Improved process for depolymerizing polyethylene terephthalate

By reacting alkali metal glycol with ethylene glycol in electrolytic cells, the problem of low BHET generation ratio in PET depolymerization is solved, and more efficient BHET generation is achieved, supporting PET recycling and new production.

CN119013338APending Publication Date: 2024-11-22EVONIK OPERATIONS GMBH
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN202280094494.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-04
Filing Date
2022-11-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to obtain the maximum proportion of bis-2-hydroxyethyl terephthalate (BHET) during the depolymerization of PET, which affects the effective recycling and new production of PET.

Method used

The alkali metal glycol solution was generated in the electrolytic cell and reacted with ethylene glycol, and the BHET generation ratio was increased through the specific electrolytic cell structure and electrode material.

Benefits of technology

A higher BHET ratio generation than traditional methods is achieved, supporting efficient recycling and new production of PET.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005069006500000174
    Figure BDA0005069006500000174
  • Figure BDA0005069006500000401
    Figure BDA0005069006500000401
  • Figure BDA0005069006500000402
    Figure BDA0005069006500000402
Patent Text Reader

Abstract

The invention relates to a process for the depolymerization of polyethylene terephthalate ("PET") in which PET reacts with an electrolytically produced alkali metal glycolate, in particular sodium or potassium glycolate, forming a mixture M1 comprising bis (2-hydroxyethyl) terephthalate ("BHET"). The method according to the invention is characterized in that BHET accounts for a particularly high proportion in the decomposition product in the mixture M1. Thus, the process of the present invention provides a high yield of BHET, which can be directly used in regenerative PET production. The invention also relates to a process for recovering PET in which BHET obtained in the PET depolymerization process is re-polymerized to PET, optionally after further purification from M1.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a process for the depolymerization of polyethylene terephthalate (= "PET"), wherein PET is reacted with an electrolytically produced alkali metal glycolate, in particular sodium glycolate or potassium glycolate, to produce a mixture M1 comprising bis-2-hydroxyethyl terephthalate (= "BHET"; CAS No.: 959-26-2).

[0002] The process according to the invention is characterized in that BHET forms a particularly high proportion in the cleavage products in the mixture M1. The process according to the invention thus provides a high yield of BHET which can be used directly in the new production of PET.

[0003] The present invention therefore also relates to a process for recycling PET, wherein BHET obtained in a depolymerization process of PET, optionally after further purification from M1, is polymerized again to give PET. Background Art

[0004] Polyethylene terephthalate (= "PET") is one of the most important plastics, which is used in textile fibers, as films, and as a material for plastic bottles. In 2007 alone, the amount used in plastic bottles was ~10 7 t(W.Caseri,Polyethylenterephthalate,RD-16-03258(2009)in F. B.Dill,G.Eisenbrand,F.Faupel,B.Fugmann,T.Gamse,R.Matissek,G.Pohnert,A.Rühling,S.Schmidt,G.Sprenger, [Online], Stuttgart, Georg Thieme Verlag, January 2022).

[0005] Due to its persistence and the amount of waste derived from PET, it constitutes one of the greatest environmental challenges today. The solution to this problem lies in the avoidance and efficient recycling of PET.

[0006] The prior art proposes a variety of PET cracking methods.

[0007] GB 784,248A describes the methanolysis of PET.

[0008] Hydrolysis methods for depolymerization of PET are described in JP 2000-309663 A, US 4,355,175 A and T. Yoshioka, N. Okayama, A. Okuwaki, Ind. Eng. Chem. Res. 1998, 37, 336-340.

[0009] The reaction of PET with ethylene glycol is described in EP 0723951 A1, US 3,222,299 A, WO 2020 / 002999 A2, by SR Shukla, AM Harad, Journal of Applied Polymer Science 2005, 97, 513-517 (“Shukla & Harad” hereinafter) and NDPingale, SR Shukla, European Polymer Journal 2008, 44, 4151-4156.

[0010] Shukla & Harad state: Glycolysis of PET produces bis-2-hydroxyethyl terephthalate (="BHET"). This cleavage product can simultaneously be used as a reactant for the production of new PET.

[0011] There is therefore interest in depolymerization processes for PET in which the greatest proportion of BHET is obtained in the pyrolysis products.

[0012] The problem addressed by the present invention is that of providing such a method. Summary of the invention

[0013] Surprisingly, a solution to the problem posed by the present invention has now been found.

[0014] The present invention relates to a depolymerization method of polyethylene terephthalate (PET), which comprises the following steps:

[0015] (a) In electrolytic cell E <1> M A Hydroxyacetate solution in ethylene glycol L1 <21> , where M A is an alkali metal cation, in particular selected from lithium, potassium, sodium, preferably selected from potassium, sodium, and most preferably selected from sodium, the electrolytic cell comprising

[0016] - at least one anode chamber K A <11> , which has at least one inlet Z KA <110> , at least one exit A KA <111> , and comprising an anode electrode E A <113> Internal I KA <112> ,

[0017] - at least one cathode chamber K K <12> , which has at least one inlet Z KK <120> , at least one exit A KK <121> , and comprising a cathode electrode EK <123> Internal I KK <122> ,

[0018] - and optionally at least one intervening intermediate chamber K M <13> , which has at least one inlet Z KM <130> , at least one exit A KM <131> and internal I KM <132> ,

[0019] Among them I KA <112> and I KM <132> Through the diffusion barrier D <14> are separated from each other, and A KM <131> By connecting V AM <15> Connect to inlet Z KA <110> , so that the liquid can be KM <132> Connect V AM <15> Pass to I KA <112> ,

[0020] in

[0021] - wherein said electrolytic cell E <1> Does not include intermediate chamber K M <13> In this case, I KA <112> and I KK <122> Through the partition wall W <16> Separated from each other,

[0022] - wherein said electrolytic cell E <1> Contains at least one intermediate chamber K M <13> In this case, I KK <122> and I KM <132> Through the partition wall W <16> Separated from each other,

[0023] The partition wall W <16> Having a surface O KK <163> One side S KK <161> and in S KK <161> and having a surface O A / MK <164> One side S A / MK <162> , wherein the partition wall W <16> So that the partition wall W <16> Solid electrolyte ceramic F containing alkali metal cations A <18> Via surface O KK <163> In S KK <161> Side and Internal I KK <122> The direct contact method comprises at least one solid electrolyte ceramic F that conducts alkali metal cations A <18> ,

[0024] And among them

[0025] - wherein said electrolytic cell E <1> Does not include intermediate chamber K M <13> In the case of <16> Solid electrolyte ceramic F containing alkali metal cations A <18> Via surface O A / MK <164> In S A / MK <162> Side and Internal I KA <112> Direct contact,

[0026] - wherein said electrolytic cell E <1> Contains at least one intermediate chamber K M <13> In the case of <16> Solid electrolyte ceramic F containing alkali metal cations A <18> Via surface O A / MK <164> In S A / MK <162> Side and Internal I KM <132> Direct contact,

[0027] (α) where, in the electrolytic cell E <1> When it does not contain the intermediate chamber K M <13> , the following steps (α1), (α2), and (α3) are performed simultaneously:

[0028] (α1) Solution L2 containing ethylene glycol <22> Guided by I KK <122> ,

[0029] (α2) will contain M A Neutral or alkaline aqueous solution L3 of a salt S as a cation <23> Guided by I KA <112> ,

[0030] (α3) in E A <113> and E K <123> Apply voltage between

[0031] or

[0032] (β) where, in the electrolytic cell E <1> When it contains at least one intermediate chamber K M <13> , the following steps (β1), (β2), and (β3) are performed simultaneously:

[0033] (β1) Solution L2 containing ethylene glycol <22> Guided by I KK <122> ,

[0034] (β2) will contain M ANeutral or alkaline aqueous solution L3 of a salt S as a cation <23> Guided by I KM <132> , then through V AM <15> , then through I KA <112> ,

[0035] (β3) in E A <113> and E K <123> Apply voltage between

[0036] It is at Exit A KK <121> Solution L1 is provided <21> , M A The concentration of glycolate is L1 <21> The ratio is in L2 <22> Medium-high,

[0037] And it is at exit A KA <111> Provide an aqueous solution of S L4 <24> , the concentration of S in L4 <24> The ratio is in L3 <23> Medium-low;

[0038] (b) Solution L1 <21> Reaction with PET to produce a mixture M1 comprising bis-2-hydroxyethyl terephthalate (="BHET").

[0039] In a further aspect, the present invention relates to a process for recycling PET, wherein the BHET obtained in the process for depolymerization according to the present invention is polymerized in step (ζ) to produce PET.

[0040] It has been found that, surprisingly, PET and the solution L1 obtained by the electrolysis method according to the invention <21> The reaction provides a higher BHET ratio than in the conventional process in which the basic alkali metal glycolate solution is obtained by mixing ethylene glycol in the corresponding alkali metal hydroxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1A and 1B

[0042] Figure 1A (=“ Figure 1A ”) shows a method for use in an electrolytic cell E according to the present invention. <1> Sodium glycolate solution L1 is produced <21> This includes the cathode chamber K K <12> and anode chamber K A <11> .

[0043] The cathode chamber K K <12> Included inside KK <122> The cathode electrode E K <123> , Entrance Z KK <120> and Exit A KK<121> .

[0044] The anode chamber K A <11> Included inside KA <112> The anode electrode E A <113> , Entrance Z KA <110> and Exit A KA <111> .

[0045] Two rooms K A <11> and K K <12> Through the two-room pool E <1> The outer wall W A <80> Internal I KK <122> It is also made of a NaSICON solid electrolyte ceramic F that can selectively penetrate sodium ions. A <18> The partition wall W <16> With internal I KA <112> The NaSICON solid electrolyte ceramic F A <18> Extended to two-room pool E <1> The partition wall has two sides S KK <161> and S A / MK <162> , its surface O KK <163> and O A / MK <164> Contact the corresponding internal I KK <122> or I KA <112> .

[0046] pH 10.5 sodium chloride aqueous solution L3 <23> Via entrance Z KA <110> Introduce internal I in the opposite direction of gravity KA <112> middle.

[0047] 1 wt% solution of sodium glycolate in ethylene glycol L2 <22> Via entrance Z KK <120> Boot into the interior KK <122> middle.

[0048] At the same time, at the cathode electrode E K <123> and the anode electrode E A <113> As a result, the internal I KK <122> In electrolyte L2 <22> The ethylene glycol in the solution is reduced to glycolate and H2(HOCH2CH2OH+e - →HOCH2CH2O - +1 / 2H2; and there is also HOCH2CH2O - +e - → - OCH2CH2O- +1 / 2H2). At the same time, sodium ions are transported from the inner KA <112> Diffusion through the NaSICON solid electrolyte ceramic F A <18> Entering the interior KK <122> In general, this increases the internal I KK <122> The concentration of sodium glycolate in the outlet A KK <121> Provides a ratio of L2 <22> Ethylene glycol solution of sodium glycolate with a high sodium glycolate concentration (about 20 wt. % sodium glycolate in ethylene glycol) L1 <21> .

[0049] Inside I KA <112> In the reaction, oxidation of chloride ions occurs to produce molecular chlorine (Cl - →1 / 2Cl2+e). At outlet A KA <111> , obtain aqueous solution L4 <24> , the content of NaCl is higher than that of L3 <23> Chlorine (Cl2) reacts in water according to the reaction Cl2+H2O→HOCl+HCl to form hypochlorous acid and hydrochloric acid, which react with other water molecules to form an acidic reaction. This acid destroys the NaSICON solid electrolyte ceramic F A <18> .

[0050] Figure 1B (=“ Figure 1B ”) shows that it contains the middle chamber K M <13> The electrolytic cell E <1> Another embodiment of the method according to the invention is in the form of a three-chamber pool E <1> Therefore, the cathode chamber K K <12> , anode chamber K A <11> and the inserted intermediate chamber K M <13> .

[0051] The cathode chamber K K <12> Included inside KK <122> The cathode electrode E K <123> , Entrance Z KK <120> and Exit A KK <121> .

[0052] The anode chamber K A <11> Included inside KA <112> The anode electrode E A <113> , Entrance Z KA <110> and Exit A KA <111> .

[0053] The intermediate chamber K M <13> Contains internal IKM <132> , Entrance Z KM <130> and Exit A KM <131> .

[0054] The internal KA <112> Through this connection V AM <15> Connect to internal I KM <132> .

[0055] The three chambers are connected by a three-chamber pool E <1> The outer wall W A <80> Intermediate Room K M <13> Internal I KM <132> It is also made of a NaSICON solid electrolyte ceramic F that can selectively penetrate sodium ions. A <18> The partition wall W <16> With cathode chamber K K <12> Internal I KK <122> The NaSICON solid electrolyte ceramic F A <18> Extended to the three-room pool E <1> The partition wall has two sides S KK <161> and S A / MK <162> , its surface O KK <163> and O A / MK <164> Contact the corresponding internal I KK <122> or I KM <132> .

[0056] The intermediate chamber K M <13> Internal I KM <132> Then it passes through the diffusion barrier D <14> , and the anode chamber K A <11> Internal I KA <112> The NaSICON solid electrolyte ceramic F A <18> and diffusion barrier D <14> Extended to the three-room pool E <1> The diffusion barrier D <14> It is a cation exchange membrane (sulfonated PTFE).

[0057] In accordance with Figure 1B In the embodiment, connecting V AM <15> Formed in electrolytic cell E <1> The outside of the electrolytic cell E is formed by a tube or hose (whose material can be selected from rubber, metal and plastic). <1> The outside of the connection V AM <15> In the three-room pool E <1> The outer wall W A <80> The outside of the middle chamber K can be used to transfer liquid from the M <13> Internal I KM<132> Lead to anode chamber K A <11> Internal I KA <112> . The connection V AM <15> Export A KM <131> (It is in the middle chamber K M <13> The bottom of the electrolytic cell E <1> The outer wall W A <80> ) connected to inlet Z KA <110> (It is in the anode chamber K A <11> The bottom of the electrolytic cell E <1> The outer wall W A <80> ).

