Method for stable blends of waste plastics and petroleum feedstocks fed to refinery units and method for making same
Through the preparation of a stable blend of petroleum-based raw materials and plastics, the problems of low regeneration efficiency and poor fuel quality in the existing technology are solved, efficient regeneration and production of high-value products are achieved, and the development of circular economy is supported.
Patent Information
- Application Number
- CN202380032655.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-01
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to effectively regenerate a large amount of single-use plastic waste, which leads to environmental pollution problems. The fuel quality generated by the pyrolysis method is poor and it is difficult to blend into the fuel supply on a large scale.
A stable blend of petroleum-based raw materials and 1-20% by weight of plastic is prepared by a two-step process of heating to higher than the melting point of the plastic and cooling to lower than the melting point to form a uniform liquid blend, which is directly fed to the refinery for conversion. Unit, avoid pyrolysis steps, improve regeneration efficiency and product quality.
It realizes efficient recycled plastic waste, produces high-value products such as gasoline, jet fuel and diesel, improves energy efficiency and environmental friendliness, and has the same quality as original polymers, supporting a larger circular economy.
Smart Images

Figure CN119013375A_ABST
Abstract
Description
Background Art
[0001] World plastic production is growing extremely rapidly. According to PlasticsEurope Market Research Group, world plastic production was 335 million tons in 2016, 348 million tons in 2017 and 359 million tons in 2018. According to McKinsey & Company, if the current trajectory continues, the global plastic waste volume is estimated to be about 260 million tons per year by 2016 and is expected to be 460 million tons per year by 2030.
[0002] Disposable plastic waste has become an increasingly important environmental issue. Currently, the options for recycling polyethylene and polypropylene waste plastics into value-added chemicals and fuel products seem to be few. Currently, only a small amount of polyethylene / polypropylene is regenerated via chemical regeneration, where the regenerated and cleaned plastic pellets are pyrolyzed in a pyrolysis unit to make fuels (naphtha, diesel), steam cracker feeds or slack wax. Most (more than 80%) are incinerated, landfilled or discarded.
[0003] Chemical regeneration methods via pyrolysis cannot have a big impact on the plastics industry at present. Current pyrolysis operations produce fuel components (products of naphtha and diesel ranges) of poor quality, but the amount is small enough so that these products can be blended into the fuel supply. However, if we must regenerate very large volumes of waste polyethylene and polypropylene to solve environmental problems, this simple blending is unsustainable. The products produced by the pyrolysis unit cannot be blended in large quantities (e.g., 5-20 volume % blending) into transportation fuels due to poor quality.
[0004] Methods for converting waste plastics into hydrocarbon lubricants are known. For example, U.S. Pat. No. 3,845,157 discloses the cracking of waste polyolefins or virgin polyolefins such as ethylene / olefin copolymers to form gaseous products, which are further processed to produce synthetic hydrocarbon lubricants. U.S. Pat. No. 4,642,401 discloses the production of liquid hydrocarbons by heating pulverized polyolefin waste at a temperature of 150-500° C. and a pressure of 20-300 bar. U.S. Pat. No. 5,849,964 discloses a method in which waste plastic materials are depolymerized into a volatile phase and a liquid phase. The volatile phase is separated into a gas phase and a condensate. The liquid phase, condensate and gas phase are refined into liquid fuel components using standard refining techniques. U.S. Pat. No. 6,143,940 discloses a process for converting waste plastics into heavy wax compositions. U.S. Pat. No. 6,150,577 discloses a method for converting waste plastics into lubricating oils. EP0620264 discloses a process for producing lubricating oil from waste or virgin polyolefins by thermally cracking the waste in a fluidized bed to form a waxy product, optionally using hydrotreatment, followed by catalytic isomerization and fractionation to recover the lubricating oil.
[0005] U.S. Publication No. 2021 / 0130699 discloses a method and system for producing regenerative hydrocarbons from regenerative waste. The regenerative waste is pyrolyzed to form a pyrolysis oil composition, at least a portion of which can then be cracked to form a regenerative olefin composition.
[0006] Other documents related to methods for converting waste plastics into lubricating oils include U.S. Patent Nos. 6288296; 6774272; 6822126; 7834226; 8088961; 8404912 and 8696994; and U.S. Patent Application Publication Nos. 2019 / 0161683; 2016 / 0362609; and 2016 / 0264885. The entire contents of the aforementioned patent documents are incorporated herein by reference.
[0007] Globally, the recycling or upgrading of plastic waste has attracted great interest, aiming to save resources and the environment. Mechanical recycling of plastic waste is quite limited due to the different types, properties, additives and contaminants in the collected plastics. Usually, the quality of the recycled plastics decreases. Chemical recycling into starting materials or value-added chemicals has become a more desired approach.
