Article having anti-fouling surface and method for forming anti-fouling surface

By forming a multi-layer structure of lubricating layer and anti-adhesive coating on the surface of industrial devices, the interfacial tension difference is used to move pollutants from the lubricating layer to the anti-adhesive coating, solving the problem of surface pollution in industrial devices and improving cleaning performance and durability.

CN119013357APending Publication Date: 2024-11-22LG CHEM LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380033569.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-19
Filing Date
2023-05-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to effectively prevent contamination of industrial devices such as display panels, sensors and radar surfaces, especially in autonomous driving systems, where pollutants are prone to adhere and cause failure, and conventional anti-pollution coatings are not durable.

Method used

Using a multi-layer structure with lubricating layer and anti-adhesive coating, the surface energy of the lubricating layer is less than 20mJ/m2, and the surface energy of the anti-adhesive coating is greater than 20mJ/m2. The contaminants are moved from the lubricating layer to the The anti-adhesion coating is removed and the hydrophobic inorganic cured layer is used in combination with the fluoro-silane cured layer.

Benefits of technology

It realizes effective prevention of contaminants, improves the cleanliness and durability of the device surface, and reduces the risk of failure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013357A_ABST
    Figure CN119013357A_ABST
Patent Text Reader

Abstract

The present disclosure relates to an article having an anti-fouling surface and a method for forming an anti-fouling surface on a surface of an article.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2022-0061622 filed in the Korean Intellectual Property Office on May 19, 2022, the disclosure of which is incorporated herein by reference in its entirety.

[0003] The present disclosure relates to articles having anti-fouling surfaces and methods for forming anti-fouling surfaces on surfaces of articles. Background Art

[0004] Anti-fouling coatings are used in industry to prevent the adhesion of foreign matter to a specific surface or the adsorption of pollutants to a specific surface.

[0005] Specifically, for example, even under normal use environments, the surfaces of display panels, camera lenses, infrared sensors, visible light sensors, camera sensors, radars, lidars, etc. are occasionally subject to contamination caused by human fingerprints, dust, or external stains.

[0006] If contamination occurs on the surface of such a device, it may block the user's field of view or cause the device to malfunction. In particular, various sensors and radars are used in autonomous driving devices that have recently attracted much attention. If contamination occurs on the surface of these devices, errors in data understanding may occur due to the contamination, which may greatly threaten the safety of autonomous driving users and people around them.

[0007] Therefore, there is a need to prevent contaminants from adhering to the surfaces of such devices and to keep the surfaces of the devices clean.

[0008] However, contaminants are easily attached to the general glass or polymer resin used as the surface substrate of such devices due to their nature. Therefore, regular cleaning is required, and a separate power source or device is required for this. In addition, even if cleaning and drying are performed, there is a problem that additional surface stains may appear.

[0009] Furthermore, in the case of a super water-repellent coating or a super oil-repellent coating for preventing adhesion of pollutants, there are surface irregularities, but the durability of these surface irregularities is not high, so there is a problem that the effect cannot last long.

[0010] Therefore, research on anti-fouling surfaces that can prevent contaminants from adhering to the surface of devices is required. Summary of the invention

[0011] Technical issues

[0012] The present disclosure relates to articles having anti-fouling surfaces and methods for forming anti-fouling surfaces on surfaces of articles.

[0013] Technical Solution

[0014] In the present disclosure, an article having an anti-fouling surface is provided, the anti-fouling surface comprising: a substrate; a first region, the first region being present on a portion of the surface of the substrate and having a lubricating layer formed thereon; and a second region, the second region being present on at least a portion of the surface of the substrate other than the first region and having an anti-adhesion coating formed thereon.

[0015] According to one embodiment of the present disclosure, the surface energy of the second region may be greater than the surface energy of the first region.

[0016] Specifically, the surface energy of the lubricating layer may be less than about 20 mJ / m 2 .

[0017] In addition, the surface energy of the anti-adhesion coating can be about 20 mJ / m 2 or larger.

[0018] In addition, the surface energy of the anti-adhesion coating can be about 40 mJ / m 2 or smaller.

[0019] According to another embodiment of the present disclosure, the second region may be formed to surround the first region.

[0020] Furthermore, the first region may be formed in a convex shape or a concave shape.

[0021] According to one embodiment of the present disclosure, the thickness of the lubricating layer may be about 0.1 μm to 200 μm, 0.1 μm or more, about 0.5 μm or more, about 1 μm or more, about 200 μm or less, about 150 μm or less, or about 100 μm or less.

[0022] Furthermore, the lubricating layer may include a hydrophobic inorganic cured layer, a fluorine-silane cured layer formed on the hydrophobic inorganic cured layer, and a fluorine oil layer formed on the fluorine-silane cured layer.

[0023] According to one embodiment of the present disclosure, the hydrophobic inorganic cured layer may include a cured product of an alkyl-trialkoxysilane and a tetraalkoxysilane.

[0024] In addition, the hydrophobic inorganic cured layer may have a thickness of about 0.05 μm to 20 μm, about 0.05 μm or more, or about 0.1 μm or more, and about 20 μm or less, about 15 μm or less, or about 10 μm or less.

[0025] According to another embodiment of the present disclosure, the fluoro-silane cured layer may include a cured product of fluoropolyether silane.

[0026] Furthermore, the fluorine oil layer may contain fluorinated polyether oil.

[0027] In addition, the sum of the thicknesses of the fluoro-silane cured layer and the fluoro oil layer may be about 0.1 μm to 200 μm, about 0.1 μm or more, about 0.5 μm or more, about 1 μm or more, about 200 μm or less, about 150 μm or less, or about 100 μm or less.

[0028] Furthermore, the anti-stick coating may contain cured polydialkylsiloxane and silicone oil.

[0029] Furthermore, the viscosity of the silicone oil may be 1000 cSt or less.

[0030] Meanwhile, in the present disclosure, a method for forming an anti-fouling surface is provided, the method comprising the following steps: forming a first region including a hydrophobic inorganic solidified layer on a portion of a surface of a substrate; forming a second region including an anti-adhesion coating on at least a portion of the surface of the substrate other than the first region; and forming a lubricating layer in the first region.

[0031] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.

[0032] Unless the context clearly indicates otherwise, the singular forms are intended to include the plural forms as well.