[0058] pH 10.5 sodium chloride aqueous solution L3 <23> Via entrance Z KM <130> , is introduced into the intermediate chamber K in the direction of gravity M The internal I KM <132> The connection V AM <15> The middle chamber K M <13> Internal I KM <132> Connected to anode chamber K A <11> Internal I KA <112> . Sodium chloride solution L3 <23> From this internal KM <132> By connecting V AM <15> , leading into the internal I KM <112> middle.

[0059] ~1 wt% solution of sodium glycolate in ethylene glycol L2 <22> Via entrance Z KK <120> Boot into the interior KK <122> middle.

[0060] At the same time, at the cathode electrode E K <123> and the anode electrode E A <113> As a result, the internal I KK <122> In electrolyte L2 <22> The ethylene glycol in the solution is reduced to glycolate and H2(HOCH2CH2OH+e - →HOCH2CH2O - +1 / 2H2; and there is also HOCH2CH2O - +e - → - OCH2CH2O - +1 / 2H2). At the same time, sodium ions move from the intermediate chamber K M <103> Internal I KM <132> Diffusion through NaSICON solid electrolyte ceramics FA <18> Entering the interior KK <122> In general, this increases the internal I KK <122> The concentration of sodium glycolate in the outlet A KK <121> Provides a ratio of L2 <22> Ethylene glycol solution of sodium glycolate with a high sodium glycolate concentration (about 20 wt. % sodium glycolate in ethylene glycol) L1 <21> .

[0061] Inside I KA <112> In the reaction, oxidation of chloride ions occurs to produce molecular chlorine (Cl - →1 / 2Cl2+e). At outlet A KA <111> , obtain aqueous solution L4 <24> , the content of NaCl is higher than that of L3 <23> Chlorine (Cl2) reacts in water according to the reaction Cl2+H2O→HOCl+HCl to form hypochlorous acid and hydrochloric acid, which react with other water molecules to form an acidic reaction. This acidity will destroy the NaSICON solid electrolyte ceramic F A <18> , but due to the arrangement in the three-chamber cell, it is limited to the anode chamber K A <11> , and therefore in the electrolytic cell E away from the NaSICON solid electrolyte ceramic F A <18> . This significantly increases its lifespan.

[0062] Figure 2A and 2B

[0063] Figure 2A (=“ Figure 2A ”) shows the preferred partition wall W <16> This contains two NaSICON solid electrolyte ceramic F A <18> and F B <19> , which are separated by the element T <17> Separated from each other and each fixed thereto in a gap-free manner. The separation element T <17> It has a rectangular parallelepiped geometry, with two opposite sides, F A <18> and F B <19> Fastened in a play-free manner (eg by adhesive).

[0064] With surface O KK <163> Side S KK <161> lies in the plane of the figure and has surface O A / MK <164> Side S A / MK <162> exist Figure 2A Not visible in the figure, behind the plane of the figure.

[0065] Figure 2B (=“ Figure 2B”) shows the preferred partition wall W <16> Another embodiment of the present invention. This comprises four NaSICON solid electrolyte ceramic F A <18> 、F B <19> 、F C <28> 、F D <29> , which are separated by the element T <17> Separated from each other and each fixed thereto in a gap-free manner. Separating element T <17> It has a cross shape with F fixed on its opposite sides. A <18> 、F B <19> 、F C <28> and F D <29> .

[0066] With surface O KK <163> Side S KK <161> lies in the plane of the figure and has surface O A / MK <164> Side S A / MK <162> exist Figure 2B Not visible in the figure, behind the plane of the figure.

[0067] Figures 3A to 3C

[0068] Figure 3A (=“ Figure 3A ”) is displayed in Figure 2A and 2B As described, for example, by means of a binder, a corresponding solid electrolyte ceramic F A <18> and F B <19> Fixed to the separation element T <17> .

[0069] Figure 3B (=“ Figure 3B ”) describes a further embodiment of a preferred partition wall W. Here, the separation element T <17> It has two concave depressions (grooves) in which two solid electrolyte ceramic F are adapted. A <18> and F B <19> For this purpose, solid electrolyte ceramics F A <18> and F B <19> The shape of the edge can be adjusted mechanically accordingly. In addition, the use of seals Di <40> , which is mounted on the separation element T, for example using an adhesive <17> and the corresponding solid electrolyte ceramic F A <18> or F B <19> The separation element T <17> Here, two or more components may be <171> and <172> constitute, as in Figure 3B In the solid electrolyte ceramic FA <18> and F B <19> With suitable geometry of the shape of the edge and the adaptation of the case, the latter can be clamped between the two components <171> and <172> This further improves the separation element T <17> / Ceramic F A <18> or F B <19> The connection stability and partition wall W <16> integrity.

[0070] Figure 3C (=“ Figure 3C ”) illustrates a further embodiment of a preferred partition wall W. This corresponds to Figure 3B described above, except that the separation element T <17> The depression (groove) in the A <18> and F B <19> ) is not concave but conical.

[0071] Figures 4A to 4D

[0072] Figure 4A (=“ Figure 4A ”) to 4D show preferred partition walls W <16> A further implementation scheme of .

[0073] exist Figure 4A The partition wall W shown in <16> Corresponding to Figure 2A The partition wall W shown in <16> , which also contains the frame element R <20> This completely covers the partition wall W <16> All surfaces except O KK <163> and O A / MK <164> In addition, the frame element R <20> Not with separate element T <17> One piece form together.

[0074] Figure 4B (=“ Figure 4B ”) shows the preferred partition wall W <16> This corresponds to another embodiment of Figure 4A The embodiment shown in FIG. 1 is different from the embodiment shown in FIG. 1 , except that it comprises two connecting partition walls W <16> The upper and lower surfaces of the frame element R <20> Besides.

[0075] Figure 4C (=“ Figure 4C ”) shows the preferred partition wall W <16> Another embodiment of Figure 4C The partition wall W shown in <16> Corresponding to Figure 2B The partition wall W shown in <16> , which also contains the frame element R <20> This completely covers the partition wall W <16> All surfaces except O KK <163> and OA / MK <164> In addition, the frame element R <20> Not with separate element T <17> One piece form together.

[0076] Figure 4D (=“ Figure 4D ”) shows the preferred partition wall W <16> This corresponds to another embodiment of Figure 4C The embodiment shown in FIG. 1 is different from the embodiment shown in FIG. 1 , except that it comprises two connecting partition walls W <16> The upper and lower surfaces of the frame element R <20> Besides.

[0077] Figure 5A and 5B

[0078] Figure 5A (=“ Figure 5A ”) shows an electrolytic cell E in a preferred embodiment of the method according to the present invention <1> This corresponds to Figure 1A The electrolytic cell shown in FIG. 1 is different in that the dividing wall W <16> The cathode chamber K K <12> Internal I KK <122> With anode chamber K A <11> Internal I KA <112> The dividing wall is Figure 2A and 2B As shown in .

[0079] Figure 5B (=“ Figure 5B ”) shows an electrolytic cell E in a preferred embodiment of the method according to the present invention <1> This corresponds to Figure 1A The electrolytic cell shown in FIG. 1 is different in that the dividing wall W <16> The cathode chamber K K <12> Internal I KK <122> With anode chamber K A <11> Internal I KA <112> The partition wall W <16> is Figures 4A to 4D The frame element R <20> Forming the outer wall W A <80> part, so that the partition wall W <16> The contained solid electrolyte ceramics are protected from pressure if they are partition walls W <16> The pressure will flow through the partition wall W <16> Furthermore, the solid electrolyte ceramic is therefore completely used for separation in the electrolytic cell E <1> Internal I KK <122> and I KA <112> , because they are not partially covered by the outer wall.

[0080] Fig. 6A and 6B

[0081] Fig. 6A (=“ Fig. 6A ”) shows that according to the present invention, Figure 1B The electrolytic cell E shown in <1> The difference is that from the middle chamber K M <13> Internal I KM <132> To anode chamber K A <11> Internal I KA <112> Connection V AM <15> Through the diffusion barrier D <14> These perforations can then be stamped into the diffusion barrier D <14> or due to the diffusion barrier D <14> In the manufacturing process (for example in the case of a textile fabric such as a filter cloth or a metal braid), the perforations may already be present therein at the beginning. In this embodiment, the entirety of these perforations connects the V AM <15> , by connecting V AM <15> , the electrolyte can be from the internal I KM <132> Boot to Internal I KA <112> middle.

[0082] Figure 6B (=“ Figure 6B ”) shows electrolytic cell E <1> Another embodiment of the method according to the invention is in the form of Figure 1B The electrolytic cell E shown in <1> , the difference is that from the middle chamber K M <13> Internal I KM <132> To anode chamber K A <11> Internal I KA <112> Connection V AM <15> Through the diffusion barrier D <14> and outer wall W A <80> This gap can be created because the additional impermeable diffusion barrier D <14> Set in electrolytic cell E <1> so that it does not completely fill the intermediate chamber K M <13> Internal I KM <132> With anode chamber K A <11> Internal I KA <112> separation, but leaving the gap as a connection V AM <15> .

[0083] Fig. 7A and 7B

[0084] Fig. 7A (=“ Fig. 7A ”) shows the preferred partition wall W <16> Another embodiment of the present invention. This comprises four NaSICON solid electrolyte ceramic FA <18> 、F B <19> 、F C <28> and F D <29> , which consists of two halves <171> and <172> Separation element T <17> The partition wall W <16> Also includes the same two halves <201> and <202> The frame element R <20> .

[0085] The partition wall W <16> It is composed of two parts that can be folded into one, wherein the separation element T <17> Half <171> With frame element R <20> Half <201> Together in one piece, and separate components T <17> Half <172> With frame element R <20> Half <202> The two parts can be connected together in one piece. <50> Connected to each other and can be locked <60> , folded in and locked in place.

[0086] The four NaSICON solid electrolyte ceramics A <18> 、F B <19> 、F C <28> and F D <29> is sandwiched between the two halves, with a ring in each case acting as a seal for sealing Di <40> .

[0087] Fig. 7A The left hand side shows the partition wall W <16> With surface O KK <163> Side S KK <161> Front view of the seal. <40> The ring is shown by the dotted outline. The right hand side of the figure shows the partition wall W <16> Side view of.

[0088] Figure 7B (=“ Figure 7B ”) shows the preferred partition wall W <16> This corresponds to another embodiment of Fig. 7A The embodiment described in the embodiment, except that it comprises nine NaSICON solid electrolyte ceramic F A <18> 、F B <19> 、F C <28> 、F D <29> 、F E <30> 、F F <31> 、F G <32> 、F H <33> 、F I <34> .

[0089] Figure 8

[0090] Figure 8 (= Figure 8 ) shows a comparison of the contents of BHET ("1"), 2-hydroxyethyl terephthalate ("MHET"; "2") and terephthalate ester ("TS"; "3") in the depolymerization using sodium glycolate obtained by the process according to the present invention and sodium glycolate obtained by a conventional process.

[0091] The bars with dense hatching “ / / / / / / / ” show the respective contents of BHET, MHET and TS in the reactor output of the depolymerization of PET according to Example E1 of the invention, wherein the sodium glycolate used for the depolymerization was obtained by electrolysis.

[0092] The black bars show the respective contents of BHET, MHET and TS in the reactor output of the depolymerization of PET according to comparative example V1, wherein only ethylene glycol was used in the depolymerization.

[0093] The bars with thick hatching “ / / / / / ” show the respective contents of BHET, MHET and TS in the reactor output of the depolymerization of PET according to comparative example V2, wherein the sodium glycolate used for the depolymerization was obtained by mixing NaOH and ethylene glycol in the reactor. DETAILED DESCRIPTION

[0094] It has now been found that, surprisingly, the glycolysis of PET proceeds particularly efficiently when electrolytically obtained alkali metal glycolates, in particular sodium glycolate or potassium glycolate, are used. It has been observed that in the process according to the invention, a higher proportion of BHET is obtained in the cleavage product by comparison with the prior art process in which glycolates obtained by dissolving the corresponding alkali metal hydroxide in ethylene glycol are used.

[0095] 1. Step (a): electrolysis to obtain a mixture containing ethylene glycol and M A Hydroxyacetate solution L1

[0096] According to the present invention, in the electrolytic cell E <1> The method according to the present invention comprises ethylene glycol and M A Solution of glycolate L1.

[0097] "Ethylene glycol" in the context of the present invention is understood to mean ethylene-1,2-diol having the chemical formula HO-CH2-CH2-OH (CAS No. 107-21-1).

[0098] In the context of the present invention, “M A "Glycolate" is understood to mean a salt of ethylene glycol and M A The term "M A "Glycolic acid salt" covers MA O-CH2-CH2-OH and M A O-CH2-CH2-OM A At least one, preferably at least M A O-CH2-CH2-OH,

[0099] The most preferred is M A O-CH2-CH2-OH and M A O-CH2-CH2-OM A .

[0100] M A is an alkali metal cation, in particular selected from lithium, sodium, potassium, and preferably selected from sodium, potassium. Most preferably, the alkali metal cation is sodium.

[0101] 1.1 Electrolytic Cell E

[0102] The M used in step (b) of the method according to the invention A Hydroxyacetate solution in ethylene glycol L1 <21> is prepared in electrolytic cell E in step (a) of the process according to the invention.

[0103] The electrolytic cell E comprises at least one anode chamber K A and at least one cathode chamber K K , and optionally at least one intervening intermediate chamber K M This also includes electrolytic cells E which have more than one anode chamber K A and / or cathode chamber K K and / or intermediate chamber K M Such electrolysis cells are described, for example, in DD 258 143 A3 and US 2006 / 0226022 A1, in which the chambers are connected to one another in the form of modules.