[0008] However, in order to achieve chemical recycling of industrial-scale single-use plastics to reduce their environmental impact, more robust methods are needed. Such methods may require unique treatment and manipulation of waste plastics. Summary of the invention
[0009] In one embodiment, a composition of a stable blend of waste plastic and petroleum-based feedstock is provided for direct conversion of waste plastic in a refinery processing unit.
[0010] The stable blend comprises a petroleum-based raw material and 1-20% by weight of plastic. In one embodiment, the plastic comprises mainly polyethylene and / or polypropylene. The plastic in the blend is present as finely dispersed microcrystalline particles with an average particle size of 10 microns to less than 100 microns, preferably less than 80 microns.
[0011] In one embodiment, a method for preparing a blend of plastic and petroleum is also provided. The method includes mixing a petroleum-based feedstock and a plastic together, and heating the mixture to a temperature above the melting point of the plastic, but not above 500° F. While continuing to mix, the plastic melt and petroleum feedstock liquid blend is cooled to a temperature below the melting point of the plastic.
[0012] Among other factors, the method of the present invention prepares a stable blend of plastics and petroleum-based raw materials. This blend of plastics and petroleum-based raw materials provides a carrier for efficiently and effectively feeding waste plastics to refinery processes to convert waste plastics into high-volume products, with good yields. It has been found that by preparing the blend of the present invention and feeding the blend to refinery operations, plastic waste can be efficiently and effectively regenerated, while also supplementing the operations of refineries in preparing more valuable products such as gasoline, jet fuel, base oil and diesel fuel. Polyethylene and polypropylene can also be efficiently and effectively produced from waste plastics. In fact, the overall regeneration method with the same product quality as the original polymer achieves positive economics. Using the blend of the present invention also saves energy and is more environmentally friendly than existing regeneration methods. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 Depicted is the current practice of pyrolyzing waste plastics to produce fuels or waxes (base case).
[0014] Figure 2 Depicted is the process of the present invention for preparing a hot, homogeneous liquid blend of plastic and petroleum feedstock, and how that blend can be fed to a refinery conversion unit.
[0015] Figure 3 The method of making the stable blend is described in detail, as well as how the stable blend can be fed to a refinery conversion unit.
[0016] Figure 4 Depicts the classification of plastic types for waste plastic recycling.
[0017] Figure 5 Shown are the results of thermogravimetric analysis (TGA) of low density polyethylene and polypropylene polymers.
[0018] Figure 6 Optical microscopy of blends prepared from polyethylene in bright field mode (A) and cross-polarized light mode (B) is shown.
[0019] Figure 7 Shown are optical microscopy examinations of blends prepared on polyethylene in the cross-polarized light mode at different temperatures during heating and cooling.
[0020] Figure 8 Optical microscopy of blends prepared from polypropylene in bright field mode (A) and cross-polarized light mode (B) is shown.
[0021] Fig. 9 Shown is optical microscopy of blends prepared on polypropylene in cross-polarized light mode at different temperatures during heating and cooling.
[0022] Fig.10 Graph depicting thermogravimetric analysis (TGA) of the thermal stability of four waste plastic samples. DETAILED DESCRIPTION
[0023] Novel blends of plastics and petroleum-based feedstocks, and methods of preparing stable blends of plastics and petroleum-based feedstocks for direct conversion of plastics in refinery processing units are disclosed.
[0024] In one embodiment, a method for preparing a stable blend of plastics, preferably waste plastics and oil is provided for storage, transportation or feeding to a refinery unit. The method comprises first selecting plastics, preferably waste plastics, containing polyethylene and / or polypropylene. These waste plastics are then sent through a blend preparation unit to make a stable blend of waste plastics and oil. The stable blend is fed to a refinery conversion unit for direct conversion of waste plastics into value-added chemicals and fuels.
[0025] The stable blend is made by a two-step process. The first step produces a hot, uniform liquid blend of a plastic melt and a petroleum feedstock. The preferred range of plastic composition in the blend is about 1-20 weight %. Preferred conditions for the preparation of the hot liquid blend include heating the plastic to a melting point higher than the plastic while vigorously mixing with the petroleum feedstock. Preferred process conditions include heating to a temperature of 250-500°F, a residence time of 5-240 minutes at the final heating temperature, and an atmospheric pressure of 0-10 psig. This can be carried out in an open atmosphere and preferably under an oxygen-free inert atmosphere.
[0026] In the second step, the hot blend is cooled to below the melting point of the plastic while continuing intensive mixing and then further cooled to a lower temperature, preferably ambient temperature, to produce a stable blend that is either an oily liquid or a waxy solid at ambient temperature, depending on the petroleum feedstock.