[0033] It will be further understood that the terms “including,” “comprising,” or “having” when used in the present disclosure indicate the presence of stated features, quantities, steps, components, or combinations thereof, but do not preclude the presence or addition of one or more other features, quantities, steps, components, or combinations thereof.

[0034] Furthermore, as used herein, when it is mentioned that a layer or an element is formed 'on' a layer or an element, the layer or the element may be directly formed on the layer or the element, or other layers or elements may be additionally formed between layers, on an object, or on a substrate.

[0035] Since the present invention can be variously modified and has various forms, its specific embodiments are shown by way of example and will be described in detail. However, it is not intended to limit the present invention to the specific forms disclosed, and it should be understood that the present invention includes all modifications, equivalents and alternatives within the concept and technical scope of the present invention.

[0036] Hereinafter, the present invention will be described in detail.

[0037] According to one aspect of the present disclosure, there is provided an article having an anti-fouling surface, the anti-fouling surface comprising: a substrate; a first region, the first region being present on a portion of the surface of the substrate and having a lubricating layer formed thereon; and a second region, the second region being present on at least a portion of the surface of the substrate other than the first region and having an anti-adhesion coating formed thereon.

[0038] The present inventors have discovered that when contaminants adhere to the surface of an article including both a first region in which a lubricating layer is formed on the surface of a substrate and a second region in which an anti-adhesive coating is formed, the contaminants move from the first region to the second region and fall off from the surface of the anti-adhesive coating in the second region, so that the contaminants do not adhere to the surface of the article, thereby completing the present invention.

[0039] First, in the article having an antifouling surface according to one aspect of the present disclosure, the term "substrate" may refer to a substrate constituting the surface of the article itself, or may mean a substrate applied separately to realize an antifouling surface on the surface of a general article.

[0040] Furthermore, on the surface of the substrate, there is a first region in which the lubricating layer is formed and a second region in which the anti-adhesive coating is formed. On the surface of the substrate, the first region and the second region may exist separately and not overlap each other.

[0041] Figure 1 The figure schematically shows a cross section of an anti-fouling surface in an article provided with the anti-fouling surface according to one embodiment of the present disclosure.

[0042] Reference Figure 1 In an article having an anti-fouling surface according to one embodiment of the present disclosure, the anti-fouling surface includes: a substrate 100; a first region 200, which exists on a portion of the surface of the substrate and has a lubricating layer formed thereon; and a second region 300, which exists on at least a portion of the surface of the substrate other than the first region and has an anti-adhesion coating formed thereon.

[0043] According to one embodiment of the present disclosure, the surface energy of the second region may be greater than the surface energy of the first region.

[0044] That is, the first region is a region in which the lubricating layer is formed, and its surface energy may have a relatively small value. In addition, the second region is a region in which the anti-sticking coating is formed, and its surface energy may have a relatively large value.

[0045] On the contrary, in the first and second partitioned regions on the surface of the article according to an embodiment of the present disclosure, the region with relatively low surface energy can be referred to as the first region in which the lubricating layer is formed. In the first and second partitioned regions on the surface of the article according to an embodiment of the present disclosure, the region with relatively high surface energy can be referred to as the second region in which the anti-adhesion coating is formed.

[0046] When contamination occurs on the anti-fouling surface, due to the difference in surface energy, the attached contaminants are pushed from the area with relatively low surface energy (i.e., the first area where the lubricating layer is formed) to the area with relatively low surface energy (i.e., the second area where the anti-adhesion coating is formed).

[0047] Specifically, when contamination occurs on the anti-contamination surface, due to the difference in surface energy between the first area and the second area, a difference between a first interfacial tension and a second interfacial tension occurs, wherein the first interfacial tension is generated at the interface between the contaminant and the surface of the first area, and the second interfacial tension is generated at the interface between the contaminant and the surface of the second area.

[0048] That is, since the first interfacial tension is greater than the second interfacial tension, some contaminants on the first region are relatively concentrated at the center of the contaminants, and some contaminants on the second region are relatively spread outward, causing the center of the contaminants to gradually move toward the second region.

[0049] Furthermore, due to the anti-adhesive coating, the contaminants pushed to the second area are directly desorbed and removed from the surface of the article.

[0050] Through this process, an anti-pollution surface can be achieved, and an article provided with such an anti-pollution surface can effectively prevent its surface from being contaminated by external pollution sources.

[0051] In other words, when the contaminant contacts both interfaces of the lubricating layer and the anti-adhesive coating, the above effect occurs due to the difference in surface tension acting on the interface between the lubricating layer and the contaminant and the interface between the anti-adhesive coating and the contaminant.

[0052] When the lubricating layer or the anti-adhesive coating is used alone, it is difficult to obtain the above-mentioned effect because spontaneous movement of contaminants due to the difference in surface tension does not occur on the layer.

[0053] Figure 2 A diagram schematically showing an effect achieved by one embodiment of the present disclosure.

[0054] Reference Figure 2 , it can be determined that due to the difference in surface energy at the interface of the lubricating layer and the anti-adhesion coating, the contaminants attached to the surface move toward the anti-adhesion coating and then fall off.

[0055] also, Figure 3 It is a schematic diagram showing an example of achieving a pollution prevention effect in a product according to an embodiment of the present disclosure.

[0056] Reference Figure 3 When the article according to one embodiment of the present disclosure is a sensor recognized by a camera, it can be determined that due to the difference in surface energy at the interface between the lubricating layer and the anti-adhesion coating, the contaminants attached to the sensor move toward the anti-adhesion coating. In this case, the possibility of sensor failure caused by the attachment of contaminants can be reduced.

[0057] For example, the lubricating layer may be a layer that can achieve a Slippery Liquid-Infused Porous Surface (SLIPS) effect. In this context, the SLIPS layer does not necessarily have to have a porous surface.

[0058] For example, the surface energy value of both the lubricating layer and the anti-adhesive coating can be about 50 mJ / m 2 or less. That is, it is desirable that both the lubricating layer and the anti-adhesion coating have low surface energies. More specifically, both the lubricating layer and the anti-adhesion coating may be hydrophobic layers. Meanwhile, the surface energy of the lubricating layer may be relatively lower than the surface energy of the anti-adhesion coating, and conversely, the surface energy of the anti-adhesion coating may be relatively higher than the surface energy of the lubricating layer.