[0104] In a preferred embodiment, the electrolytic cell E comprises an anode chamber K A and cathode chamber K K , and optionally an intervening intermediate chamber K M .

[0105] The electrolytic cell E generally has an outer wall W A The outer wall W A In particular, it is made of a material selected from the group consisting of steel (preferably rubberized steel), plastic (especially from (thermosetting polydicyclopentadiene), PVC (polyvinyl chloride), PVC-C (post-chlorinated polyvinyl chloride), PVDF (polyvinylidene fluoride). A In particular, it may be perforated for inlet and outlet. AInside is at least one anode chamber K A , at least one cathode chamber K K , in the embodiment in which the electrolytic cell E comprises one chamber, at least one intervening intermediate chamber K M .

[0106] 1.1.1 Cathode chamber K K

[0107] At least one cathode chamber K K Has at least one entry Z KK , at least one exit A KK , and comprising a cathode electrode E K Internal I KK .

[0108] If the electrolytic cell E does not contain an intermediate chamber K M , the anode chamber K A Internal I KA Through the partition wall W and the cathode chamber K K Internal I KK If the electrolytic cell E comprises at least one intermediate chamber K M , then the cathode chamber K K Internal I KK Through the partition wall W and the intermediate chamber K M Internal I KM Separation.

[0109] The dividing wall W and its arrangement in the electrolytic cell E are further described below (Section 1.1.4).

[0110] 1.1.1.1 Cathode Electrode E K

[0111] Cathode chamber K K Contains internal I KK , which in turn comprises a cathode electrode E K Such useful cathode electrodes E K is any electrode familiar to the person skilled in the art which is stable under the conditions of step (a) of the process according to the invention. These are described in particular in paragraph

[025] of WO 2014 / 008410 A1 or in paragraph

[030] of DE 10360758 A1. The electrode E K Can be selected from the group consisting of mesh wool, three-dimensional matrix structure and "ball". Cathode electrode E K In particular, it comprises a material selected from the group consisting of steel, nickel, copper, platinum, platinum-plated metal, palladium, carbon-supported palladium, and titanium, and more preferably selected from the group consisting of steel and nickel. K Preferably it comprises steel, even more preferably VA steel (= stainless steel).

[0112] In the electrolytic cell E (which contains the intermediate chamber K M ) in the embodiment, the intermediate chamber is located in the anode chamber K A and the cathode chamber K K between.

[0113] 1.1.1.2 Entrance Z KK and Exit A KK

[0114] The cathode chamber K K Also contains at least one entry Z KK and at least one exit A KK This enables the addition of liquid (e.g. solution L2) to the cathode chamber K K Internal I KK , and remove the liquid (such as solution L1) present therein. Here, inlet Z KK and Exit A KK So that the liquid flows through the cathode chamber K K Internal I KK When the cathode electrode E K The contact is connected to the cathode chamber K K When optionally also comprising M A A solution L2 of glycolate in ethylene glycol is led through the cathode chamber K K Internal I KK This is when the solution L1 is discharged at outlet A during step (a) of the method according to the invention. KK prerequisites obtained from the

[0115] Entrance Z KK and Exit A KK The addition to the electrolytic cell E can be carried out by methods known to the person skilled in the art, for example by means of holes in the outer wall and corresponding connections (valves) which simplify the introduction and discharge of liquids.

[0116] 1.1.2 Anode chamber K A

[0117] At least one anode chamber K A Has at least one entry Z KA , at least one exit A KA , and comprising an anode electrode E A Internal I KA .

[0118] If the electrolytic cell E contains an intermediate chamber K M , then the anode chamber K A Internal I KA Through the diffusion barrier D and the intermediate chamber K M Internal I KM Separation.

[0119] If the electrolytic cell E does not contain the intermediate chamber K M , then the internal I of the anode chamber K KA The cathode chamber K is separated from the cathode chamber K by a partition wall W. K Internal I KK Separation.

[0120] 1.1.2.1 Anode electrode E A

[0121] The anode chamber K A Contains internal I KA , which in turn comprises an anode electrode E A Such useful anode electrodes E A is any electrode familiar to the person skilled in the art which is stable under the conditions of step (a) of the process according to the invention. These are described in particular in paragraph

[024] of WO 2014 / 008410 A1 or in paragraph

[031] of DE 10360758 A1. The electrode E A The anode electrode E may consist of one layer or a plurality of mutually parallel planar layers which may be perforated or expanded. A In particular, it comprises a material selected from ruthenium oxide, iridium oxide, nickel, cobalt, nickel tungstate, nickel titanate, supported on a carrier such as titanium or A material of the group consisting of a noble metal such as, in particular, platinum on an iron / nickel / cobalt alloy (iron / nickel / cobalt alloy, wherein the individual components are preferably as follows: 54% by mass of iron, 29% by mass of nickel, 17% by mass of cobalt). Further possible anode materials are, in particular, stainless steel, lead, graphite, tungsten carbide, titanium diboride. Preferably, the anode electrode E A Contains a titanium anode coated with ruthenium oxide / iridium oxide (RuO2+IrO2 / Ti).

[0122] 1.1.2.2 Entrance Z KA and Exit A KA

[0123] Anode chamber K K Also includes entry Z KA and Exit A KA This enables the addition of liquid (e.g. solution L3) to the cathode chamber K A Internal I KA , and remove the liquid (such as solution L4) present therein. Here, inlet Z KA and Exit A KA So that the liquid flows through the anode chamber K A Internal I KA When the anode electrode E A The contact is connected to the anode chamber K A When the solution L3 of salt S is led through the anode chamber K A Internal I KAThis is when the solution L4 is discharged at outlet A during step (a) of the method according to the invention. KA prerequisites obtained from the

[0124] Entrance Z KA and Exit A KA The connection to the electrolytic cell E can be made by methods known to the person skilled in the art, for example by means of holes in the outer wall and corresponding connections (valves) which simplify the introduction and discharge of liquids. M In a particular embodiment, the inlet Z KA It is also possible within the electrolytic cell, for example in the form of perforations in the diffusion barrier D.

[0125] 1.1.3 Optional intermediate chamber K M

[0126] The electrolytic cell E used in step (a) of the process according to the invention optionally has at least one intermediate chamber K M Optional intermediate chamber K M Located in cathode chamber K K and anode chamber K A It contains at least one entrance Z KM , at least one exit A KM and internal I KM .

[0127] If the electrolytic cell E contains an intermediate chamber K M , then the anode chamber K A Internal I KA Through the diffusion barrier D and the intermediate chamber K M Internal I KM In that case, A KM Also by connecting V AM With entrance Z KA connection so that the liquid can flow from I KM , by connecting V AM Guide to I KA middle.

[0128] 1.1.3.1 Diffusion barrier D

[0129] Optional intermediate chamber K M Internal I KM Through the diffusion barrier D and the anode chamber K A Internal I KA Separated from the cathode chamber K by a partition wall W K Internal I KK Separation.

[0130] The material used for the diffusion barrier D may be any material which is stable under the conditions of step (a) of the method according to the invention and which prevents or delays the diffusion of protons from the anode chamber K. A Internal I KA The liquid present in the chamber is transferred to an optional intermediate chamber K M Internal I KM materials.

[0131] The diffusion barrier D used is in particular a non-ion-specific partition wall or a membrane permeable to specific ions. The diffusion barrier D is preferably a non-ion-specific partition wall.

[0132] The material of the non-ionic partition wall is in particular selected from the group consisting of a fabric (in particular a woven fabric or a metal braid), a glass (in particular a sintered glass or a glass frit), a ceramic (in particular a ceramic frit), a diaphragm, and is more preferably a woven fabric or a metal braid, and particularly preferably a woven fabric. The woven fabric preferably comprises a plastic, more preferably a plastic selected from the group consisting of PVC, PVC-C, polyvinyl ether ("PVE"), polytetrafluoroethylene ("PTFE").

[0133] If the diffusion barrier D is a "membrane permeable to specific ions", this means, according to the invention, that the respective membrane promotes the diffusion of specific ions therethrough in preference to other ions. More particularly, this means a membrane that promotes the diffusion of ions of a specific charge type therethrough in preference to ions of the opposite charge. Even more preferably, a membrane permeable to specific ions also promotes the diffusion of specific ions of one charge type therethrough in preference to other ions of the same charge type.

[0134] If the diffusion barrier D is a “membrane permeable to specific ions”, the diffusion barrier D is in particular an anion-conducting membrane or a cation-conducting membrane.

[0135] According to the present invention, anion-conducting membranes are those membranes that selectively conduct anions, preferably membranes that selectively conduct specific anions. In other words, they promote the diffusion of anions therethrough in preference to the diffusion of cations therethrough, in particular in preference to the diffusion of protons therethrough; even more preferably, they additionally promote the diffusion of specific anions therethrough in preference to the diffusion of other anions therethrough.

[0136] According to the invention, cation-conducting membranes are those that selectively conduct cations, preferably membranes that selectively conduct specific cations. In other words, they promote the diffusion of cations therethrough in preference to the diffusion of anions therethrough; even more preferably, they additionally promote the diffusion of specific cations therethrough in preference to the diffusion of other cations therethrough, still more preferably, the diffusion of cations that are not protons, more preferably sodium cations, therethrough in preference to the diffusion of protons therethrough.

[0137] More specifically, "favoring the diffusion of a particular ion X over the diffusion of other ions Y" means that at a given temperature, the diffusion coefficient (in m 2 / s) is 10 times, preferably 100 times, preferably 1000 times higher than the diffusion coefficient of ion type Y for the membrane in question.

[0138] If the diffusion barrier D is a "membrane permeable to certain ions", it is preferably an anion-conducting membrane, since this is particularly efficient in preventing protons from passing from the anode chamber K to the anode chamber K. A Diffusion to the intermediate chamber K M middle.

[0139] The anion-conducting membrane used is in particular a membrane that is selective for the anions contained in the salt S. Such membranes are known to the person skilled in the art and can be used. According to the invention, the salt S contains M A As a cation.

[0140] The salt S is preferably M A The invention further comprises a halide, sulfate, sulfite, nitrate, bicarbonate or carbonate of the present invention, and even more preferably a halide.

[0141] The halide is fluoride, chloride, bromide, iodide. The most preferred halide is chloride.

[0142] The anion-conducting membrane used is preferably a membrane which is selective for halides, preferably chlorides.

[0143] For example, MA Hickner, AMHerring, EB Coughlin, Journal of Polymer Science, Part B: Polymer Physics 2013, 51, 1727-1735, CGArges, V. Ramani, PN Pintauro, Electrochemical Society Interface 2010, 19, 31-35, in WO 2007 / 048712 A2, and Volkmar M. Schmidt, Elektrochemische Verfahrenstechnik: Grundlagen, Reaktionstechnik, Prozessoptimierung [Electrochemical Engineering: Fundamentals, Reaction Technology, Process Optimization], first edition (October 8, 2003) textbook, page 181 describes anion-conducting membranes.

[0144] Even more preferably, the anion-conducting membrane used is therefore an organic polymer, in particular selected from polyethylene, polybenzimidazole, polyetherketone, polystyrene, polypropylene and fluorinated membranes such as polyperfluoroethylene, preferably polystyrene, wherein these have a moiety selected from -NH3 + 、-NRH2 + 、-NR3 + , =NR + ;-PR3 + wherein R is an alkyl group preferably having 1 to 20 carbon atoms, or other cationic groups. They preferably have a group selected from -NH3 + 、-NRH2 + and-NR3 + , more preferably selected from -NH3 + and-NR3 + , even more preferably -NR3 + Covalently bonded functional groups.

[0145] When the diffusion barrier D is a cation-conducting membrane, it is particularly important for M A Even more preferably, the diffusion barrier D is an alkali metal cation conducting membrane, even more preferably a potassium and / or sodium ion conducting membrane, most preferably a sodium ion conducting membrane.

[0146] Cation-conducting membranes are described, for example, on page 181 of the textbook Volkmar M. Schmidt, Elektrochemische Verfahrenstechnik: Grundlagen, Reaktionstechnik, Prozessoptimierung, 1st edition (October 8, 2003).

[0147] Even more preferably, the cation-conducting membrane used is therefore an organic polymer, in particular selected from polyethylene, polybenzimidazole, polyetherketone, polystyrene, polypropylene and fluorinated membranes such as polyperfluoroethylene, preferably polystyrene and polyperfluoroethylene, wherein these carry a moiety selected from -SO3 - 、-COO - 、-PO3 2- and-PO2H - , preferably -SO3 - Covalently bonded functional groups (described in DE 102010 062 804A1, US Pat. No. 4,831,146).

[0148] This may be, for example, sulfonated polyperfluoroethylene (having CAS number: 31175-20-9 ). These are known to the person skilled in the art, for example from paragraph

[058] of WO 2008 / 076327 A1, paragraph

[0042] of US 2010 / 0044242 A1 or US 2016 / 0204459 A1, and are commercially available as For example, S.A. Mareev, D. Yu. Butylskii, N.D. Pismenskaya, C. Larchet, L. Dammak, V.V. Nikonenko, Journal of Membrane Science 2018, 563, 768-776 describes membrane.

[0149] If a cation-conducting membrane is used as diffusion barrier D, this may be, for example, a polymer functionalized with sulfonic acid groups, in particular a polymer of the formula P NAFION A polymer wherein n and m can independently be 1 to 10 6 An integer of 10 to 10 is preferred. 5 An integer of 10 is more preferred. 2 Up to 10 4 An integer.

[0150]

[0151] 1.1.3.2 Entrance Z KM and Exit A KM

[0152] Optional intermediate chamber K M Also includes entrance Z KM and Exit A KM This enables the addition of liquid (e.g. solution L3) to the intermediate chamber K M Internal I KM , and the liquid present therein (such as solution L3) is transferred to the anode chamber K A Internal I KA .