[0027] In one embodiment, the stable blend is made from a petroleum feedstock and 1-20% by weight of waste plastic, wherein the plastic is in the form of finely divided micron-sized particles having an average particle size of 10 microns to less than 100 microns.
[0028] Several advantages are achieved by the blends of the present invention and their uses. For example, stable blends of plastics and petroleum raw materials can be stored for long periods of time at ambient temperature and pressure. During storage, no agglomeration, sedimentation of polymer particles, and chemical / physical degradation of the blend are observed. This allows for easier handling of waste plastic materials for storage or transportation.
[0029] The stable blend can be easily handled by using standard pumps commonly used in refineries or warehouses or by using a pump equipped with a transport tank. Depending on the blend, some heating of the blend above its pour point is required to pump the blend for transfer or feeding to a conversion unit in a refinery. During heating, no agglomeration of the polymer was observed.
[0030] To feed the refinery unit, the stable blend is further heated above the melting point of the plastic to produce a homogenous liquid blend of petroleum and plastic. This hot homogenous liquid blend is directly fed to the refinery processing unit for converting waste plastic into high-value products at high yields.
[0031] Refinery conversion units such as fluid catalytic cracking (FCC) units, hydrocracking units and hydrotreating units convert the heat uniform liquid blend of plastics and petroleum raw materials in the presence of a catalyst, while converting plastics and petroleum raw materials. The presence of a catalyst in the conversion unit allows waste plastics to be converted into products of higher value at an operating temperature lower than the usual pyrolysis temperature. The yield of undesirable by-products (waste gas, tar, coke) is lower than that of typical pyrolysis methods. For hydroprocessing units (hydrocracking units and hydrotreating units), hydrogen is added to the unit to improve the conversion of plastics. The blend can produce additional synergistic benefits from the interaction of plastics and petroleum raw materials during the conversion process. Fluid catalytic cracking and hydrocracking methods are preferred modes for catalytic conversion of stable blends.
[0032] In one embodiment, a stable blend of plastic and petroleum feedstock can be sent to a coker unit to thermally convert the waste plastic. In this case, there is no substantial advantage in reactor temperature or product yield compared to the pyrolysis process. The advantage of the coker unit is its feed flexibility, which is reflected in the unit's ability to process blends with very high nitrogen, sulfur, and metal impurities.
[0033] Stable blends of plastics and petroleum feedstocks allow for more efficient regeneration of waste plastics. Use of the blends of the invention is much more energy efficient than current pyrolysis methods and allows for regeneration with a lower carbon footprint. By efficiently converting waste plastics back into virgin quality polymers or value-added chemicals and fuels, the improved process will allow for the establishment of a circular economy on a significantly larger scale.
[0034] A simplified process diagram of a basic example of a waste plastic pyrolysis method is shown in Figure 1 The preparation of hot homogeneous liquid blends of plastic and petroleum raw materials is shown in Figure 2 Shown in. Figure 3 The preparation of a stable blend of waste plastic and petroleum-based feedstock is depicted in detail. The figure depicts two process steps associated with the preparation of the blend.
[0035] As mentioned above, Figure 1A pyrolysis diagram of waste plastic fuel or wax conventionally operated in the current industry is shown. Typically, waste plastics are sorted together 1. Clean plastic waste 2 is converted into waste gas 4 and pyrolysis oil (liquid product) in a pyrolysis unit 3. The waste gas 4 from the pyrolysis unit 3 is used as fuel to operate the pyrolysis unit. An on-site distillation unit separates the pyrolysis oil to produce naphtha and diesel 5 products, which are sold to the fuel market. The heavy pyrolysis oil fraction 6 is recycled back to the pyrolysis unit 3 to maximize the fuel yield. The char 7 is removed from the pyrolysis unit 3. The heavy fraction 6 is rich in long-chain linear hydrocarbons and is very waxy (i.e., paraffin is formed when cooled to ambient temperature). Wax can be separated from the heavy fraction 6 and sold to the wax market.
[0036] However, using the blend of the present invention avoids pyrolysis of waste plastics. Instead, a stable blend of petroleum feedstock and waste plastics is prepared, which can be fed to a refinery unit. Thus, the pyrolysis step can be avoided, which is a significant energy saving.
[0037] The blend of the present invention is prepared in a hot blend preparation unit, where the operating temperature is above the melting point of the plastic (about 150-250° C.) to produce a hot homogeneous liquid blend of plastic and oil. The hot homogeneous liquid blend of plastic and oil can be directly fed to a refinery unit.
[0038] Alternatively, the blend is prepared in a stable blend preparation unit, wherein the hot uniform liquid blend is cooled to ambient temperature in a controlled manner to allow easy storage and transportation. By using this method, a stable blend can be prepared in a facility away from a refinery, and it can be transported to a refinery unit. The stable blend is then heated to a melting point higher than the plastic to feed the refinery conversion unit. The stable blend is a physical mixture of micron-sized plastic particles finely suspended in petroleum-based oil, wherein the average particle size of the plastic particles is 10 microns to less than 100 microns. The mixture is stable, and the plastic particles will not settle or agglomerate when stored for a long time.