[0059] Specifically, for example, the surface energy of the lubricating layer may be less than about 20 mJ / m 2 , less than about 18mJ / m 2 , less than about 15mJ / m 2 , or less than about 12 mJ / m 2 .

[0060] When the surface energy of the lubricating layer is outside the above range, the above-mentioned effect of moving contaminants from the lubricating layer to the anti-sticking coating layer cannot be produced.

[0061] In addition, the surface energy of the anti-adhesion coating can be about 20 mJ / m 2 or greater, about 20mJ / m 2 or greater, or about 25mJ / m 2 or greater, and about 40mJ / m 2 or less, 35mJ / m 2 or less, or about 30mJ / m 2 or smaller.

[0062] When the surface energy of the anti-sticking coating is outside the above range, the above-mentioned effect of moving contaminants from the lubricating layer to the anti-sticking coating cannot be produced, and there may be a problem that contaminants do not fall off the anti-sticking coating.

[0063] The surface energy can be measured by dropping droplets of water and diiodomethane on the surface, measuring the contact angle using a contact angle meter, and then calculating it by inputting the measured values ​​into a model equation.

[0064] Specifically, the surface energy can generally be calculated using the Fowkes equation or the van Oss Chaudhury Good equation.

[0065] According to another embodiment of the present disclosure, the second region may be formed to surround the first region.

[0066] Figure 4 The image schematically shows an anti-fouling surface observed from above in an article provided with the anti-fouling surface according to one embodiment of the present disclosure.

[0067] Reference Figure 4 , it can be determined that the second area 300 surrounds the first area 200 .

[0068] exist Figure 4 In the case of FIG. 1 , the first region is shown in a circular shape, and the second region is shown in a square shape. This is because it is for convenience of explanation that the second region is shown around the shape of the first region, and the shapes of the first region and the second region are not necessarily limited to a circle or a specific polygon.

[0069] Furthermore, the anti-pollution surface may have one first region and one second region as shown in the drawings, or may have a plurality of first regions and second regions, wherein the number of first regions and the number of second regions are not necessarily the same.

[0070] Figure 5 The image schematically shows an anti-fouling surface observed from above in an article provided with the anti-fouling surface according to another embodiment of the present disclosure.

[0071] According to one embodiment of the present disclosure, the average area of ​​the first region is preferably about 5 cm 2 or smaller.

[0072] Furthermore, it may be desirable that the area ratio of the first region in which the lubricating layer is formed to the total area of ​​the first region and the second region is about 20% to about 80%.

[0073] When the area of ​​the first region is too large or the ratio of the first region is too high, that is, when the area ratio of the first region in which the lubricating layer is formed to the total area is too large, there may be a problem that the contaminants attached to the surface do not move from the first region to the second region but remain in the middle of the first region. Additionally, when the area of ​​the first region is too narrow or the ratio of the first region is too low, that is, when the area ratio of the first region in which the lubricating layer is formed to the total area is too small, there may be disadvantages in transparency and visibility.

[0074] Additionally, the first region may be formed in a convex shape or a concave shape. By forming the first region in a convex shape or a concave shape, the above-mentioned effect of moving the contaminants attached to the surface from the first region to the second region can be further promoted.

[0075] Figure 6 and Figure 7 The figure schematically shows a cross section of an anti-fouling surface in an article provided with the anti-fouling surface according to one embodiment of the present disclosure.

[0076] Reference Figure 6 and Figure 7 In the article having an anti-fouling surface according to one embodiment of the present disclosure, a substrate 100, a first region 200 formed in a concave or convex shape, and a second region 300 may be defined.

[0077] In the drawings, the first region formed in a concave or convex shape is shown in an arc form, but the present disclosure is not necessarily limited thereto. The first region may have a concave or convex cross section in the form of various curves or polygons.

[0078] According to one embodiment of the present disclosure, the thickness of the lubricating layer may be about 0.1 μm to 200 μm, or about 0.1 μm or more, about 0.5 μm or more, or about 1 μm or more, and about 200 μm or less, about 150 μm or less, or about 100 μm or less.

[0079] When the thickness is too thin, problems such as deterioration of durability and lubricating effect may occur, whereas when the thickness is too thick, problems such as cracks in the lubricating layer or excessive flow of lubricating fluid may occur.

[0080] Furthermore, the lubricating layer may include a hydrophobic inorganic cured layer, a fluorine-silane cured layer formed on the hydrophobic inorganic cured layer, and a fluorine oil layer formed on the fluorine-silane cured layer.

[0081] Herein, the fluorine-silane cured layer and the fluorine oil layer may be clearly distinguished by the boundary between the layers, or may not be separated into layers because the boundary between the layers is unclear, depending on the characteristics of the constituent materials of the fluorine-silane cured layer and the fluorine oil layer.

[0082] The hydrophobic inorganic cured layer may be formed by curing a coating solution for forming the hydrophobic inorganic cured layer (hereinafter, referred to as a first coating solution).

[0083] According to one example of the present disclosure, the hydrophobic inorganic cured layer may include a cured product of an alkyl-trialkoxysilane and a tetraalkoxysilane, and the first coating solution may include an alkyl-trialkoxysilane and a tetraalkoxysilane.

[0084] According to one embodiment of the present disclosure, the alkyl-trialkoxysilane may be a compound represented by the following Chemical Formula 1.

[0085] [Chemical formula 1]

[0086] R11-Si(R12)(R13)(R14)

[0087] In Chemical Formula 1, R11 is an alkyl group having 1 to 5 carbon atoms, and R12 to R14 are each independently an alkoxy group having 1 to 5 carbon atoms.

[0088] More specifically, R11 may be a methyl group, an ethyl group, a propyl group, a butyl group or a pentyl group, and may be linear or branched.

[0089] R12 to R14 may each independently be a methoxy group, an ethoxy group, a propoxy group, a butoxy group or a pentyloxy group, and may be linear or branched.