[0153] Entrance Z KM and Exit A KM The connection to the electrolytic cell E can be made by methods known to the person skilled in the art, for example by means of holes in the outer wall and corresponding connections (valves) which simplify the introduction and discharge of liquids. Outlet A KM It is also possible within the electrolytic cell, for example in the form of perforations in the diffusion barrier D.

[0154] 1.1.3.3 Connect V AM

[0155] In the electrolytic cell E used in step (a) of the process according to the invention, outlet A KM So that the liquid can be KM , by connecting VAM Guide to I KA In the way by connecting V AM With entrance Z KA connect.

[0156] The connection V AM It can be formed in the electrolytic cell E and / or outside the electrolytic cell E and is preferably formed in the electrolytic cell.

[0157] 1) If the connection V AM If the diffusion barrier D is formed in the electrolytic cell E, it is preferably formed by at least one perforation in the diffusion barrier D. This embodiment is preferred in particular when the diffusion barrier D used is a non-ion-specific partition wall, in particular a metal braid or a woven fabric. This serves as a diffusion barrier D and, due to the braided nature, has the function of serving as a connection V from the outset. AM perforations and gaps.

[0158] 2) In particular, when the diffusion barrier D used is a membrane permeable to specific ions, the embodiment described below is preferred: In this embodiment, the connection V AM Formed outside the electrolytic cell E, preferably by extending outside the electrolytic cell E KM and Z KA The connection is formed, especially because the outer wall W A Exit A KM The middle chamber K M Internal I KM and formed, preferably in the intermediate chamber K M The bottom of the inlet Z KM More preferably, in the middle chamber K M The top of the wall W A Entrance Z KA In the anode chamber K A Internal I KA is formed, preferably in the anode chamber K A The bottom of the outlet is formed, and these are connected by a conduit, such as a pipe or a hose (preferably comprising a material selected from rubber and plastic). KA It is more preferred that in the anode chamber K A top of.

[0159] "In the middle room K M The bottom outlet A KM ” means: Exit A KM So that the solution L3 leaves the intermediate chamber K in the direction of gravity. M Connect to electrolytic cell E in this way.

[0160] "In the anode chamber K A The bottom entrance Z KA" means: the entrance Z KA So that the solution L3 enters the anode chamber K in the opposite direction of gravity. A Connect to electrolytic cell E in this way.

[0161] "In the middle room K M The top entrance Z KM " means: the entrance Z KM So that the solution L3 enters the middle chamber K in the direction of gravity. M Connect to electrolytic cell E in this way.

[0162] "In the anode chamber K A Exit A at the top KA ” means: Exit A KA So that the solution L4 leaves the anode chamber K in the opposite direction of gravity. A This method is installed on the electrolytic cell E.

[0163] When exit A KM Through the outer wall W A In the middle room K M The bottom of the inlet Z KA Through the outer wall W A In the anode chamber K A This embodiment is particularly advantageous and therefore preferred when the bottom of the anode chamber K is formed. A The gases formed in the anode chamber K can be removed from the anode chamber K4 in a particularly simple manner. A Remove to separate them further. Figure 1B Such an embodiment is shown.

[0164] When connecting V AM When formed outside the electrolytic cell E, Z KM and A KM Especially arranged in the intermediate chamber K M The outer wall W A The opposite end (i.e., for example, Z KM At the bottom of electrolytic cell E and A KM at the top of the electrolytic cell E, or vice versa), and Z KA and A KA Arranged in the anode chamber K A The outer wall W A The opposite end (i.e. Z KA At the bottom of electrolytic cell E and A KA at the top of the electrolytic cell E, or vice versa), such as at Figure 1B By virtue of this geometry, L3 must flow through the two chambers K M and K A In this Z KA and ZKM may be formed on the same side of the electrolytic cell E, in which case A KM and A KA is also automatically formed on the same side of the electrolytic cell E. Alternatively, as in Figure 1B In the embodiment shown, Z KA and Z KM may be formed on the opposite side of the electrolytic cell E, in which case A KM and A KA It is then automatically formed on the opposite side of the electrolytic cell E as well.

[0165] 3) When the connection V AM This can be ensured in particular when formed in an electrolytic cell E, since one side of the electrolytic cell E (“side A”, which is the top or bottom of the electrolytic cell E, preferably as Figure 6B The top shown in FIG. 1 contains the inlet Z KM and Exit A KA , and the diffusion barrier D extends from this side ("A side") into the electrolytic cell E, but does not completely reach the side of the electrolytic cell E opposite to the A side ("B side", which is the bottom or top of the electrolytic cell E), and at the same time covers 50% or more of the height of the three-chamber cell E, preferably 60% to 99% of the height of the three-chamber cell E, more preferably 70% to 95% of the height of the three-chamber cell E, even more preferably 80% to 90% of the height of the three-chamber cell E, and more preferably 85% of the height of the three-chamber cell E. Because the diffusion barrier D does not contact the B side of the three-chamber cell E, the diffusion barrier D and the outer wall W of the B side of the three-chamber cell E are not completely covered. A In that case, the gap is the connection between V AM With this geometry, L3 must flow completely through both chambers K M and K A .

[0166] These embodiments optimally ensure that the salt water solution L3 is A Prior to contact, an acid-sensitive solid electrolyte flows through, which results in the formation of acid.

[0167] According to the present invention, the "bottom of the electrolytic cell E" is the bottom of the electrolytic cell E (e.g. Figure 1B A KM L3 in the case of Figure 1A , 1B , 6A and 6B KK In the case of L2, and in Figure 1A and 1B Z KA L3 in the case of ) is supplied to the side of the electrolytic cell E through it in the opposite direction of gravity.

[0168] According to the present invention, the "top end of the electrolytic cell E" is the top end of the electrolytic cell E (e.g. Figure 1A , 1B , 6A and 6B, in A KA In the case of L4 and in A KK L1 in the case of) in the opposite direction of gravity through the side of the electrolytic cell E through which it leaves, or the electrolytic cell E so that the solution (e.g. Figure 1B , 6A and Z in 6B KM L3 in the case of ) is supplied to the side of the electrolytic cell E through it in the same direction as gravity.

[0169] 1.1.3.4 Intermediate chamber K M Further embodiments of

[0170] In a preferred embodiment of the electrolytic cell E, the internal I KM Also comprises at least one additional feature selected from:

[0171] 1) internal components arranged such that they cause turbulence in the electrolyte L3;

[0172] 2) Mixing equipment;

[0173] 3) Additional introduction of an inert gas (for example nitrogen or a noble gas) via an additional inlet at the bottom end of the intermediate chamber and an additional outlet at the top end of the intermediate chamber. When the salt S is a carbonate or bicarbonate, it is also possible to introduce an inert gas (for example nitrogen or a noble gas) from the intermediate chamber via the additional inlet at the bottom end and the additional outlet at the top end of the intermediate chamber. KM Any gases formed (eg CO2) are removed.

[0174] By virtue of these additional preferred embodiments 1), 2) and 3), as the electrolyte L3 flows through I KM , eddies and turbulence are formed in the electrolyte L3. This further hinders the formation of a pH gradient in the intermediate chamber and thus prevents the ASC from being destroyed due to a too low pH. This increases the lifetime of the ASC.

[0175] 1.1.4 Partition wall W

[0176] The electrolytic cell E used in step (a) of the process according to the invention comprises a partition wall W. The partition wall W comprises at least one solid electrolyte ceramic F which conducts alkali metal cations. A In a preferred embodiment, the partition wall W is made of a solid electrolyte ceramic F that conducts alkali metal cations. A constitute.

[0177] In an alternative preferred embodiment of the present invention, the partition wall W comprises at least two alkali metal cation-conducting solid electrolyte ceramics ("alkali metal cation-conducting solid electrolyte ceramics" are abbreviated herein as "ASC") F, which are optionally separated from each other by a separation element T. A and F B .

[0178] The partition wall W has two sides S opposite to each other. KK and S A / MK , which means that the side S A / MK YesS KK The two sides S KK and S A / MK In particular, these include planes which are substantially parallel to one another.

[0179] The geometry of the dividing wall W is otherwise not further restricted and can be matched in particular to the cross section of the electrolytic cell E in which the dividing wall W is used. For example, it can have a cuboid geometry and thus a rectangular cross section, or a frustocone or cylindrical geometry and thus a circular cross section.

[0180] Optionally, the partition wall W can also have a cuboid geometry with rounded corners or projections (which in turn can have holes). The partition wall W then has projections ("rabbit ears"), via which the partition wall W can be fixed to the electrolytic cell or the frame parts of the partition wall W can be fixed to each other.

[0181] The side S of the partition wall W KK With surface O KK , and the side S of the partition wall W A / MK With surface O A / MK .

[0182] The feature "partition wall" means that the partition wall W is liquid-tight. Therefore, there is no liquid-tight partition wall through which an aqueous solution, an alcohol solution, an alcohol or water can pass from S KK Side flow to S A / MK The partition wall W comprises at least two solid electrolyte ceramics F that conduct alkali metal cations. A and F B and the optional separation element T, this means that F A and F B And at least one separating element T, if present, is adjacent to each other in a gap-free manner.

[0183] The dividing wall W usable in the electrolytic cell E in step (a) of the process according to the invention also encompasses embodiments in which the dividing wall W comprises more than two ASCs, for example four or nine or twelve ASCs, wherein the ASCs are directly adjacent to each other or separated from each other by separation elements T.

[0184] When the ASCs are directly adjacent to each other, however, this requires precise fitting of the respective adjacent ASCs to avoid the formation of gaps between them through which aqueous liquids or water or ethylene glycol or ethylene glycol solutions can flow from the SSCs. KK Side flow to S A / MK It is therefore advantageous and preferred that, when the partition wall W contains more than one ASC, all ASCs contained by the partition wall W are separated from each other by at least one separating element T in the partition wall W, which means that no ASC directly adjoins any other ASC, i.e. there is no separating element T in between.

[0185] The partition wall W is further characterized in that: the ASC F A Via surface O KK and through the surface O A / MK The two can be in direct contact. Wherein the partition wall W comprises at least two ASC F A 、F B In the embodiment of the present invention, it is preferred that all ASCs contained in the partition wall W are connected to the partition wall through the surface O KK and through the surface O A / MK The two can be in direct contact.

[0186] The term “directly contactable” with respect to the ASC contained in the partition wall W means that the surface O KK and O A / MK At least a portion of the ASC is formed by the surface of the ASC included in the partition wall W, which means that the ASC included in the partition wall W is formed on both surfaces O KK and O A / MK directly accessible, so that they can be found on both surfaces O KK and O A / MK The area is wetted with, for example, an aqueous solution, a glycol solution, ethylene glycol or water.

[0187] The arrangement of the ASCs in the partition wall W means that for each ASC contained in the partition wall W, there is a KK Side surface O KK To S A / MK Side surface O A / MK pathway that is directed entirely through the corresponding ASC.

[0188] When the partition wall W has at least one separating element T, the at least one separating element T is usually also formed via the surface O KKat least a portion of and through the surface O A / MK At least a portion of may be in direct contact.

[0189] “Directly contactable” in relation to the at least one separating element T optionally contained in the partition wall W means that: the surface O KK and O A / MK A part of the separation element T is formed by the surface of the separation element T, which means that the separation element T has two surfaces O KK and O A / MK directly accessible, so that the separation element T can be KK and O A / MK The area is wetted with, for example, an aqueous solution, an alcoholic solution, alcohol or water.

[0190] In particular with regard to the arrangement of the optional separating elements T in the partition wall W, this means that for the separating elements T optionally contained in this partition wall W, there are KK Side surface O KK To S A / MK Side surface O A / MK A path which leads through the separation element T and optionally through the seal Di, but not through the ASC.

[0191] In a preferred embodiment of the partition wall W, the surface O A / MK At least 50%, more preferably at least 60%, even more preferably at least 70%, even more preferably at least 85% of the ASC is formed by the ASC comprised by the partition wall W.

[0192] In a preferred embodiment of the partition wall W, the surface O KK At least 50%, more preferably at least 60%, even more preferably at least 70%, even more preferably at least 85% of the ASC is formed by the ASC comprised by the partition wall W.

[0193] In the embodiment in which the partition wall W has more than one ASC, in particular, the surface O KK 50% to 99%, more preferably at least 60% to 96%, even more preferably 70% to 92%, even more preferably 85% to 90% is formed by the ASC contained in the partition wall W. KK The remainder of the surface O is even more preferably formed by the separating element T and the optional frame element R. At the same time, in the embodiment in which the partition wall W has more than one ASC, in particular, the surface O A / MK 50% to 99%, more preferably at least 60% to 96%, even more preferably 70% to 92%, even more preferably 85% to 90% is formed by the ASC contained in the partition wall W. A / MK The remainder of is even more preferably formed by a separating element T and an optional frame element R.

[0194] In a preferred embodiment, the partition wall W <16> Solid electrolyte ceramics containing conductive alkali metal cations F A and optionally a frame element R. Even more preferably, the partition wall W <16> Solid electrolyte ceramics F that conduct alkali metal cations A constitute.

[0195] In another preferred embodiment, the partition wall W comprises at least four ASC F A 、F B 、F C and F D , and even more preferably contains exactly four ASIC F A 、F B 、F C and F D .

[0196] In a further preferred embodiment, the partition wall W comprises at least nine ASC F A 、F B 、F C 、F D 、F E 、F F 、F G 、F H and F I , and even more preferably contains exactly nine ASCII A 、F B 、F C 、F D 、F E 、F F 、F G 、F H and F I .

[0197] In a further preferred embodiment, the partition wall W comprises at least twelve ASC F A 、F B 、F C 、F D 、F E 、F F 、F G 、F H 、F I 、F J 、F K and F L , and even more preferably contains exactly twelve ASIC F A 、F B 、F C 、F D 、F E 、F F 、FG 、F H 、F I 、F J 、F K and F L .