[0039] When a single plastic is used, the meaning of heating the blend to a temperature above the melting point of that plastic is clear. However, if the waste plastic contains more than one waste plastic, the melting point of the plastic with the highest melting point is exceeded. Therefore, the melting points of all plastics must be exceeded. Similarly, if the blend is cooled to below the melting point of a plastic, the temperature must be cooled to below the melting points of all plastics contained in the blend.
[0040] Compared to pyrolysis units, these blend preparation units operate at much lower temperatures (~500-600°C vs. 120-250°C). Therefore, using the blends of the present invention in conjunction with a refinery can provide a significantly more energy efficient process compared to thermal cracking processes such as pyrolysis.
[0041] The use of the waste plastics / petroleum blend of the present invention also improves the total hydrocarbon yield obtained by the waste plastics. The increase in this yield is significant. The hydrocarbon yield using the blend of the present invention provides a hydrocarbon yield of up to 98%. On the contrary, a large amount of (about 10-30% by weight) light products and about 5-10% by weight of char are produced by the pyrolysis of waste plastics. As mentioned above, these light hydrocarbons are used as the fuel for running the pyrolysis device. Therefore, the liquid hydrocarbon yield from the pyrolysis device is at most 70-80%.
[0042] When the blend of the present invention is sent to a refinery unit such as an FCC unit, only a small amount of waste gas is produced. The catalytic cracking method used in the refinery unit is different from the thermal cracking method used in pyrolysis. When using a catalytic method, the generation of undesirable light fraction by-products such as methane and ethane is minimized. The refinery unit has an effective product fractionation, and all hydrocarbon product streams can be effectively utilized to produce high-value materials. The refinery co-feed will only produce about 2% of waste gas (H2, methane, ethane, ethylene). C3 streams and C4 streams are captured to produce useful products, such as cyclic polymers and / or high-quality fuel products. Therefore, the use of the oil / plastic blend of the present invention provides an increased hydrocarbon from plastic waste, and a more energy-efficient regeneration method compared to thermal methods such as pyrolysis. When considering the regeneration of waste plastics, the benefits of the blend of the present invention are significant.
[0043] In some cases, waste plastics are converted into clean fuels than the production of fuels by original petroleum raw materials requires less energy. Along with the collection of waste plastics and the improvement of processing, the gain of energy efficiency will further improve.Compared with the corresponding fuel manufactured by pure petroleum raw materials, such fuel produced by the blend of waste plastics and oil will have regeneration content and lower carbon footprint.Method of the present invention can produce gasoline, jet fuel and diesel with regeneration content and lower CO2 (lower carbon) clean footprint by waste plastics.
[0044] Figure 2 A method for preparing a hot, homogeneous blend of plastic and petroleum feedstock is shown, which can be used for direct injection into a refinery unit. The preferred range of plastic composition in the blend is about 1-20 weight %. If high molecular weight polypropylene (average molecular weight of 250,000 or greater) waste plastic or high density polyethylene (density greater than 0.93 g / cc) is used as the main (e.g., at least 50 weight %) waste plastic, the amount of waste plastic used in the blend is more preferably about 10 weight %. The reason is that the pour point and viscosity of the blend will be high. In one embodiment, the plastic may contain an average molecular weight M w In another embodiment, the plastic may include a polypropylene with an average molecular weight M of 5000 to 150000. w Polypropylene with a density of 150,000 to 400,000.
[0045] Preferred conditions for preparing a hot, homogeneous liquid blend include heating the plastic to above the melting point of the plastic while vigorously mixing with the petroleum feedstock. Preferred process conditions include heating to a temperature of 250-500°F with a residence time of 5-240 minutes at the final heating temperature, and an atmospheric pressure of 0-10 psig. This can be accomplished in an open atmosphere and preferably in an oxygen-free, inert atmosphere.
[0046] A hot, intimate blend of a plastic melt and a petroleum feedstock is prepared by mixing the petroleum feedstock and the plastic together, and then heating the mixture to above the melting point of the plastic, but not above 500°F, while mixing thoroughly. Alternatively, it is prepared by melting only the plastic, and then adding the plastic melt to the warm or hot petroleum feedstock, while mixing thoroughly. Alternatively, it is prepared by heating only the petroleum to a temperature above the melting point of the plastic, and then slowly adding the solid plastic to the hot petroleum liquid, while mixing the mixture thoroughly and maintaining the temperature above the melting point of the plastic.