[0090] Specifically, the alkyl-trialkoxysilane can be, for example, at least one selected from the following: methyl-trimethoxysilane, methyl-triethoxysilane, methyl-tripropoxysilane, methyl-tributoxysilane, methyl-tripentoxysilane, ethyl-trimethoxysilane, ethyl-triethoxysilane, ethyl-trippropoxysilane, ethyl-tributoxysilane, ethyl-tripentoxysilane, propyl-trimethoxysilane, propyl-triethoxysilane, propyl-trippropoxysilane, propyl-tributoxysilane, propyl-tripentoxysilane, butyl-trimethoxysilane, butyl-triethoxysilane, butyl-trippropoxysilane, butyl-tributoxysilane, butyl-tripentoxysilane, pentyl-trimethoxysilane, pentyl-triethoxysilane, pentyl-trippropoxysilane, pentyl-tributoxysilane, and pentyl-tripentoxysilane.

[0091] The above-mentioned alkyl-trialkoxysilane is a component of the main network of the inorganic coating film formed by sol-gel reaction in the composition. At this time, the alkyl group can improve the flexibility of the network structure and alleviate the stress generated when the silanols or the silanols react with the substrate surface. When only using alkylsilane, the number of silanols participating in the reaction is small, which is unfavorable for reducing the surface energy during the subsequent fluorine coating, and when only using alkoxysilane, the above-mentioned stress relief effect cannot be obtained.

[0092] According to one embodiment of the present disclosure, the tetraalkoxysilane may be a compound represented by the following Chemical Formula 2.

[0093] [Chemical formula 2]

[0094] Si(R21)(R22)(R23)(R24)

[0095] In Chemical Formula 2, R21 to R24 are each independently an alkoxy group having 1 to 5 carbon atoms.

[0096] More specifically, R21 to R24 may each independently be a methoxy group, an ethoxy group, a propoxy group, a butoxy group or a pentyloxy group, and may be linear or branched.

[0097] Specifically, the tetraalkoxysilane may be, for example, at least one selected from the group consisting of tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, and tetrapentoxysilane.

[0098] The tetraalkoxysilane as described above can increase the silanol groups that can participate in the reaction between the above-mentioned silanols in the composition or between the silanols and the substrate surface, and this helps to achieve a surface with low surface energy by increasing the reactivity with fluorosilane in a subsequent process.

[0099] When tetraalkoxysilane is used in excess, the reaction between silanols may excessively proceed, thereby causing strong shrinkage throughout the network, which may lead to problems of cracks or poor adhesion.

[0100] Therefore, when alkyl-trialkoxysilane and tetraalkoxysilane are used in an appropriate ratio, the problem of cracks occurring in the entire coating network can be prevented, and an appropriate amount of silanol reactive groups can be provided on the surface.

[0101] Furthermore, an organic acid may also be used in the first coating solution.

[0102] According to one embodiment of the present disclosure, the organic acid may be a carboxylic acid having 1 to 5 carbon atoms.

[0103] Specifically, the organic acid may be, for example, at least one selected from the group consisting of formic acid, acetic acid, and propionic acid.

[0104] The above organic acids are used as catalysts to promote the hydrolysis of silane groups in the composition and can play a role in determining the overall network structure. Under acidic conditions with low pH, the hydrolysis rate is better than the condensation reaction rate, so the bonds of the silane form a linear structure. On the other hand, under alkaline conditions, the condensation reaction rate is faster, thereby forming a granular structure. Inorganic acids such as hydrochloric acid can also be used instead of organic acids, but organic acids can be more beneficial in controlling the gel time.

[0105] In addition, the first coating solution may include about 1 to 50 parts by weight of tetraalkoxysilane based on 100 parts by weight of the alkyl-trialkoxysilane.

[0106] When too little tetraalkoxysilane is used, the amount of silanol that reacts with fluorosilane is too small, making it difficult to reduce the surface energy to an appropriate level. When too much tetraalkoxysilane is used, the stress acting on the entire coating network increases due to the excessive reaction of silanol, which may cause cracks in the coating or cause a problem of reduced adhesion of the coating.

[0107] In addition, the first coating solution may include about 1 to 10 parts by weight of the organic acid based on 100 parts by weight of the alkyl-trialkoxysilane.

[0108] When too little organic acid is included, the hydrolysis rate decreases, making it difficult to obtain an appropriate linear structure network, which may cause a problem of reduced physical properties of the coating film. When too much is included, it becomes difficult to control the reaction due to reduced gel time, and there is an excessive amount of organic acid that does not participate in the network, which may cause a problem of reduced mechanical properties of the coating film.

[0109] The pH of the first coating solution may be about 7 or less, about 5 or less, or about 3 or less, and about 1 or more, or about 2 or more.

[0110] pH can affect the hydrolysis rate and condensation reaction rate, and the difference between these two reaction rates determines the structure of the coating film. In addition, it affects the storage stability of the prepared coating solution.

[0111] From this viewpoint, a stable inorganic coating film can be obtained under acidic conditions having a pH within the above range.

[0112] In addition to the above components, the first coating solution may further include an organic solvent. Such an organic solvent may specifically include alcohol or ether, and the amount of the organic solvent may be appropriately selected in consideration of coating and drying after coating.

[0113] In addition, the thickness of the hydrophobic inorganic solidified layer may be about 0.05 μm to 20 μm, about 0.05 μm or more, or about 0.1 μm or more, and 20 μm or less, about 15 μm or less, or about 10 μm or less. When the thickness of the hydrophobic inorganic solidified layer is too thin, physical properties such as coating hardness may be reduced, and when the thickness of the hydrophobic inorganic solidified layer is too thick, there may be problems of coating cracking or peeling.

[0114] In addition, the fluorine-silane cured layer may be formed by curing a coating solution for forming a fluorine-silane cured layer (hereinafter, referred to as a second coating solution).

[0115] According to another embodiment of the present disclosure, the fluoro-silane cured layer may include a cured product of fluoropolyether silane.

[0116] According to one embodiment of the present disclosure, the fluoropolyether silane may be a compound including a moiety represented by the following Chemical Formulas 3-1 to 3-4.

[0117] [Chemical formula 3-1]

[0118] CF3-

[0119] [Chemical formula 3-2]

[0120] -CF2-CF2-O-

[0121] [Chemical formula 3-3]

[0122] -CF2-CF2-CF2-O-

[0123] [Chemical formula 3-4]

[0124] -Si(R31)(R32)(R33)

[0125] In Chemical Formula 3-4, R31 to R33 are each independently an alkoxy group having 1 to 5 carbon atoms.