[0198] The arrangement of at least two ASCs next to each other in the partition wall W leads to an advantage over the arrangement of only one ASC, namely the further expansion direction of the ASC in the event of temperature fluctuations occurring in the operation of the electrolytic cell. The NaSICON sheets serving as partition walls are bound in the electrolytic cell by the outer wall of the electrolytic cell or by a solid plastic frame. It is not possible to dissipate mechanical stresses in this way, which would occur in the event of expansion within the NaSICON, which could lead to cracking of the ceramic.

[0199] In contrast, each ASC within the partition wall W is preferably adjacent to a separation element T, which results in two beneficial effects, both of which increase the long-term stability of the ASC:

[0200] - Each ASC has a further degree of freedom available, i.e. the dimension in which it can expand. As well as expansion in the z-direction (i.e. beyond the thickness of the ceramic sheet at right angles to the plane of the partition wall W), expansion in the x and / or y-directions is now also possible, i.e. horizontally and vertically in the plane of the partition wall W. This expansion direction does not exist or is at least greatly restricted when the ASC, for example as a solid sheet, spans the cross section of the electrolytic cell and abuts the solid wall of the electrolytic cell.

[0201] - Compared to a partition wall of equal size consisting of only one ASC, the partitioning into a plurality of small ASCs has the effect that the stresses occurring in the smaller ASCs are also smaller in absolute terms, can be dissipated more quickly and therefore stresses which would rupture the ASC cannot build up quickly.

[0202] As a result, the tendency of the "separated" ASCs in the partition wall W to rupture is significantly reduced compared to using one piece.

[0203] 1.1.4.1 Alkali metal cation-conducting solid electrolyte ceramics "ASC"

[0204] The partition wall W contains a useful solid electrolyte ceramic F that conducts alkali metal cations. A 、F B is any solid electrolyte through which cations (especially alkali metal cations, even more preferably sodium cations) can be transferred from S A / MK Side conveyor to S KKside. Such solid electrolytes are known to the skilled person and are described, for example, in DE 10 2015 013 155 A1, WO 2012 / 048032 A2, paragraphs

[0035] ,

[0039] ,

[0040] , US 2010 / 0044242 A1, paragraphs

[0040] ,

[0041] , DE 10360758 A1, paragraphs

[014] to

[025] . They are sold commercially under the names NaSICON, LiSICON, KSICON. Sodium-ion-conducting solid electrolytes are preferred, and this even more preferably has a NaSICON structure. NaSICON structures usable according to the invention are also described, for example, by N. Anantharamulu, K. Koteswara Rao, G. Rambabu, B. Vijaya Kumar, Velchuri Radha, M. Vithal, J Mater Sci 2011, 46, 2821-2837.

[0205] In a preferred embodiment of the partition wall W, the partition wall W comprises a solid electrolyte ceramic that conducts alkali metal cations, and in particular, an ASH F A Independently having the formula M I 1+2w+x-y+z M II w M III x Zr IV 2-w-x-y M V y (SiO4) z (PO4) 3-z The NaSICON structure.

[0206] M I Select Na + , Li + , preferably Na + .

[0207] M II Here is a divalent metal cation, preferably selected from Mg 2+ , Ca 2+ , Sr 2+ , Ba 2+ 、Co 2+ 、Ni 2+ , more preferably selected from Co 2+ 、Ni 2+ .

[0208] M III Here is a trivalent metal cation, preferably selected from Al 3+ , Ga 3+Sc 3+ ,La 3+ , Y 3+ , Gd 3+ 、Sm 3+ 、Lu 3+ , Fe 3 + Cr 3+ , more preferably selected from Sc 3+ ,La 3+ , Y 3+ , Gd 3+ 、Sm 3+ , particularly preferably selected from Sc 3+ , Y 3+ ,La 3+ .

[0209] M V Here is a pentavalent metal cation, preferably selected from V 5+ , Nb 5+ 、 5+ .

[0210] The Roman numerals I, II, III, IV, V indicate the oxidation number of the corresponding metal cation present therein. w, x, y, z are real numbers, where 0≤x<2, 0≤y<2, 0≤w<2, 0≤z<3,

[0211] And wherein w, x, y, z are selected such that 1+2w+x-y+z≥0 and 2-wxy≥0.

[0212] Even more preferably according to the present invention, the NaSICON structure has the formula Na (1+v) Zr2Si v P (3–v) O 12 The structure of , where v is a real number, for which 0≤v≤3. Most preferably, v=2.4.

[0213] In the partition wall W (which comprises at least two ASC F A 、F B ), all ASCs contained in the partition wall W have the same structure.

[0214] 1.1.4.2 Separation Component T

[0215] In the partition wall W of the present invention (wherein it comprises at least two ASC F A 、F B ), the partition wall W preferably comprises a separation element T. In that case, according to the present invention, the separation element T separates at least two solid electrolyte ceramics F conducting alkali metal cations contained in the partition wall W. A and FB , which means that it is inserted into the partition wall W containing at least two solid electrolyte ceramics F conducting alkali metal cations. A and F B between.

[0216] A suitable separating element T, which is preferably contained by the dividing wall W, is any object by means of which the respective ASCs can be arranged separated from one another. The ASCs are adjacent to the separating element T without gaps in order not to impair the function of the dividing wall, which in the electrolytic cell E is to separate the cathode chamber from the adjacent intermediate chamber or anode chamber in a liquid-tight manner.

[0217] The shape of the separation element T can be selected by those skilled in the art according to the number of ASCs contained in the partition wall W in the preferred embodiment.

[0218] For example, if the partition wall W comprises two or three ASCs, these may each be separated by a land disposed between the ASCs to serve as a separation element T.

[0219] If the partition wall W comprises four or more ASCs, these may be separated by separating elements T in the form of a cross or a grid.

[0220] In the partition wall W of the present invention (wherein it comprises at least two ASC F A 、F B ), it is particularly preferred that the partition wall W comprises at least four ASCs, and even more preferred that the separation element T in that case is in the form of a cross or a grid, since this then ensures that all three dimensions are fully available to the ASCs for thermal expansion / contraction.

[0221] The separation element T can here consist of one piece. In that case, the ASC is fixed to the separation element T without gaps, for example by means known to the person skilled in the art, for example by means of an adhesive, preferably using epoxy resins, phenolic resins. Alternatively or additionally, the separation element T can also be shaped such that the corresponding ASC can be assembled or clamped into the separation element. This can already be implemented in a corresponding manner in the production of the partition wall W.

[0222] In a preferred embodiment in which the partition wall W comprises a separation element, this comprises in particular a seal Di between the separation element T and the ASC. Figure 3B , 3C ). This ensures that the partition wall W is liquid-tight in a particularly effective manner. The seal Di can be selected by a person skilled in the art for the corresponding ASC or the corresponding separation element T.

[0223] The seal Di contains, in particular, a material selected from the group consisting of an elastomer and an adhesive, preferably an elastomer.

[0224] Useful elastomers are especially rubbers, preferably ethylene-propylene-diene rubber ("EPDM"), fluoropolymer rubber ("FPM"), perfluoropolymer rubber ("FFPM"), acrylonitrile-butadiene rubber ("NBR").

[0225] In a further preferred embodiment, the separation element T comprises at least two parts T1 and T2 which can be fixed to each other and thus sandwich the ASC therebetween.

[0226] In this embodiment, it is then particularly preferred to install a seal Di between the separation element T and the ASC in order to ensure liquid tightness.

[0227] The separation element T preferably comprises a material selected from the group consisting of plastic, glass, wood. More preferably, the separation element T consists of plastic.

[0228] Even more preferably, the plastic is a plastic selected from the group consisting of polypropylene, polystyrene, polyvinyl chloride, post-chlorinated polyvinyl chloride ("PVC-C").

[0229] 1.1.4.3 Frame element R

[0230] In a further preferred embodiment, the partition wall W also comprises a frame element R. The frame element R differs from the separating element T in that it is not arranged between the alkali metal cation-conducting solid electrolyte ceramics contained in the partition wall W, i.e. does not separate these from one another. The frame element R in particular at least partially, preferably completely, delimits the surface O KK and O A / MK This means more particularly that the frame element R at least partially, preferably completely, surrounds the surface O KK and O A / MK .

[0231] The frame element R may or may not be a surface O KK and O A / MK The frame element R is preferably a surface O KK and O A / MK part.

[0232] The frame element R is in particular directly contactable or accessible via a surface O KK and O A / MK Rather than being directly contactable, it is preferably directly contactable.

[0233] “Not directly contactable” with respect to the frame element R optionally included in the partition wall W means that the frame element R is formed only as a part of the partition wall W and not as a side element. KK and S A / MKMore particularly, the frame element R in that case forms the partition wall W which is not the side S KK and S A / MK At least 1%, more preferably at least 25%, more preferably at least 50%, even more preferably 100% of the surface area of ​​the side.

[0234] “Directly contactable” in relation to the frame element R optionally included in the partition wall W means that the surface O KK and O A / MK A part of the partition wall W is formed by the surface of the frame element R, which means that the frame element R included in the partition wall W is formed on both surfaces O KK and O A / MK directly accessible, so that it can be directly accessible on both surfaces O KK and O A / MK The area is wetted with, for example, an aqueous solution, an alcoholic solution, alcohol or water.

[0235] With regard to the arrangement of the frame elements R in the partition wall W, this means that: then there is a KK Side surface O KK To S A / MK Side surface O A / MK Path, which is guided entirely through frame element R.

[0236] This includes the following implementations:

[0237] -Surface O KK and O A / MK A portion of the edge of Figure 4B , 4D displayed);

[0238] -Surface O KK and O A / MK The edge of Figure 4A , 4C , 7A, and 7B).

[0239] In this case, the frame element R may also be formed as a partition wall W instead of as a side S. KK and S A / MK More particularly, the frame element R forms at least a portion of the surface of those sides of the partition wall W which are not the sides S. KK and S A / MK At least 1%, more preferably at least 25%, more preferably at least 50%, even more preferably 100% of the surface area of ​​the side.

[0240] Figure 4B and Figure 4D For example, a plurality of embodiments are shown in which the frame element R forms a partition wall W other than the side S. KKand S A / MK at least a portion of the surfaces of those sides.

[0241] Figure 4A and Figure 4C For example, embodiments are shown in which the frame element R completely forms the partition wall W without forming the side S KK and S A / MK of the surfaces of those sides.

[0242] The frame element R is made of a material selected from the group consisting of plastic, glass, wood. More preferably, the frame element R is made of plastic.

[0243] Even more preferably, the plastic is a plastic selected from the group consisting of polypropylene, polystyrene, polyvinyl chloride, PVC-C.

[0244] In a further preferred embodiment, when the partition wall W comprises a separation element T and a frame element R, the frame element R and the separation element T are made of the same material, even more preferably both are made of plastic, which is even more preferably selected from polypropylene, polystyrene, polyvinyl chloride, PVC-C.

[0245] The frame element R can here consist of one piece. In that case, the ASC is fixed to the frame element R without play, for example by means known to the person skilled in the art, for example by means of an adhesive, for which epoxy resins and phenolic resins are particularly suitable. Alternatively or additionally, the frame element R can also be shaped such that the corresponding ASC can be fitted or clamped into the frame element R.

[0246] This also means that: in which the partition wall W contains at least two ASC F A 、F B In a preferred embodiment of the ASC, the at least one separating element T and the frame element R, the ASC, the at least one separating element T and the frame element R are adjacent to one another in a gap-free manner.

[0247] Therefore, there is no gap between the separation element T, the frame element R and the ASC contained in the partition wall W through which ethylene glycol, ethylene glycol solution, aqueous solution or water can flow from S to KK Side flow to S A / MK side or vice versa).

[0248] Furthermore, especially when the partition wall W comprises at least two ASC F A 、F B, frame element R and at least one separating element T, and the frame element R and at least one separating element T are at least partially in one piece with each other, the frame element R can be composed of at least two parts, which are fixed to each other and sandwich the ASC between them. For example, the partition wall W can have a hinge, by which the two parts of the frame element R can be opened and closed. In addition, the partition wall W can have a lock, by which the two parts of the frame element R can be locked in place in the closed state ( Fig. 7A ).

[0249] In the closed state, the ASC and (if it is not in one piece with the frame element R) the separating element T may then be clamped between two parts of the frame element R. In this embodiment, a seal may then be installed between the separating element T and the ASC or between the frame element R and the ASC to ensure liquid tightness.

[0250] In a preferred embodiment, when the partition wall W comprises at least two ASC F A 、F B , a frame element R and at least one separating element T, at least a portion of the separating element T is in one piece with at least a portion of the frame element R. More particularly, this means that at least a portion of the separating element T is incorporated into the frame element R in that case.

[0251] Preferably, the at least one separating element T and the frame element R are then in one piece.

[0252] The embodiment of the frame element R has the advantage that it can serve as part of the outer wall during assembly of the electrolytic cell E. This part of the partition wall W does not intersect with the corresponding inner wall. KK ,I KA or I KM The solution is contacted with at least one solid electrolyte ceramic F A In addition, the portion of the partition wall W sandwiched between the outer walls or forming part of it is subjected to pressure, which makes the brittle solid electrolyte ceramic F A Instead, a breakage-resistant and cheaper material is therefore selected for the frame R.

[0253] 1.1.4.4 Fabrication of partition wall W

[0254] The partition wall W can be produced by methods known to those skilled in the art.

[0255] The partition wall W utilized in the embodiment of the method according to the invention may be an ASC F cut or formed by methods known to those skilled in the art. A .

[0256] If the partition wall W comprises a frame element R or at least one separating element T, the ASC contained by the partition wall (optionally together with a seal) can be placed in a casting mold and the separating element can be cast using liquid plastic and then solidified (injection molding method). During the solidification process, this then surrounds the ASC.

[0257] Alternatively, the separation element T is cast separately (or partially) and then fixed to the at least two ASCs in a gap-free manner (eg adhesively).