[0047] With reference to the attached drawings Figure 2 , a step-by-step preparation method for preparing a hot homogeneous liquid blend is shown. Mixed waste plastics are sorted to produce post-consumer waste plastics 21 containing polyethylene and / or polypropylene. The waste plastics are cleaned 22 and then mixed with oil 24 in a hot blend preparation unit 23. After mixing in 23, a homogeneous blend of plastic and oil 25 is recovered. Optionally, a filtering device (not shown) can be added to remove any undissolved plastic particles or any solid impurities present in the hot liquid blend. The hot blend of plastic and oil is then combined with a refinery feedstock such as vacuum gas oil (VGO) 20 and becomes a mixture 26 of plastic / oil blend and VGO, which can then be sent to a refinery unit.
[0048] Figure 3 A method for preparing a stable blend of plastic and oil is shown. The stable blend is produced in a stable blend preparation unit by a two-step process. The first step produces a hot, homogeneous liquid blend of the plastic melt and the petroleum feedstock. Figure 2 The hot blends described are prepared the same. The preferred range of plastic composition in the blend is about 1-20 wt %. If high molecular weight polypropylene (average molecular weight of 250,000 or greater) waste plastics or high density polyethylene (density greater than 0.93 g / cc) is used as the main (e.g., at least 50 wt %) waste plastics, the amount of waste plastics used in the blend is more preferably about 10 wt %. The reason is that the pour point and viscosity of the blend will be high.
[0049] Preferred conditions for preparing a hot, homogeneous liquid blend include heating the plastic to above the melting point of the plastic while vigorously mixing with the petroleum feedstock. Preferred process conditions include heating to a temperature of 250-500°F with a residence time of 5-240 minutes at the final heating temperature, and an atmospheric pressure of 0-10 psig. This can be accomplished in an open atmosphere and preferably in an oxygen-free, inert atmosphere.
[0050] In the second step, the hot blend is cooled to below the melting point of the plastic while continuing to intensively mix with the petroleum feedstock, and then further cooled to a lower temperature, preferably ambient temperature, to produce a stable blend of plastic and oil.
[0051] It has been found that a stable blend is an intimate physical mixture of plastic and petroleum feedstock. The plastic is in a "deagglomerated" state. The plastic maintains a fine dispersion of solid particles in the petroleum feedstock at temperatures below the melting point of the plastic, particularly at ambient temperature. The blend is stable and can be easily stored and transported. In a refinery, the stable blend can be heated in a preheater to above the melting point of the plastic to produce a hot, uniform liquid blend of plastic and petroleum. The hot liquid blend can then be fed to a refinery unit as a co-feed with conventional refinery feeds.
[0052] exist Figure 3 , other details of the preparation of a stable blend are shown. The stable blend is manufactured in a two-step process in a stable blend preparation unit 100. As shown, clean waste 22 is sent to a stable blend preparation unit 100. The selected plastic waste 22 is heated and mixed with a refinery feedstock oil 24. The plastic waste is heated to a temperature higher than the melting point of the plastic to melt the plastic. The petroleum feedstock is mixed with the heated plastic at 23. The mixing is usually quite intense. The mixing and heating conditions can generally include heating at a temperature of about 250-500°F, with a residence time of 5-240 minutes at the final heating temperature. Heating and mixing can be completed in an open atmosphere or in an oxygen-free inert atmosphere. The result is a hot, uniform liquid blend 25 of plastic and oil. Optionally, a filtering device (not shown) can be added to remove any undissolved plastic particles or any solid impurities present in the hot, uniform liquid blend.
[0053] The hot blend 25 is then cooled to below the melting point of the plastic while continuing to mix the plastic with the petroleum feedstock 101. Cooling is typically continued, typically to ambient temperature, to produce a stable blend of the plastic and oil 102. At the refinery, the stable blend may be fed to a preheater 29 which heats the blend to above the melting point of the plastic to produce a mixture 26 of the plastic / oil blend and VGO which is then fed to the refinery conversion unit.
[0054] Preferred plastic starting materials for the blends of the present invention are sorted waste plastics containing mainly polyethylene and polypropylene (plastic recycling classification types 2, 4 and 5). The pre-sorted waste plastics are cleaned and shredded or pelletized to feed the blend preparation unit. Figure 4 Depicted is a classification of plastic types used for waste plastic recycling. Classification types 2, 4, and 5 are high density polyethylene, low density polyethylene, and polypropylene, respectively. Any combination of polyethylene and polypropylene waste plastics can be used. Classification 6 polystyrene can also be present in limited amounts.
[0055] Proper sorting of waste plastics is very important in order to minimize contaminants such as N, Cl and S. Plastic waste containing polyethylene terephthalate (plastic recycling classification type 1), polyvinyl chloride (plastic recycling classification type 3) and other polymers (plastic recycling classification type 7) needs to be sorted to less than 5%, preferably less than 1% and most preferably less than 0.1%. The method of the present invention can tolerate moderate amounts of polystyrene (plastic recycling classification type 6). Waste polystyrene needs to be sorted to less than 20%, preferably less than 10% and most preferably less than 5%.