[0126] The fluoropolyether silane is a compound having a fluorocarbon at one end, an alkoxysilane group at the other end, and a fluoroethoxy or fluoropropoxy group in the middle. It can form a hard coating by directly forming a covalent bond with the first coating, and can greatly reduce the surface energy of the coating due to a large number of fluorine chains.

[0127] In the second coating solution, fluoropolyether silane may be used together with an alkoxyfluoroalkyl-based solvent.

[0128] The alkoxyfluoroalkyl-based solvent used herein may be an ether compound represented by Chemical Formula 4 below.

[0129] CF3-(CF2)nO-(CH2)m-CH3

[0130] In the chemical formula, n and m may be an integer of 1 to 5, each independently.

[0131] In the ether compound, an alkyl group not substituted with fluorine is bonded to one side of oxygen, and an alkyl group in which all hydrogen atoms are replaced with fluorine is bonded to the other side of oxygen.

[0132] Such an ether compound is excellent in compatibility with the above-mentioned fluoropolyether silane compound, and can uniformly disperse the fluoropolyether silane compound in the second coating solution.

[0133] Furthermore, the fluorine oil layer may be formed by applying a coating solution for forming a fluorine oil layer (hereinafter, referred to as a third coating solution).

[0134] According to one embodiment of the present disclosure, the fluorine oil layer may include fluorinated polyether oil.

[0135] In addition, the fluorinated polyether oil may be a compound including groups represented by the following Chemical Formulas 4-1 to 4-3.

[0136] [Chemical formula 4-1]

[0137] CF3-

[0138] [Chemical formula 4-2]

[0139] -CF2-CF2-O-

[0140] [Chemical formula 4-3]

[0141] -CF2-CF2-CF2-O-.

[0142] The polyether oil is a perfluoropolyether containing CF3 at both ends and a perfluoroalkylene oxide repeating unit inside, and can achieve anti-fouling performance by maintaining excellent bonding with the fluoro-silane cured layer while providing a lubricating effect.

[0143] When the third coating solution is applied on the metal surface provided with the fluorosilane cured layer, the coating thickness may be about 0.1 μm to about 100 μm.

[0144] When the thickness is too thin, the lubricating effect may be reduced, and when the thickness is too thick, the lubricant may flow on the surface.

[0145] In addition, the sum of the thicknesses of the fluoro-silane cured layer and the fluoro oil layer may be about 0.1 μm to about 200 μm, about 0.1 μm or more, about 0.5 μm or more, or about 1 μm or more, and about 200 μm or less, about 150 μm or less, or about 100 μm or less.

[0146] When the cured thickness of the fluorosilane cured layer is too thin, the coating is not properly formed, and the fluorine content of the surface may be low, making it impossible to maintain a suitable low surface energy. When the cured thickness of the fluorosilane cured layer is too thick, the polymer silane may agglomerate, which may cause problems such as uneven coating and reduced economic efficiency.

[0147] Additionally, the anti-stick coating may include cured polydialkylsiloxane and silicone oil.

[0148] In this case, the silicone oil can be confined within the polydialkylsiloxane cross-linked polymer, which can show the excellent anti-adhesion performance and excellent durability of the coating. In addition, the coating surface remains solid, not smooth, and the silicone component does not flow out to the surface.

[0149] The anti-sticking coating may be formed of a two-component coating solution including a first liquid including polydialkylsiloxane having ethylenically unsaturated groups at both ends, an organic solvent, and silicone oil, and a second liquid including a cross-linking agent.

[0150] The polydialkylsiloxane may be a compound represented by Chemical Formula 5 below.

[0151] [Chemical formula 5]

[0152]

[0153] In Chemical Formula 5,

[0154] n is the repetition number of the siloxane repeating unit, and is an integer from 10 to 1,000,

[0155] R1 and R8 are each independently hydrogen or an alkyl group having 1 to 5 carbon atoms, and

[0156] R2 to R7 are each independently an alkyl group having 1 to 5 carbon atoms.

[0157] n may be about 10 or more, about 30 or more, or about 50 or more, and 1000 or less, about 500 or less, about 300 or less, or about 100 or less.

[0158] The polydialkylsiloxane monomer having ethylenically unsaturated groups at both ends is a type of long-chain monomer and can be polymerized with other monomer components.

[0159] When a coating layer is formed using such a polydialkylsiloxane monomer and a crosslinking agent and polymerization is performed, a crosslinking bond is formed by the polydialkylsiloxane monomer and the crosslinking agent, thereby forming a network structure by chains of dialkylsiloxane units.

[0160] In particular, the polydialkylsiloxane monomer as described above has almost the same chemical characteristics as silicone oil to achieve anti-adhesion performance, and has excellent compatibility with silicone oil. Therefore, silicone oil can be well captured by the polydialkylsiloxane in the network structure.

[0161] That is, when a coating layer is formed using the coating composition according to one aspect of the present disclosure, the silicone oil component is captured in the crosslinked network by the polydialkylsiloxane monomer and the crosslinking agent, thereby achieving an anti-adhesion effect. In addition, the silicone oil may not flow out of the crosslinked network.

[0162] Furthermore, the polydialkylsiloxane monomer as described above has a very strong bonding strength after cross-linking polymerization, and when a coating is formed, the durability of the coating can be greatly improved.

[0163] In addition, the number of siloxane repeating units in the polydialkylsiloxane monomer determines the length of the polydialkylsiloxane chain, and is ultimately related to the size of the voids in the cross-linked network structure after cross-linking polymerization. In addition, the size of the voids is directly related to whether silicone oil flows out of the cross-linked network.

[0164] In this regard, n can be about 10 or more, about 30 or more, or about 50 or more, and 1000 or less, about 500 or less, about 300 or less, or about 100 or less. However, the present disclosure is not necessarily limited thereto, and the value of n is more related to the molecular size of the silicone oil used together.

[0165] At this time, the weight ratio of the polydialkylsiloxane component:silicone oil is preferably about 1:5 to about 5:1, about 1:5 to about 3.5:1, or 1:3.5 to 2.5:1.

