an angle α of less than 10°, in particular less than 3°, at least 0.5°.

11. A rotationally symmetrical magnetic sheet for a lamination stack (4) of an electric machine (6), characterized in that: The magnetic sheet (2) has a thickness (42) between 100 μm and 250 μm and has a sintered metal phase with an iron content of at least 95% by weight, wherein a plurality of radially extending winding teeth (8) are provided and an anisotropic magnetic grain structure (34) is present along the radial extension direction (44) of the winding teeth (8).

12. A laminated core for an electric machine, comprising a plurality of stacked magnetic laminations (2), the magnetic laminations being produced by the method according to any one of claims 1 to 10.

13. An electric machine comprising the lamination stack (4) according to claim 12.

14. The motor according to claim 13, characterized in that The motor (6) is an electric motor.