[0258] 1.1.4.5 Arrangement of the dividing wall W in the electrolytic cell E

[0259] 1) The partition wall W is formed so that the solid electrolyte ceramic F containing the partition wall W conducts alkali metal cations. A With S KK Side interior I KK Via surface O KK This type of direct contact is arranged in electrolytic cell E.

[0260] When the partition wall W contains at least two ASC F A ,F B , at least one separating element T and an optionally present frame element R, the partition wall W is arranged in the electrolytic cell E so that the solid electrolyte ceramic F conducting alkali metal cations contained in the partition wall W A and F B , and preferably also a separation element T via the surface O KK With S KK Side interior I KK Direct contact.

[0261] This means that the partition wall W is arranged in the electrolytic cell E so that when S KK Side interior I KK When the solution L2 is completely filled, the solution L2 flows through the surface O KK At least the solid electrolyte ceramic F that conducts alkali metal cations contained in the partition wall W A contact, so that from F A Ions (e.g., alkali metal ions, such as sodium and lithium) can enter the solution L2.

[0262] When the partition wall W comprises at least two ASC F A 、F B , at least one separating element T and optionally a frame element R, this means that the partition wall W is arranged in the electrolytic cell E so that when S KK Side interior I KK When the solution L2 is completely filled, the solution L2 flows through the surface O KKAt least two solid electrolyte ceramics F conducting alkali metal cations included in the partition wall W A and F B contact, and preferably also contact with the separation element T, so that the A and F B Ions (e.g., alkali metal ions, such as sodium and lithium) can enter the solution L2.

[0263] 2) In addition, the electrolytic cell E does not contain an intermediate chamber K M In the embodiment of the present invention, the partition wall W is arranged in the electrolytic cell E so that the solid electrolyte ceramic F conducting alkali metal cations contained in the partition wall W A With S A / MK Side interior I KA Via surface O A / MK Direct contact.

[0264] When the partition wall W contains at least two ASC F A ,F B , at least one separating element T and optionally a frame element R, and when the electrolytic cell E does not contain an intermediate chamber K M This means that the partition wall W is arranged in the electrolytic cell E so that the solid electrolyte ceramic conducting alkali metal cations contained in the partition wall W and preferably also the separation element T are connected via the surface O A / MK With S A / MK Side interior I KA Direct contact.

[0265] This means the following: in which the electrolytic cell E does not contain an intermediate chamber K M In the embodiment, the partition wall W and the anode chamber K A Internal I KA Adjacent.

[0266] In these embodiments, the dividing wall W is then arranged in the electrolytic cell E so that when S A / MK Side interior I KA When the solution L3 is completely filled, the solution L3 flows through the surface O A / MK At least the solid electrolyte ceramic F that conducts alkali metal cations contained in the partition wall W A contact, so that ions from solution L4 (e.g., alkali metal ions such as sodium and lithium) can enter ASCF A .

[0267] When the partition wall W comprises at least two ASC F A 、F B , at least one separating element T and optionally a frame element R, this means that the partition wall W is arranged in the electrolytic cell E so that when S A / MKSide interior I KA When the solution L3 is completely filled, the solution L3 flows through the surface O A / MK At least two solid electrolyte ceramics F conducting alkali metal cations included in the partition wall W A and F B and preferably also in contact with a separation element T so that ions from solution L3 (e.g., alkali metal ions such as sodium, lithium) can enter the ASC F A and F B .

[0268] 3) In addition, the electrolytic cell E comprises at least one intermediate chamber K M In the case of the present invention, the partition wall W is arranged in the electrolytic cell E so that the solid electrolyte ceramic F containing the partition wall W that conducts alkali metal cations A With S A / MK Side interior I KM Via surface O A / MK Direct contact.

[0269] When the partition wall W contains at least two ASC F A ,F B , at least one separating element T and optionally a frame element R, and when the electrolytic cell E comprises at least one intermediate chamber K M This means that the partition wall W is arranged in the electrolytic cell E so that the solid electrolyte ceramic conducting alkali metal cations contained in the partition wall W and preferably also the separation element T are connected via the surface O A / MK With S A / MK Side interior I KM Direct contact.

[0270] This means the following: in which the electrolytic cell E comprises at least one intermediate chamber K M In the embodiment of the present invention, the partition wall W and the intermediate chamber K M Internal I KM Adjacent.

[0271] In these embodiments, the dividing wall W is then arranged in the electrolytic cell E so that when S A / MK Side interior I KM When the solution L3 is completely filled, the solution L3 flows through the surface O A / MK At least the solid electrolyte ceramic F that conducts alkali metal cations contained in the partition wall W A contact, so that ions from solution L3 (e.g., alkali metal ions such as sodium and lithium) can enter ASCF A .

[0272] When the partition wall W comprises at least two ASC F A 、F B, at least one separating element T and optionally a frame element R, this means that the partition wall W is arranged in the electrolytic cell E so that when S A / MK Side interior I KM When the solution L3 is completely filled, the solution L3 flows through the surface O A / MK At least two solid electrolyte ceramics F conducting alkali metal cations included in the partition wall W A and F B and preferably also in contact with a separation element T so that ions from solution L3 (e.g., alkali metal ions such as sodium, lithium) can enter the ASC F A and F B .

[0273] In a preferred embodiment of electrolytic cell E, the surface O formed by ASC KK At least 50%, especially at least 70%, preferably at least 90%, most preferably 100% of the portion of the inner KK touch.

[0274] In a preferred embodiment of the electrolytic cell E without an intermediate chamber, the surface O formed by the ASC A / MK At least 50%, especially at least 70%, preferably at least 90%, most preferably 100% of the portion of the inner KA touch.

[0275] In a preferred embodiment of the electrolytic cell E having at least one intermediate chamber, the surface O formed by the ASC A / MK At least 50%, especially at least 70%, preferably at least 90%, most preferably 100% of the portion of the inner KM touch.

[0276] 1.2 Step (a) of the method according to the invention

[0277] Step (a) of the method according to the invention involves A Preparation of a solution L1 of glycolate in ethylene glycol, wherein M A is an alkali metal cation. The method is carried out in an electrolytic cell E.

[0278] M A Preferably selected from Li + , K + , Na, more preferably K + 、Na + Most preferably, M A =Na + .

[0279] 1.2.1 Without intermediate chamber K M The electrolytic cell E of the method according to the invention

[0280] In which the electrolytic cell E does not contain an intermediate chamber K M In the case of , steps (α1), (α2), and (α3) are performed simultaneously.

[0281] 1.2.1.1 Step (α1)

[0282] In step (α1), a mixture containing ethylene glycol (preferably containing an alkali metal glycolate M A A solution L2 of glycolate and ethylene glycol is introduced through I KK .

[0283] Solution L2 is preferably free of water. According to the present invention, "free of water" means that the weight (mass ratio) of water in solution L2 is ≤1:10, more preferably ≤1:20, even more preferably ≤1:100, even more preferably ≤0.5:100, even more preferably ≤1:1000, even more preferably ≤1:10 000, based on the weight of ethylene glycol in solution L2.

[0284] If solution L2 contains M A Hydroxyacetate, based on total solution L2, M A The mass proportion of glycolate in solution L2 is in particular >0 to 30% by weight, preferably 0.1 to 20% by weight, more preferably 0.2 to 10% by weight, more preferably 0.5 to 5% by weight, most preferably 0.7 to 2% by weight, most preferably 1% by weight.

[0285] If solution L2 contains M A Hydroxyacetate, then in solution L2, M A The mass ratio of glycolate to ethylene glycol is especially in the range of 1:1000 to 1:5, more preferably in the range of 1:250 to 3:20, even more preferably in the range of 1:120 to 1:8, even more preferably 1:100.

[0286] 1.2.1.2 Step (α2)

[0287] In step (α2), the A A neutral or alkaline aqueous solution L3 of a salt S as a cation is introduced through I KA .

[0288] The salt S is preferably M A The invention further comprises a halide, sulfate, sulfite, nitrate, bicarbonate or carbonate of the present invention, and even more preferably a halide.

[0289] The halide is fluoride, chloride, bromide, iodide. The most preferred halide is chloride.

[0290] The pH of the aqueous solution L3 is ≥ 7.0, preferably in the range of 7 to 12, more preferably in the range of 8 to 11, even more preferably 10 to 11, most preferably 10.5.

[0291] The mass proportion of salt S in aqueous solution L3, based on the total solution L3, is preferably in the range of >0 wt % to 20 wt %, preferably 1 wt % to 20 wt %, more preferably 5 wt % to 20 wt %, even more preferably 10 wt % to 20 wt %, most preferably 20 wt %.

[0292] 1.2.1.3 Step (α3)

[0293] In step (α3), in E A and E K Apply voltage between.

[0294] This results in a current from the charge source to the anode, charge via the ions to the cathode and finally current back to the charge source. The charge source is known to those skilled in the art and is typically a rectifier which converts alternating current into direct current and can generate a specific voltage via a voltage transformer.

[0295] This in turn has the following consequences:

[0296] At Exit A KK Solution L1, M A The concentration of glycolate was higher in L1 than in L2.

[0297] At Exit A KA An aqueous solution of S L4 is obtained, and the concentration of S in L4 is lower than that in L3.

[0298] In step (α3) of the method according to the invention, in particular, a voltage is applied such that a current flows whose current density (= current supplied to the electrolytic cell versus I KA The ratio of the area of ​​the anolyte in contact with the solid electrolyte is between 10 and 8000 A / m 2 In the range of 100 to 2000 A / m 2 In the range of 300 to 800 A / m 2 and even more preferably 494 A / m 2 This can be determined by a person skilled in the art in a standard manner. A Internal I KA The area of ​​the solid electrolyte in contact with the anolyte present is in particular 0.00001 to 10 m 2 , preferably 0.0001 to 2.5 m 2 , more preferably 0.0002 to 0.15 m 2 , even more preferably 2.83m2 .

[0299] It is obvious that step (α3) of the method according to the invention is carried out in the anode chamber K A Internal I KA At least partially accommodates L3 and the cathode chamber K K Internal I KK The at least partial accommodation of L2 is carried out such that both L3 and L2 are in contact with the ASC contained by the partition wall W and in particular also with the separating element T when the partition wall W contains an ASC.

[0300] In step (α3) occurs at E A and E K The fact of charge transfer between KK and I KA At the same time, L2 and L3 are accommodated separately so that they cover the electrode E K / E A to the extent that the circuit is completed.

[0301] In particular, the flow in L3 is continuously directed through I KA And the liquid flow of L2 passes through I KK , and the liquid flow of L3 at least partially, preferably completely covers the electrode E A The liquid flow of L2 at least partially, preferably completely covers the electrode E K This is the situation.

[0302] In a further preferred embodiment, the method according to the invention is carried out continuously, ie step (α1) and step (α2) are carried out continuously, while a voltage is applied according to step (α3).

[0303] After implementing step (α3), at outlet A KK Solution L1, M A The concentration of glycolate is higher in L1 than in L2. If L2 already contains M A Hydroxyacetate, then M in L1 A The concentration of glycolate is preferably 1.01 to 200.2 times higher than in L2, more preferably 5.04 to 100.8 times, even more preferably 10.077 to 50.4 times, even more preferably 18.077 to 20.08 times, most preferably 20.00 times higher than in L2, wherein M A The mass proportion of glycolate in L1 and in L2 is more preferably in the range of 0.1% to 50% by weight, even more preferably 1% to 20% by weight.

[0304] At Exit A KA An aqueous solution of S L4 is obtained, and the concentration of S in L4 is lower than that in L3.

[0305] In aqueous solution L3, cation M A The concentration of the cation M in the aqueous solution L4 is preferably in the range of 0.5 to 5 mol / l, more preferably 1 mol / l. A The concentration is more preferably 0.5 mol / l lower than in the aqueous solution L3 used in each case.

[0306] More particularly, steps (α1) to (α3) according to the present invention are carried out at a temperature of 20°C to 110°C, preferably 50°C to 105°C, more preferably 80°C to 99°C, even more preferably 90°C to 95°C and a pressure of 0.5 bar to 1.5 bar, preferably 0.9 bar to 1.1 bar, more preferably 1.0 bar.

[0307] During the implementation of steps (α1) to (α3) of the method according to the present invention, hydrogen is usually KK It can be formed through outlet A KK , removed from the cell together with solution L1. In a particular embodiment of the invention, the mixture of hydrogen and solution L1 can then be separated by methods known to those skilled in the art. When the alkali metal compound used is a halide (especially a chloride), chlorine or another halogen gas may be present in the cell. KA and the gas can be formed together with the solution L4 through the outlet A KK Remove from the pool.

[0308] In addition, it is also possible to form oxygen and / or carbon dioxide which can be removed in the same manner. In a particular embodiment of the present invention, the mixture of chlorine, oxygen and / or CO2 and solution L4 can then be separated by methods known to those skilled in the art. After chlorine, oxygen and / or CO2 gases have been separated from solution L4, it is also possible to separate these by methods known to those skilled in the art.

[0309] 1.2.2 In the case of a system with an intermediate chamber K M The electrolytic cell E of the method according to the invention

[0310] The electrolytic cell E comprises at least one intermediate chamber K M In the case of , steps (β1), (β2), and (β3) are performed simultaneously.

[0311] Preferably, the electrolytic cell E comprises at least one intermediate chamber K M , and then perform steps (β1), (β2), (β3) simultaneously.

[0312] 1.2.2.1 Step (β1)

[0313] In step (β1), a mixture containing ethylene glycol (preferably containing an alkali metal glycolate M Aand ethylene glycol) solution L2 is guided through I KK .

[0314] Solution L2 is preferably free of water. According to the present invention, "free of water" means that the weight (mass ratio) of water in solution L2 is ≤1:10, more preferably ≤1:20, even more preferably ≤1:100, even more preferably ≤0.5:100, based on the weight of ethylene glycol in solution L2.