[0166] When too much silicone oil is included outside the above range, the mechanical properties of the anti-adhesion coating formed from the composition may be reduced, and curing for forming the coating may proceed slowly. In addition, when too little silicone oil is included, a problem of deterioration of anti-adhesion performance may occur.

[0167] In addition, the organic solvent may include at least one selected from the group consisting of methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, 2-butanol, xylene, and toluene.

[0168] The solvent is used to uniformly disperse the silicone oil, and the present disclosure is not necessarily limited thereto. A solvent having high solubility in the silicone oil may be appropriately selected from ketones, alcohols, acetates, and aromatic compounds and used.

[0169] According to one embodiment of the present disclosure, the viscosity of the silicone oil may be 500 cSt or less, or 1 cSt or more and less than 500 cSt. The lower limit may be about 1 cSt or more, about 5 cSt or more, or about 7 cSt or more, and the upper limit may be less than about 500 cSt, about 400 cSt or less, about 300 cSt or less, or about 150 cSt or less.

[0170] When the viscosity of silicone oil is too low, the amount of oil required to achieve the anti-sticking effect increases, which may reduce the adhesion to the adherend and cause coating peeling. When the viscosity of silicone oil is too high, the oil may flow out to the surface during coating, causing oil contamination.

[0171] Furthermore, it may be desirable to use silicone oil having a weight average molecular weight of about 1,000 to about 10,000, or about 1,000 to about 5,000.

[0172] As in the case where the viscosity of the silicone oil is low, when the molecular weight of the silicone oil is too low, the oil content increases to achieve the anti-adhesion effect, and this may cause problems such as peeling of the coating due to poor adhesion to the substrate when evaluating heat resistance. As in the case where the viscosity of the silicone oil is too high, when the molecular weight of the silicone oil is too high, the oil may flow out to the surface during coating and cause contamination by the oil.

[0173] According to one embodiment of the present disclosure, the first liquid may preferably further comprise a volatile branched siloxane compound.

[0174] Such volatile branched siloxanes can improve the dispersibility of silicone oils, polydialkylsiloxanes having ethylenically unsaturated groups, and other similar compounds, thereby improving the coating characteristics when forming a coating. In addition, the volatile branched siloxanes can be volatilized after application and removed from the coating.

[0175] Examples of such compounds include tetrakis(trialkylsiloxy)silane compounds, in which the alkyl group may be a linear or branched alkyl group having 1 to 4 carbon atoms.

[0176] More specifically, the volatile branched siloxane compound may include tetrakis(trimethylsiloxy)silane, tetrakis(triethylsiloxy)silane, tetrakis(tripropylsiloxy)silane, tetrakis(triisopropylsiloxy)silane, tetrakis(tributylsiloxy)silane, tetrakis(triisobutylsiloxy)silane, and the like.

[0177] Additionally, the crosslinking agent may include a siloxane compound containing three or more ethylenically unsaturated groups.

[0178] Specifically, the crosslinking agent may be a cyclic siloxane in which siloxane repeating units are linked as follows.

[0179]

[0180] In the above chemical formula, n may be 3 or more and 10 or less, or 3 to 7 or less, and

[0181] R1 and R2 are each independently an alkyl group having 1 to 5 carbon atoms, or an olefin having 2 to 5 carbon atoms containing an ethylenically unsaturated group, and at least one of R1 and R2 is an olefin having 2 to 5 carbon atoms containing an ethylenically unsaturated group.

[0182] In the coating composition according to one embodiment of the present disclosure, the polydialkylsiloxane having ethylenically unsaturated groups at both ends may be polymerized around the cross-linking agent to form a mesh-like cross-linked network.

[0183] According to another embodiment of the present disclosure, the first liquid and the second liquid may each independently further include silica surface-modified with an ethylenically unsaturated group.

[0184] Specifically, the silica compound surface-modified with an ethylenically unsaturated group may be in a form in which an ethylenically unsaturated group such as a vinyl group, an alkylated vinyl group having 1 to 5 carbon atoms, or a dialkylated vinyl group having 1 to 5 carbon atoms is attached to the terminal of a silanol group on the surface of the silica group.

[0185] In the silica compound surface-modified with an ethylenically unsaturated group, the ethylenically unsaturated group is connected to the above-mentioned crosslinking agent and / or the polydialkylsiloxane compound having ethylenically unsaturated groups at both ends during polymerization. Therefore, the silica compound surface-modified with an ethylenically unsaturated group can also play a role in forming a mesh-like crosslinked network, and in particular, can improve the mechanical properties and dimensional stability of the coating formed by polymerization.

[0186] At the same time, a method for forming an anti-fouling surface is provided, the method comprising the following steps: forming a first region including a hydrophobic inorganic solidified layer on a portion of a surface of a substrate; forming a second region including an anti-adhesion coating on at least a portion of the surface of the substrate other than the first region; and forming a lubricating layer in the first region.

[0187] For details on the coating solutions required to form the respective layers, refer to the above.

[0188] When applying the coating solution, the application method is not particularly limited, and a method commonly used in the technical field to which the present invention pertains may be selected, such as direct application with a tool such as a brush, spraying after appropriately adjusting the viscosity, or coating using a rod.

[0189] After application, drying may be performed at room temperature for about 10 minutes to about 1 hour. These drying conditions may vary depending on the type and amount of solvent used together.

[0190] After drying, curing may be performed at a temperature of about 100° C. to about 150° C. for about 30 minutes to about 2 hours.

[0191] Beneficial Effects

[0192] According to one embodiment of the present disclosure, it is possible to effectively prevent contaminants from being attached to the surface of an article. BRIEF DESCRIPTION OF THE DRAWINGS

[0193] Figure 1 The figure schematically shows a cross section of an anti-fouling surface in an article provided with the anti-fouling surface according to one embodiment of the present disclosure.

[0194] Figure 2 A diagram schematically showing an effect achieved by one embodiment of the present disclosure.

[0195] Figure 3 is a schematic diagram showing how a pollution prevention effect is achieved in an article according to one embodiment of the present disclosure.

[0196] Figure 4 The image schematically shows an anti-fouling surface observed from above in an article provided with the anti-fouling surface according to one embodiment of the present disclosure.