[0056] Washing waste plastics can remove metal pollutants, such as sodium, calcium, magnesium, aluminum and non-metallic pollutants from other waste sources. Non-metallic pollutants include pollutants such as silicon dioxide from Group IV of the periodic table, pollutants such as phosphorus and nitrogen compounds from Group V, pollutants such as sulfur compounds from Group VI, and halide pollutants such as fluoride, chloride and iodide from Group VII. Residual metals, non-metallic pollutants and halides need to be removed to less than 50ppm, preferably less than 30ppm and most preferably less than 5ppm.
[0057] The petroleum blended with waste plastics is generally a petroleum feedstock for a refinery. Preferably, the petroleum blended oil is identical to the petroleum feedstock of a refinery. Petroleum may also include any petroleum-derived oil or petroleum-based materials. In one embodiment, the petroleum feedstock oil may include atmospheric gas oil, vacuum gas oil (VGO), atmospheric residue or heavy raw materials recovered from other refinery operations. In one embodiment, the petroleum feedstock oil blended with waste plastics includes VGO. In one embodiment, the petroleum feedstock oil blended with waste plastics includes light cycle oil (LCO), heavy cycle oil (HCO), FCC naphtha, gasoline, diesel, toluene and / or an aromatic solvent derived from petroleum.
[0058] In one embodiment, the petroleum feedstock used in the preparation of the blend includes vacuum gas oil, atmospheric gas oil, reformate, light cycle oil, heavy fuel oil, refinery hydrocarbon streams (containing toluene, xylenes, heptane or benzene), or pure toluene, pure xylenes, coker naphtha, C5-C6 isomerized paraffinic naphtha, FCC naphtha, hydrocracker bottoms, gasoline, jet fuel, diesel or some mixture thereof.
[0059] The most preferred petroleum feedstock is gas oil, heavy reformate or various recycle streams, which are fed to the catalytic conversion unit. The plastic and petroleum feedstock in the blend are then converted together into higher value products via catalytic conversion.
[0060] More than one petroleum feedstock can be used to optimize the blend properties. For example, viscosity and pour point can be lowered by adding lighter petroleum feedstocks such as light cycle oil, gasoline or diesel.
[0061] Optionally, a solvent such as benzene, toluene, xylene or heptane may be added to the blend to reduce the viscosity or pour point of the blend of plastic and petroleum feedstock for easier processing.
[0062] Without wishing to be bound by theory, the method of the present invention prepares a stable blend for catalytic conversion in a refinery unit, which is a close physical mixture of plastic and petroleum feedstock. The method of the present invention produces a stable blend of petroleum feedstock and plastic, wherein the plastic is in a "deagglomerated" state. The plastic retains its state of "finely dispersed" solid particles in the petroleum feedstock at ambient temperature. The blend is stable and can be easily stored and transported. In a refinery, the stable blend can be preheated to a uniform liquid blend of heat above the melting point of the plastic to produce plastic and petroleum, and then the hot liquid blend is fed to a conversion unit. Then both the petroleum feed and the plastic are simultaneously converted in a conversion unit such as a fluid catalytic cracking (FCC) or hydrocracking (HCR) unit using a typical refinery catalyst containing zeolite and other active components such as silica-alumina, alumina and clay.
[0063] The following examples are provided to further illustrate the methods of the present invention and their benefits. The examples are illustrative and not limiting.
[0064] Example 1: Properties of original plastic samples and petroleum feedstocks used for blend preparation
[0065] Four commercially available plastic samples were purchased: low-density polyethylene (LDPE, plastic A), high-density polyethylene (HDPE, plastic B), and two polypropylene samples with average molecular weights of ~12,000 (PP, plastic C) and ~250,000 (PP, plastic D), and their properties are summarized in Table 1.
[0066] Table 1 Properties of the original plastics used
[0067] The petroleum feedstocks used to prepare stable blends with plastics include hydrotreated vacuum gas oil (VGO), aromatics 100 solvent, light cycle oil (LCO) and diesel. Their properties are shown in Table 2 below. Aromatics 100 is a commercially available aromatic solvent made from petroleum-based materials and contains mainly C9-C 10 Dialkylbenzenes and trialkylbenzenes.
[0068] Table 2 Properties of petroleum raw materials used for blend preparation
[0069] Thermogravimetric analysis (TGA) was performed on Plastic A (LDPE) and Plastic C (Polypropylene) to verify the thermal stability of the plastic materials at blend preparation temperatures well above those at which the plastics dissolve. Figure 5 The TGA results shown indicate that the LDPE sample is stable up to 800°F and the polypropylene sample is stable up to 700°F.