[0315] If solution L2 contains M A Hydroxyacetate, based on total solution L2, M A The mass proportion of glycolate in solution L2 is in particular >0 to 30% by weight, preferably 0.1 to 20% by weight, more preferably 0.2 to 20% by weight, more preferably 0.5 to 5% by weight, most preferably 0.7 to 2% by weight, most preferably 1% by weight.

[0316] If solution L2 contains M A Hydroxyacetate, then in solution L2, M A The mass ratio of glycolate to ethylene glycol is especially in the range of 1:1000 to 1:5, more preferably in the range of 1:250 to 3:20, even more preferably in the range of 1:120 to 1:8, even more preferably 1:100.

[0317] 1.2.2.2 Step (β2)

[0318] In step (β2), the A A neutral or alkaline aqueous solution L3 of a salt S as a cation is introduced through I KM , then through V AM , then through I KA .

[0319] The salt S is preferably M A The invention further comprises a halide, sulfate, sulfite, nitrate, bicarbonate or carbonate of the present invention, and even more preferably a halide.

[0320] The halide is fluoride, chloride, bromide, iodide. The most preferred halide is chloride.

[0321] The pH of the aqueous solution L3 is ≥ 7.0, preferably in the range of 7 to 12, more preferably in the range of 8 to 11, even more preferably 10 to 11, most preferably 10.5.

[0322] The mass proportion of salt S in aqueous solution L3, based on the total solution L3, is preferably in the range of >0 wt % to 20 wt %, preferably 1 wt % to 20 wt %, more preferably 5 wt % to 20 wt %, even more preferably 10 wt % to 20 wt %, most preferably 20 wt %.

[0323] 1.2.2.3 Step (β3)

[0324] In step (β3), in E A and E K Apply voltage between.

[0325] This results in a current from the charge source to the anode, charge via the ions to the cathode and finally current back to the charge source. The charge source is known to those skilled in the art and is typically a rectifier which converts alternating current into direct current and can generate a specific voltage via a voltage transformer.

[0326] This in turn has the following consequences:

[0327] At Exit A KK Solution L1, M A The concentration of glycolate was higher in L1 than in L2.

[0328] At Exit A KA An aqueous solution of S L4 is obtained, and the concentration of S in L4 is lower than that in L3.

[0329] In step (β3) of the method according to the invention, in particular, a voltage is applied such that a current flows whose current density (= current supplied to the electrolytic cell versus I KM The ratio of the area of ​​the anolyte in contact with the solid electrolyte is between 10 and 8000 A / m 2 In the range of 100 to 2000 A / m 2 In the range of 300 to 800 A / m 2 and even more preferably 494 A / m 2 This can be determined by a person skilled in the art in a standard manner. M The area of ​​the solid electrolyte in contact with the anolyte present is in particular 0.00001 to 10 m 2 , preferably 0.0001 to 2.5 m 2 , more preferably 0.0002 to 0.15 m 2 , even more preferably 2.83m 2 .

[0330] It is obvious that step (β3) of the method according to the invention is carried out in two chambers K M and K A Internal I KA and I KM At least partially accommodates L3 and the internal I KKThe at least partial accommodation of L2 takes place in such a way that both L3 and L2 are in contact with the solid electrolyte contained in the partition wall W and in particular also with the separating element T when the partition wall W contains a solid electrolyte.

[0331] In step (β3), A and E K The fact that charge transfer occurs between KK ,I KM and I KA At the same time, L2 and L3 are accommodated separately so that they cover the electrode E K / E A to the extent that the circuit is completed.

[0332] In particular, the flow in L3 is continuously directed through I KM 、V AM and I KA And the liquid flow of L2 passes through I KK , and the liquid flow of L3 at least partially, preferably completely covers the electrode E A The liquid flow of L2 at least partially, preferably completely covers the electrode E K This is the situation.

[0333] In a further preferred embodiment, the method according to the invention is carried out continuously, ie step (β1) and step (β2) are carried out continuously, while a voltage is applied according to step (β3).

[0334] After implementing step (β3), at outlet A KK Solution L1, M A The concentration of glycolate is higher in L1 than in L2. If L2 already contains M A Hydroxyacetate, then M in L1 A The concentration of glycolate is preferably 1.01 to 200.2 times higher than in L2, more preferably 5.04 to 100.80 times, even more preferably 10.077 to 50.40 times, even more preferably 18.077 to 20.08 times, most preferably 20.00 times higher than in L2, wherein M A The mass proportion of glycolate in L1 and in L2 is more preferably in the range of 0.1% to 50% by weight, even more preferably 1% to 20% by weight.

[0335] At Exit A KA An aqueous solution of S L4 is obtained, and the concentration of S in L4 is lower than that in L3.

[0336] In aqueous solution L3, cation M A The concentration of the cation M in the aqueous solution L4 is preferably in the range of 0.5 to 5 mol / l, more preferably 1 mol / l.A The concentration is more preferably 0.5 mol / l lower than in the aqueous solution L3 used in each case.

[0337] More particularly, steps (β1) to (β3) according to the present invention are carried out at a temperature of 20°C to 110°C, preferably 50°C to 105°C, more preferably 80°C to 99°C, even more preferably 90°C to 95°C and a pressure of 0.5 bar to 1.5 bar, preferably 0.9 bar to 1.1 bar, more preferably 1.0 bar.

[0338] During the implementation of steps (β1) to (β3) of the method according to the invention, hydrogen is usually present in the cathode chamber I KK It can be formed through outlet A KK , removed from the cell together with solution L1. In a particular embodiment of the invention, the mixture of hydrogen and solution L1 can then be separated by methods known to those skilled in the art. When the alkali metal compound used is a halide (especially a chloride), chlorine or another halogen gas may be present in the cell. KA and the gas can be formed together with the solution L4 through the outlet A KK Remove from this pond. In addition, also may form oxygen and / or carbon dioxide which can be removed in the same manner. In a specific embodiment of the present invention, chlorine, oxygen and / or CO2 and the mixture of solution L4 can then be separated by methods well known to those skilled in the art. After chlorine, oxygen and / or CO2 gas has separated from solution L4, then also may separate these by methods well known to those skilled in the art.

[0339] 1.2.2.4 Additional advantages of steps (β1) to (β3)

[0340] This implementation of steps (β1) to (β3) brings further unexpected advantages that were not expected according to the prior art. Without having to sacrifice the alkoxide solution from the cathode space as a buffer solution as in the prior art, steps (β1) to (β3) of the method according to the invention protect the acid-sensitive solid electrolyte from corrosion. Therefore, the method according to the invention is more efficient than the procedure described in WO 2008 / 076327 A1, in which the product solution is used for the intermediate chamber, which reduces the overall conversion rate.

[0341] 2. Step b): PET and solution L1 <21> Reactions

[0342] In step (b) of the process according to the invention, the mixture obtained in step (a) comprising ethylene glycol and M A Hydroxyacetate solution L1 <21> Reaction with PET to produce mixture M1 comprising BHET.

[0343] 2.1 PET starting materials

[0344] The PET used in step (b) of the process according to the invention may be any PET which has to be depolymerized. Typically, such PET is present as waste, in particular at home, in industry or in agriculture.

[0345] In an embodiment of the process according to the invention, the PET to be depolymerized is therefore in a mixture with other plastics, in particular at least one plastic selected from polyethylene ("PE"), polyvinyl chloride ("PVC"). This is generally the case when PET from plastic waste is to be depolymerized in the process according to the invention. In this embodiment, the PET is at least partially separated from the other plastics, preferably by sorting, before being subjected to step (b) of the process according to the invention.

[0346] In an embodiment of the method according to the invention, the PET is subjected to at least one pretreatment step.

[0347] Such a pretreatment step is described, for example, in DE 10032899 C2.

[0348] According to the invention, before being used in step (b), the PET is subjected to at least one pretreatment step selected from a chemical pretreatment step, a comminution step.

[0349] In case the PET is in a mixture with other plastics, before being used in step (b), the PET is preferably subjected to at least one pretreatment step selected from at least partial separation from the other plastics, preferably by sorting, a chemical pretreatment step, a comminution step.

[0350] In the case of PET in a mixture with other plastics, the PET is more preferably first at least partially separated from the other plastics, then subjected to at least one chemical pretreatment and finally comminuted.

[0351] The chemical pretreatment step is in particular a washing step. Such a washing step has the advantage that any impurities, in particular food residues, cosmetic residues and / or body secretions (e.g. blood, semen, excrement) are removed before step (b) is carried out. Such impurities can reduce the efficiency of the reaction in step (b) and / or deteriorate the purity of the BHET thus obtained.

[0352] In the chemical pretreatment step, especially in the washing step, the waste is heated in a washing solution at a temperature of 30 to 99°C, preferably 50 to 90°C, more preferably 70 to 85°C.

[0353] Typical cleaning solutions are familiar to those skilled in the art and are preferably selected from:

[0354] - an aqueous solution of a surfactant (preferably a nonionic surfactant);

[0355] - an aqueous solution of an alkali metal hydroxide or an alkaline earth metal hydroxide, preferably an aqueous solution of NaOH.

[0356] The treatment time in the chemical pretreatment step, especially the washing step, is especially from 1 minute to 12 hours, preferably from 10 minutes to 6 hours, more preferably from 30 minutes to 2 hours, even more preferably from 45 to 90 minutes, most preferably 60 minutes.

[0357] After the PET has been treated by the chemical pretreatment steps, in particular the washing steps, the aqueous solution is separated off, for example by filtration, and the cleaned PET is preferably washed once with water to remove residues of the washing solution.

[0358] The PET waste thus obtained is then dried, in particular in a drying oven.

[0359] The temperature for drying here is in particular in the range from 30 to 120°C, preferably from 50 to 100°C, more preferably from 60 to 90°C, most preferably 80°C.

[0360] The comminution step has the advantage that the surface area of ​​the PET available for the reaction in step (b) is increased. This increases the reaction rate of the reaction in step (b). The comminution can be carried out in equipment known to those skilled in the art, such as a crusher or a cutting die machine.

[0361] In a further embodiment of the method according to the invention, the PET is decolorized or colored in a controlled manner before being subjected to step (b). This can be carried out by methods known to those skilled in the art, such as decolorization with hydrogen peroxide or coloring with dyes.

[0362] 2.2 Reaction conditions

[0363] PET contains ethylene glycol and M A Hydroxyacetate solution L1 <21> The reaction to produce the mixture M1 can be carried out under conditions familiar to the person skilled in the art.

[0364] Preferably, the reaction in step (b) is carried out until (i.e., reaches) time t b , at the time t b , at least P=10%, preferably at least P=20%, more preferably at least P=25%, more preferably at least P=30%, more preferably at least P=40%, more preferably at least P=50%, more preferably at least P=60%, more preferably at least P=70%, more preferably at least P=80%, more preferably at least P=90%, more preferably at least P=95%, even more preferably at least P=99% of the PET used in step (b) has been converted.

[0365] The percentage P is calculated by the following formula:

[0366] P=(n TS +n MHET +n BHET ) / n PET .

[0367] n PET Here are the molar amounts of repeating units of the following structure (III) in the PET used in step (b):

[0368]

[0369] n TS is the time from the start of step (b) to time t b , the molar amount of TS formed in step (b).

[0370] n MHET is the time from the start of step (b) to time t b , the molar amount of MHET formed in step (b).

[0371] n BHET is the time from the start of step (b) to time t b , the molar amount of BHET formed in step (b).

[0372] The structures of compounds BHET, MHET, and TS are as follows:

[0373]

[0374] "MHET" also encompasses the corresponding carboxylate salts of the shown structure.

[0375] "TS" also encompasses the corresponding mono- and di-carboxylates of the shown structure.

[0376] The reaction in step (b) is especially carried out at a temperature of at least 100°C, preferably at a temperature in the range of ≥100°C to ≤197°C, more preferably at a temperature in the range of ≥130°C to ≤197°C, more preferably at a temperature in the range of ≥150°C to ≤197°C, more preferably at a temperature in the range of ≥175°C to ≤197°C.

[0377] The reaction in step (b) is preferably carried out at the boiling temperature of the ethylene glycol. Even more preferably, the ethylene glycol is refluxed, which means that the ethylene glycol evaporates from the reaction, condenses and then returns to the reaction. The reflux can be established by means familiar to those skilled in the art (e.g. in a distillation apparatus).

[0378] Based on the total weight of PET used in the process, the M used in the process AThe total weight of glycolate is in particular in the range from 0.1% to 100% by weight, preferably in the range from 0.5% to 80% by weight, more preferably in the range from 1.0% to 50% by weight, more preferably in the range from 1.5% to 25% by weight, more preferably in the range from 2.0% to 10% by weight, more preferably in the range from 2.5% to 6.0% by weight, more preferably in the range from 3.5% to 5.0% by weight, most preferably 3.9% by weight.

[0379] The reaction can be carried out using apparatus familiar to those skilled in the art.

[0380] After step (b) of the process according to the invention has been concluded, a mixture M1 is obtained in which the molar amount of BHET (n BHET ) and the sum of the molar amounts of MHET and TS (n MHET +n TS ) is in the range of 1:1 to 1000:1, preferably 2:1 to 500:100, more preferably 4:1 to 300:1, even more preferably 10:1 to 100:1, still more preferably 13:1 to 60:1, still more preferably 13:1 to 24:1.

[0381] η=n BHET / (n MHET +n TS )

[0382] 2.3 Preferred step c)

[0383] In a preferred further step (c), BHET is at least partially separated from M1. This is even more preferably carried out by crystallization and / or distillation. Even more preferably, the BHET in step (c) is filtered off from M1 and then crystallized.

[0384] 3. Methods for recycling PET

[0385] In the process for recovering polyethylene in step (ζ), the BHET obtained in the mixture M1 in the process according to the invention is preferably polymerized to PET.