[0197] Figure 5 The image schematically shows an anti-fouling surface observed from above in an article provided with the anti-fouling surface according to another embodiment of the present disclosure.

[0198] Figure 6 and Figure 7 The figure schematically shows a cross section of an anti-fouling surface in an article provided with the anti-fouling surface according to one embodiment of the present disclosure.

[0199] Figure 8 A diagram briefly illustrating a process for manufacturing an article provided with an anti-fouling surface according to one embodiment of the present disclosure.

[0200] Fig. 9 is a photograph showing the evaluation of the anti-fouling performance of an anti-fouling article according to one embodiment of the present disclosure. DETAILED DESCRIPTION

[0201] Hereinafter, the functions and effects of the present invention will be described in more detail through specific examples. However, these examples are only for illustrative purposes, and the present invention is not intended to be limited by these examples.

[0202] The lubricating layer is composed of a hydrophobic inorganic cured layer, a fluorine-silane cured layer formed on the hydrophobic inorganic cured layer, and a fluorine oil layer formed on the fluorine-silane cured layer.

[0203] A coating solution for forming a hydrophobic inorganic cured layer (hereinafter, referred to as coating solution 1-1) was prepared as follows.

[0204] 5 parts by weight of methyl-trimethoxysilane as an alkyl-trialkoxysilane component, 1 part by weight of tetraethoxysilane as a tetraalkoxysilane component, and 4 parts by weight of 6% by weight acetic acid diluted in water as an organic acid component were mixed (pH: about 2.3).

[0205] Coating solution 1-1 was prepared by diluting 100 parts by weight of the above coating solution with about 50 parts by weight of isopropyl alcohol as a solvent.

[0206] A coating solution for forming a fluoro-silane cured layer (hereinafter, referred to as coating solution 1-2) was prepared as follows.

[0207] As the fluoropolyether silane component, Optool-DSX (perfluoropolyether silane manufactured by Daikin) was used by dissolving Optool-DSX at a concentration of 1% by weight in a solvent (Novec-7200 manufactured by 3M).

[0208] The coating solution for forming a fluorine oil layer (hereinafter referred to as coating solution 1-3) was prepared as follows.

[0209] As the fluorinated polyether oil component, DEMNUM-S65 (perfluoropolyether manufactured by Daikin) was used by dissolving it in a solvent (Novec-7200 manufactured by 3M) at a concentration of 1 wt % (surface energy after drying: 18 mN / m 2 ; based on manufacturer's TDS data).

[0210] A coating solution for forming an anti-sticking coating (hereinafter, referred to as a second coating solution) was prepared by using 2 parts by weight of Sylgard (R) 184 silicone elastomer kit (a base resin manufactured by Dow) and 0.2 parts by weight of a cross-linking agent as a polydialkylsiloxane having ethylenically unsaturated groups at both ends and a cross-linking agent, preparing 3.3 parts by weight of a polydimethylsiloxane-based silicone oil manufactured by Gelest having a viscosity of 10 cSt (kinematic viscosity, surface energy of 21 mN / m, based on the manufacturer's TDS data) measured at 25° C. as silicone oil, and using 3 parts by weight of methyl ethyl ketone as a solvent, followed by mixing.

[0211] Example 1

[0212] To produce articles with anti-fouling surfaces, follow Figure 8 The process shown in .

[0213] Figure 8 A diagram briefly illustrating a process for manufacturing an article provided with an anti-fouling surface according to one embodiment of the present disclosure.

[0214] As a substrate for forming a lubricating layer (hereinafter, referred to as a first substrate 110), a 1 cm×1 cm and 1 mm thick slide glass was prepared. The coating solution 1-1 was applied to the surface of the first substrate using a brush, dried at room temperature for about 30 minutes, and then cured at a temperature of about 130° C. for about 1 hour to form a hydrophobic inorganic solidified layer 210 having a thickness of about 5 μm.

[0215] The coating solution 1-2 was applied thereto using a brush, dried at room temperature for about 30 minutes, and then cured at a temperature of about 130° C. for about 1 hour to form a fluoro-silane cured layer 220 having a thickness of about 50 nm.

[0216] Separately, as a substrate for forming an anti-adhesive coating (hereinafter, referred to as a second substrate 120), a 3 cm×3 cm and 1 mm thick slide glass was prepared Then, the second coating solution was applied to the surface of the second substrate using a roller (about 1 mm based on dry thickness).

[0217] Before the second coating solution applied to the surface of the second substrate is completely cured, the first substrate is positioned so that the second coating solution surrounds the first substrate on which the fluoro-silane cured layer is formed in the center. Then, the article is cured at room temperature for about 6 hours to prepare a sample having an anti-adhesive coating 300 with a dry thickness of about 1 mm (surface energy of the anti-adhesive coating: 23 mJ / m 2 ).

[0218] The coating solution 1-3 was applied to a thickness of about 10 μm on the fluoro-silane cured layer 220 of the first substrate surrounded by the anti-adhesive coating layer of the second substrate using a brush to form a fluorine oil layer 230 .

[0219] Example 2

[0220] The procedure was performed in the same manner as in Example 1, except that the lubricating layer was formed to have a convex shape by using a convex lens having a diameter of 2 cm as a first substrate and a concave lens having a diameter of 3.5 cm as a second substrate.

[0221] Example 3

[0222] A coating solution (coating solution 1-3) for forming a fluorine oil layer was prepared as follows.

[0223] As the fluorinated polyether oil component, DEMNUM-S200 (perfluoropolyether manufactured by Daikin) was used by dissolving it in a solvent (Novec-7200 manufactured by 3M) at a concentration of 1 wt % (surface energy after curing: 19 mN / m 2 ; based on manufacturer's TDS data).

[0224] Other than that, the steps are the same as in Example 1.

[0225] Example 4

[0226] The procedure was carried out in the same manner as in Example 1, except that a Teflon sheet for antistatic purposes (manufacturer: ALPHAFLON, product name: AG018AD.AS, thickness: 0.18 mm, surface energy: 19 mN / m 2 ) were attached to the substrate to form a lubricating layer without using coating solutions 1-1 and 1-2.

[0227] Comparative Example 1

[0228] A lubricating layer is formed only in the center of the substrate surface (without an anti-stick coating).