[0070] Example 2 - Preparation of Stable Blends of VGO and Virgin Plastics
[0071] Several blends of VGO and plastic were prepared by adding plastic pellets (Plastics AD in Table 1) to hydrotreated vacuum gas oil (Petroleum Feed #1 in Table 2).
[0072] The following procedure was used. At ambient temperature, VGO feed (waxy solid) was added to a beaker. The VGO was heated with a heating mantle while stirring with a magnetic stirrer. The temperature of the VGO was gradually increased to 275-400°F, and then pre-weighed plastic pellets (solid) were slowly added to the hot VGO while stirring and heating. After the plastic pellets were dissolved, the stirred solution was then kept at the final temperature for an additional 30 minutes for blends with LDPE and plastic C polypropylene, or for 60 minutes for blends with HDPE and plastic D polypropylene. Visual observation indicated that the blend was completely homogeneous. Upon cooling to ambient temperature, the blend of plastic and VGO showed the visual appearance of a waxy solid of VGO, but the hardening temperature (or solidification temperature or pour point) was different from the starting VGO.
[0073] To assess material handling needs, the pour point (according to ASTM D5950-14) and viscosity (according to ASTM D445) of the blends were measured. Material stability was observed by visual observation. The blends of plastic melt and VGO were stable and no changes were observed during the 3 month observation period. Table 3 below summarizes a list of the prepared samples and their properties.
[0074] Table 3 Preparation of stable blends of plastics and VGO
[0075] Example 3 - Preparation of Stable Blends of Aromatic Solvents and Plastics
[0076] Several blends of the aromatic solvent and the four plastic samples were prepared by adding plastic pellets to the aromatic solvent (Petroleum Feed #2 of Table 2).
[0077] Preparation of these blends was performed using the procedure described in Example 2, except that the solvent temperature was 250°F prior to plastic addition and the final hold time was 60 minutes. The properties of the blends are shown in Table 4 below.
[0078] Table 4 Preparation of stable blends of plastics and aromatic solvents
[0079] Example 4 - Preparation of blends of VGO and virgin plastic
[0080] Several blends of vacuum gas oil (VGO) and two plastic samples (Plastics A and C of Table 1) were prepared by adding plastic pellets to hydrotreated vacuum gas oil (Petroleum Feed #1 of Table 2) using an autoclave.
[0081] The following procedure was used. At ambient temperature, pre-weighed plastic pellets (solid) and VGO feed (waxy solid) were added to an intermittent autoclave unit. The autoclave was purged with N2 gas to remove the air in the container, and then the inlet and outlet valves were closed. The mixture was stirred with an impeller at 1600RPM, while the mixture was heated to a target temperature of 177°C (350°F) or 232°C (450°F) by raising the temperature set point by 10°C every 10 minutes using an external heating jacket. Then, the temperature was maintained at the target temperature for 2 hours, and then cooled to ambient temperature while maintaining stirring. Pressure was monitored throughout the time. Typically, pressure accumulated up to 8psig at 450°F, and then returned to 1psig when cooled, indicating that there was no reaction between plastic and VGO. The slight pressure buildup near the target heating temperature was due to the evaporation of lightweight materials in VGO.
[0082] The blend product showed no visible plastic residue at ambient temperature and was completely homogeneous by visual observation. The blend of plastic and VGO showed the appearance of a waxy solid of VGO. The blend of plastic and VGO was stable and no changes were observed during the 3 month observation period.
[0083] To assess material handling needs, the pour point (according to ASTM D5950-14) and viscosity (according to ASTM D445) of the blends were measured. In addition, the content of hot heptane insoluble material was measured according to the ASTM D3279 procedure. The hot heptane insoluble method determines the weight percentage of insoluble material in hot heptane at 80°C in oil. The method uses a 0.8 micron membrane filter to separate insoluble materials. The heptane insoluble content provides information about the undissolved plastic in the blend. Table 5 below summarizes a list of the prepared samples and their properties.
[0084] Table 5 Preparation of stable blends of plastics and VGO
[0085] The pour point and viscosity values are used to guide the selection of equipment and operating procedures. The blends made by adding plastics show a moderate increase in pour point and viscosity compared to the pure VGO base case. These changes can be handled using typical refinery operating equipment with little or no changes. The blend tank is heated above the pour point to change the physical state of the blend to a liquid that is easily transferred. The liquid blend can then be transferred to a transport container or refinery unit via pumping using a pump or via discharge using gravity or via the use of a pressure differential.