[0386] This polymerization is known to the person skilled in the art as "polycondensation" and is described, for example, in EP 0 723 951 A1 and in the book "Modern Polyesters: Chemistry and Technology of Polyesters and Copolyesters (edited by J. Scheirs and T. E. Long, 2003, John Wiley & Sons, Ltd ISBN: 0-471-49856-4), page 2, Chapter 2 "Poly (Ethylene Terephthalate) Polymerization—Mechanism, Catalysis, Kinetics, Mass Transfer and Reactor Design", by Th. Rieckmann and S. describe.

[0387] In particular, for this purpose, in step (ζ), BHET is polymerized back to PET in the presence of a catalyst, in particular a catalyst selected from the group consisting of antimony compounds, preferably Sb2O3.

[0388] Preferably, in step (ζ), the polymerization of BHET to PET is carried out at least at the boiling temperature of ethylene glycol. In particular, during the polymerization in step (ζ), ethylene glycol is removed from the reaction mixture to shift the reaction equilibrium to the polymer PET side.

[0389] More preferably, in step (ζ), the polymerization of BHET to PET is carried out at the boiling temperature of ethylene glycol. Even more preferably, in that case, during the polymerization in step (ζ), ethylene glycol is removed from the reaction mixture to shift the reaction equilibrium to the polymer PET side.

[0390] This is achieved in particular by distillation at a pressure of <1 bar, preferably 0.1 mbar, at the corresponding boiling temperature of the ethylene glycol at the corresponding pressure.

[0391] Example

[0392] 1. Inventive Example E1:

[0393] 1.1 Preparation of ethylene glycol solution of sodium glycolate by electrolysis

[0394] 1.1.1 Experimental setup

[0395] Electrolytic recovery of sodium glycolate is carried out in a three-chamber electrolytic cell.

[0396] The middle chamber was separated from the anode chamber by a filter cloth and from the cathode chamber by a 15 x 15 cm Nasicon ceramic.

[0397] The anode used was a DSA [“Dimensionally Stable Anode”; a titanium anode coated with ruthenium oxide / iridium oxide (RuO 2 +IrO 2 / Ti)]; the cathode consisted of VA steel (VA means “corrosion resistant”; stainless steel).

[0398] A Gamry Reference 3000 (AE) potentiostat and a Reference 30K Booster were used as the power supply.

[0399] The cathode chamber of the electrolytic cell is connected to a 250 ml heatable jacketed container with a magnetic stirrer, from which the electrolyte can be pumped by means of a peristaltic pump through the conductivity measurement point and a further 100 ml glass heat exchanger into the cathode chamber of the electrolytic cell. From there the catholyte can be pumped into the jacketed container. The catholyte is thus circulated.

[0400] A thermostat with a PT 100 sensor (a platinum sensor with a nominal resistance of 100Ω at a temperature of 0° C.) and a heat exchanger were used to measure and regulate the temperature of the electrolyte on the cathode side.

[0401] The middle chamber of the electrolytic cell is connected to a reservoir container, from which the electrolyte is pumped using a peristaltic pump into the middle chamber, then via a filter cloth into the anode chamber and from there via a pH measurement point into a collecting container.

[0402] A thermostat or heat exchanger with a PT 100 sensor is used to measure and regulate the temperature of the electrolyte on the anode side. The anolyte is not circulated.

[0403] 1.1.2 Experimental procedures:

[0404] The thermostat for the cathode side is adjusted to 90° C. and started. 650 g of a 1 wt % sodium glycolate solution is introduced into a heatable jacketed container and a peristaltic pump is started (delivery rate 1000 ml / h), so that the sodium glycolate solution is pumped through the conductivity measurement point and a further heat exchanger into the cathode chamber of the electrolytic cell. Then the glycolate is made to flow out of the cathode chamber and returned to the jacketed container. The glycolate and the chamber are thus kept at a controlled temperature of 90° C. The thermostat for the NaCl side is adjusted to 105° C. and a peristaltic pump for the NaCl brine is started (delivery rate 4000 ml / h). A 20 wt % NaCl brine at pH 11 is pumped from a liquid storage container through a heat exchanger into the intermediate chamber of the electrolytic cell. From there, it flows through a filter cloth into the anode chamber and then out of the cell into the pH measurement point and then into a collecting container. The NaCl brine is not circulated. As soon as the cathode chamber is heated to 90°C and the anode side at the pH measurement point is at a temperature of 80°C, the current of the electrolytic cell is turned on. For this purpose, the potentiostat is switched to constant current operation. The current is fixed at 10 amperes and the voltage is controlled accordingly. Then, the conductivity measurement values ​​of the glycolate and the pH measurement values ​​of the NaCl brine are recorded.

[0405] The current, voltage, temperature of glycolate, conductivity of glycolate, pH of brine and temperature of brine were recorded every 20 seconds. The hydrogen formed and the chlorine formed were removed by suction. The chlorine was neutralized with NaOH in a gas scrubber.

[0406] The electrolysis was carried out for 4 hours. Then, the current was switched off and the cell was completely emptied.

[0407] The sodium glycolate solution had a concentration of -20 wt%.

[0408] 1.2 Depolymerization of PET using ethylene glycol solution of sodium glycolate from electrolysis

[0409] In the process according to the invention, 100 g of PET were initially charged to the autoclave together with 800 g of ethylene glycol. The solution was then heated to 150° C. while stirring. As soon as the temperature reached 150° C., 19.5 g of a 20% solution of sodium glycolate in ethylene glycol (corresponding to 0.046 mol) from the electrolysis were added. The reaction was carried out during five hours and the reactor output was analyzed after cooling. Figure 8 The conversions of the obtained BHET (1), mono-2-hydroxyethyl terephthalate (= "MHET") (2) and terephthalic acid (= "TS") (3) are shown (determined by gas chromatography; in % conversion based on the repeating units of the structure (Ξ) of the PET used; sparse hatching " / / / / ").

[0410] 2. Comparative Example V1:

[0411] In a comparative experiment, 100 g of PET were initially charged into the autoclave together with 800 g of ethylene glycol. The solution was then heated to 150° C. while stirring. The reaction was carried out during five hours and the reactor output was analyzed after cooling. Figure 8 The obtained conversions of BHET (1), MHET (2) and TS (3) are shown in FIG. 1 (black, “■”).

[0412] 3. Comparative Example V2:

[0413] In a comparative experiment, 100 g of PET were initially charged into the autoclave together with 800 g of ethylene glycol. The solution was then heated to 150° C. while stirring. As soon as the temperature reached 150° C., 3.7 g of a 50% aqueous solution of NaOH (corresponding to 0.046 moles) were added. The reaction was carried out during five hours and the reactor output was analyzed after cooling. Figure 8 The obtained conversions of BHET (1), MHET (2) and TS (3) are shown in FIG. 5 (thick hatching, “ / / / / ”).

[0414] 4. Results

[0415] Comparison of the contents of BHET, MHET and TS in the depolymerization products of Inventive Example E1 and Comparative Examples V1 and V2 (see Figure 8 ) show that the depolymerization of ethylene glycol solutions of sodium glycolate obtained using electrolysis provides a higher BHET ratio. This is advantageous because more product is obtained as a result, which can be directly converted into new PET products in the polycondensation.

[0416] 6. Reference symbols in the drawings

Claims

1. A depolymerization method for polyethylene terephthalate (PET), comprising the following steps: (a) In electrolytic cell E <1> M A Hydroxyacetate solution in ethylene glycol L1 <21> , where M A is an alkali metal cation, the electrolytic cell E <1> Include - at least one anode chamber K A <11> , which has at least one inlet Z KA <110> , at least one exit A KA <111> , and comprising an anode electrode E A <113> Internal I KA <112> , - at least one cathode chamber K K <12> , which has at least one inlet Z KK <120> , at least one exit A KK <121> , and comprising a cathode electrode E K <123> Internal I KK <122> , - and optionally at least one interposed intermediate chamber K M <13> , which has at least one inlet Z KM <130> , at least one exit A KM <131> and internal I KM <132> , Among them I KA <112> and I KM <132> Through the diffusion barrier D <14> are separated from each other, and A KM <131> By connecting V AM <15> Connect to inlet Z KA <110> , so that the liquid can flow from I KM <132> Via the connection V AM <15> Pass to I KA <112> , in - wherein said electrolytic cell E <1> Does not include intermediate chamber K M <13> In this case, I KA <112> and I KK <122> Through the partition wall W <16> Separated from each other, - wherein said electrolytic cell E <1> Contains at least one intermediate chamber K M <13> In this case, I KK <122> and I KM <132> Through the partition wall W <16> Separated from each other, wherein the partition wall W <16> Having a surface O KK <163> One side S KK <161> and in S KK <161> The opposite side of the side and having a surface O A / MK <164> One side S A / MK <162> , wherein the partition wall W <16> Solid electrolyte ceramic F comprising at least one conductive alkali metal cation A <18> , so that the partition wall W <16> Solid electrolyte ceramic F containing alkali metal cations A <18> Through the surface O KK <163> In the S KK <161> Side and interior I KK <122> Direct contact, And among them - wherein said electrolytic cell E <1> Does not include intermediate chamber K M <13> In the case of <16> The solid electrolyte ceramic F containing the conductive alkali metal cation A <18> Through the surface O A / MK <164> In the S A / MK <162> Side and interior I KA <112> Direct contact, - wherein said electrolytic cell E <1> Contains at least one intermediate chamber K M <13> In the case of <16> The solid electrolyte ceramic F containing the conductive alkali metal cation A <18> Through the surface O A / MK <164> In the S A / MK <162> Side and interior I KM <132> Direct contact, (α) wherein, in the electrolytic cell E <1> When it does not contain the intermediate chamber K M <13> , the following steps (α1), (α2), and (α3) are performed simultaneously: (α1) Solution L2 containing ethylene glycol <22> Guided by I KK <122> , (α2) will contain M A Neutral or alkaline aqueous solution L3 of a salt S as a cation <23> Guided by I KA <112> , (α3) in E A <113> and E K <123> Apply voltage between or (β) wherein, in the electrolytic cell E <1> When it contains at least one intermediate chamber K M <13> , the following steps (β1), (β2), and (β3) are performed simultaneously: (β1) Solution L2 containing ethylene glycol <22> Guided by I KK <122> , (β2) will contain M A Neutral or alkaline aqueous solution L3 of a salt S as a cation <23> Guided by I KM <132> , then through V AM <15> , then through I KA <112> , (β3) in E A <113> and E K <123> Apply voltage between At the outlet A KK <121> Solution L1 is provided <21> , M A The concentration of glycolate is L1 <21> The ratio is in L2 <22> Medium-high, And it is at the outlet A KA <111> Provide an aqueous solution of S L4 <24> , the concentration of S in L4 <24> The ratio is in L3 <23> Medium-low; (b) Solution L1 <21> Reaction with PET to produce a mixture M1 comprising bis-2-hydroxyethyl terephthalate BHET.

2. The method according to claim 1, wherein the solid electrolyte ceramic F conducting alkali metal cations A <18> With formula M I 1+2w+x-y+z M II w M III x Zr IV 2-w-x-y M V y (SiO4) z (PO4) 3-z The structure: Among them, M I Selected from Na + and Li + , M IIis a divalent metal cation, M III is a trivalent metal cation, M V is a pentavalent metal cation, The Roman numerals I, II, III, IV, and V indicate the oxidation number of the corresponding metal cations present therein. And w, x, y, z are real numbers, where 0≤x<2, 0≤y<2, 0≤w<2, 0≤z<3, And wherein w, x, y, z are selected such that 1+2w+x-y+z≥0 and 2-wxy≥0.

3. The method according to claim 1 or 2, wherein the electrolytic cell E <1> Does not include intermediate chamber K M <13> .

4. The method according to claim 1 or 2, wherein the electrolytic cell E <1> Contains at least one intermediate chamber K M <13> .

5. The method according to any one of claims 1 to 4, wherein M A Selected from the group consisting of potassium and sodium.

6. The process according to any one of claims 1 to 5, wherein step b) is carried out until at least P=10% of the PET used in step (b) has been converted.

7. The process according to any one of claims 1 to 6, wherein step (b) is carried out at the boiling temperature of ethylene glycol.

8. The method according to any one of claims 1 to 7, wherein in step (b) a sufficient amount of solution L1 is used <21> , so that based on the total weight of PET used in step (b), the M used in step (b) A The total weight of glycolate is in the range of 0.1 wt% to 100 wt%.

9. The process according to any one of claims 1 to 8, wherein in a further step (c) BHET is at least partially separated from M1.

10. The process according to claim 9, wherein the at least partial separation of BHET from M1 in step (c) is performed by crystallization and / or distillation.

11. The method according to any one of claims 1 to 10, wherein: Before being used in step (b), the PET is subjected to at least one pretreatment step selected from a chemical pretreatment step, a comminution step.

12. A process for recovering polyethylene terephthalate, wherein BHET is obtained by the process according to any one of claims 1 to 11 and the BHET thus obtained is polymerized to PET in step (ζ).

13. The process of claim 12, wherein the polymerization of BHET to PET in step (ζ) is carried out at at least the boiling temperature of ethylene glycol.

14. The process according to claim 12 or 13, wherein the polymerization in step (ζ) is carried out in the presence of a catalyst.

15. The process according to claim 14, wherein the catalyst is selected from antimony compounds.

Citation Information

Patent Citations

  • Process for processing PET containers using heat treatment

    DE10032899C2

  • Methods for the preparation of 1,1-diarylalkanes and derivatives thereof

    DE102010062804A1

  • Electrolyte material with NASICON structure for solid-state sodium-ion batteries and method for its production

    DE102015013155A1

  • Electrochemical production of alkali alcoholate, used as intermediate, reactant or catalyst in organic synthesis, uses sodium- or potassium-ion-conducting ceramic membrane separating anolyte containing salt and alcoholic catholyte

    DE10360758A1

  • Process to prepare bis (2-hydroxyethyl) terephthalate

    EP0723951A1