[0229] As a substrate for forming a lubricating layer, a 3 cm×3 cm and 1 mm thick slide glass was prepared. Coating solution 1-1 was applied to the surface of the first substrate using a brush, dried at room temperature for about 30 minutes, and then cured at a temperature of about 130° C. for about 1 hour to form a hydrophobic inorganic cured layer with a thickness of about 5 μm.

[0230] The coating solution 1-2 was applied thereto using a brush, dried at room temperature for about 30 minutes, and then cured at a temperature of about 130° C. for about 1 hour to form a fluoro-silane cured layer having a thickness of about 50 nm.

[0231] The coating solution 1-3 was applied to the fluorine-silane cured layer 220 in a thickness of about 10 μm using a brush to form a fluorine oil layer.

[0232] Comparative Example 2

[0233] The anti-adhesive coating is formed only in the center of the substrate surface.

[0234] As a substrate, a slide glass of 3 cm×3 cm and 1 mm thick was prepared.

[0235] The second coating solution was applied to the center of the substrate in a size of 1 cm×1 cm using a brush and cured at room temperature for about 6 hours to prepare a test specimen having a coating layer with a dry thickness of about 1 mm.

[0236] For reference, both Comparative Examples 1 and 2 can be considered as examples of forming a hydrophobic surface on a slide glass having a hydrophilic surface.

[0237] Comparative Example 3

[0238] The steps were performed in the same manner as in Example 1, except that the process for forming the hydrophobic inorganic cured layer 210 and the fluoro-silane cured layer 220 was omitted, and only the fluorine oil layer 230 was formed by applying the coating solution 1-3 with a thickness of about 10 μm on the first substrate surrounded by the anti-adhesion coating of the second substrate using a brush.

[0239] Evaluation of antifouling performance

[0240] As pollutants for evaluation, a saturated aqueous solution of potassium chloride (KCl) (hydrophilic substance) and an instant adhesive (Loctite 495) (hydrophobic substance) were prepared.

[0241] 100 μl of each contaminant was dropped on the lubricating layer interface of Examples and Comparative Examples, and whether spontaneous migration of the contaminant from the lubricating layer to the anti-sticking coating layer occurred and whether the contaminant fell off from the anti-sticking coating layer were evaluated as O and X, respectively.

[0242] The results of each assessment are summarized in the table below.

[0243] [Table 1]

[0244]

[0245] In the antifouling article according to one embodiment of the present disclosure, even if contaminants adhere, the contaminants move from the lubricating layer to the anti-adhesive coating at the interface between the lubricating layer and the anti-adhesive coating, and then fall off from the anti-adhesive coating. As a result, it was determined that the antifouling performance was very excellent.

[0246] However, if only a lubricating layer is formed (Comparative Example 1), only an anti-sticking coating is formed (Comparative Example 2), or the lubricating layer is not properly formed even if it has a structure similar to that of the present disclosure, it is determined that the spontaneous movement or shedding of contaminants is not properly achieved, resulting in insufficient anti-contamination performance.

[0247] Fig. 9 is a photograph showing the evaluation of the anti-fouling performance of an anti-fouling article according to one embodiment of the present disclosure.

[0248] Reference Fig. 9 , it can be seen that the contaminants move from the lubricating layer to the anti-adhesion coating at the interface between the lubricating layer and the anti-adhesion coating, and then fall off from the anti-adhesion coating.

Claims

1. A product having an anti-pollution surface, the anti-pollution surface comprising: substrate; a first region that is present on a portion of the surface of the substrate and has a lubricating layer formed thereon; as well as A second region that exists on at least a portion of the surface of the substrate other than the first region and has an anti-adhesion coating formed thereon.

2. The article having an anti-fouling surface according to claim 1, The surface energy of the second region is greater than the surface energy of the first region.

3. The article having an anti-fouling surface according to claim 1, The surface energy of the lubricating layer is less than 20 mJ / m 2 .

4. The article having an anti-fouling surface according to claim 1, The surface energy of the anti-adhesion coating is 20 mJ / m 2 or larger.

5. The article having an anti-fouling surface according to claim 1, The surface energy of the anti-adhesion coating is 40 mJ / m 2 or smaller.

6. The article having an anti-fouling surface according to claim 1, The second region is formed to surround the first region.

7. The article having an anti-fouling surface according to claim 1, The first region is formed in a convex shape or a concave shape.

8. The article having an anti-fouling surface according to claim 1, The lubricating layer has a thickness of 0.1 μm to 200 μm.

9. The article having an anti-fouling surface according to claim 1, The lubricating layer includes a hydrophobic inorganic cured layer, a fluorine-silane cured layer formed on the hydrophobic inorganic cured layer, and a fluorine oil layer formed on the fluorine-silane cured layer.

10. The article having an anti-fouling surface according to claim 9, The hydrophobic inorganic cured layer comprises a cured product of an alkyl-trialkoxysilane and a tetraalkoxysilane.

11. The article having an anti-fouling surface according to claim 9, The thickness of the hydrophobic inorganic cured layer is 0.05 μm to 20 μm.

12. The article having an anti-fouling surface according to claim 9, The fluoro-silane cured layer comprises a cured product of fluoropolyether silane.

13. The article having an anti-fouling surface according to claim 9, The fluorine oil layer comprises fluorinated polyether oil.

14. The article having an anti-fouling surface according to claim 9, The total thickness of the fluorine-silane cured layer and the fluorine oil layer is 0.1 μm to 200 μm.

15. The article having an anti-fouling surface according to claim 1, The anti-adhesion coating comprises cured polydialkylsiloxane and silicone oil.

16. The article having an anti-fouling surface according to claim 15, The viscosity of the silicone oil is 1000 cSt or less.

17. A method for forming an anti-fouling surface, comprising the steps of: forming a first region including a hydrophobic inorganic cured layer on a portion of a surface of a substrate; forming a second region including an anti-sticking coating on at least a portion of the surface of the substrate other than the first region; as well as A lubricating layer is formed in the first region.

Citation Information

Patent Citations

  • Slippery self-lubricating polymer surfaces

    CN104704067A

  • Pattern formed body

    CN105814490A

  • Liquid and viscoelastic material repellent and Anti-biofouling coatings

    CN110072694A

  • Anti-reflective coated articles and method of making them