[0086] The stable blends remain as physical mixtures at temperatures up to 80°C. The hot heptane insolubility test can be used to separate plastics from the blends. At 80°C, all waxes in VGO are dissolved in heptane solvent (Example 2-1 in Table 5). The weight percentage of heptane insoluble material comes from the undissolved plastics filtered out using a 0.8 micron membrane filter. The amount recovered as solid material matches well with the amount of plastic we added to the blend formulation. The heptane insoluble results in Table 5 clearly show that plastics are physical mixtures of solid particles dispersed in VGO in the blend at 80°C, and most of the plastic particles can be effectively separated using a 0.8 micron filter. Optical microscopy analysis shows that the plastics are finely dispersed microcrystalline particles with a particle size of about 10 microns to 80 microns (shown in Example 5).
[0087] Example 5A - Optical Microscopy of Stable Blends with Low Density Polyethylene
[0088] Figure 6Optical microscopy images of the prepared blend (Example 4-1) of polyethylene (Plastic A) and VGO in bright field mode (A) and cross-polarized light mode (B) at ambient temperature are shown. At ambient temperature, the blend is a physical mixture of finely dispersed plastic particles and petroleum. The average particle size of the polyethylene particles is 10 microns. The fine micron-sized polyethylene is uniformly distributed in the VGO, and they have the visual appearance of micelles.
[0089] Figure 7 Optical microscopy (OLM) images of the prepared blends of polyethylene (Plastic A) and VGO (Example 4-1) in the cross-polarized light mode at different temperatures during heating and cooling are shown. At ambient temperature, the polyethylene remains as microcrystalline particles with an average particle size of 10 microns ( Figure 6 and Figure 7 A). When heated to 90°C, most of the polyethylene melts, and at 106°C, all of the polyethylene is completely melted and forms a homogeneous hot liquid blend with VGO. When cooled, the polyethylene begins to recrystallize at about 90°C and becomes crystalline particles again at an ambient temperature of 25°C ( Figure 7 F) and Figure 7 A shows the plastic particles in the prepared blend compared to Figure 7 The recrystallized plastic shown in F exhibits a larger average particle size of about 19 microns, which may be due to the fact that the blend was cooled in the OLM stage without stirring the plastic / VGO blend. The results indicate that if the blend is cooled without stirring, the blend may contain larger sized plastic particles. This finding reveals that continued vigorous stirring during the cooling step is desirable to produce a stable blend of petroleum and micron-sized plastic particles.
[0090] Example 5B - Optical Microscopy of Stable Blends with Polypropylene
[0091] Figure 8 Optical microscopy images of the prepared blend of polypropylene (plastic C) and VGO (Example 4-4) at ambient temperature in bright field mode (A) and cross-polarized light mode (B) are shown. The average particle size of the polypropylene is about 20 microns. Fine crystallites of polypropylene are uniformly distributed in the VGO, and they have the visual appearance of micelles.
[0092] Fig. 9 Optical microscopy (OLM) images of the prepared blends of polypropylene (Plastic C) and VGO (Example 4-4) in the cross-polarized light mode at different temperatures during heating and cooling are shown. At ambient temperature, the polypropylene remains as microcrystalline particles with an average particle size of 20 microns ( Figure 8 and Fig. 9A). Upon heating to 129°C, most of the polyethylene melts, and at 132°C, all of the polypropylene is completely melted and forms a homogeneous hot liquid blend. Upon cooling, the polypropylene begins to recrystallize at about 93°C and becomes crystalline particles again at ambient temperature. The recrystallized particles have a larger average particle size of about 78 microns because the blend is cooled in the OLM stage without stirring with VGO. Similarly, Fig. 9 A shows the plastic particles in the prepared blend compared to Fig. 9 The recrystallized plastic shown in F appears to have a much larger average particle size. This finding reveals that continued vigorous stirring during the cooling step is desirable to produce a stable blend of petroleum and microcrystalline plastic particles.
[0093] Example 6 - Preparation of blends of VGO and plastics with HDPE and higher molecular weight polypropylene
[0094] Two blends of vacuum gas oil (VGO) and plastic (each of Plastics B and D in Table 1) were prepared using an autoclave. The VGO was similar to petroleum feed #1, but had a higher pour point. These blends were prepared using the procedure described in Example 4, except that the heating temperature was 232°C (450°F) and the holding time at 450°F was 4 hours. The blends produced were solid at ambient temperature and had the appearance of VGO wax. Table 6 shows the properties of the blends.
[0095] Table 6 Preparation of stable blends of plastics and VGO
[0096] Example 7 - Viscosity Improvement of Stable Blends Added with Light Petroleum
[0097] This example shows that the addition of light cycle oil (LCO, Petroleum Feed #3) or diesel (Petroleum Feed #4) significantly reduces the viscosity, making feed handling easier.
[0098] Example 7-1 was prepared by adding 20 wt% light cycle oil to Example 6-2 (a blend of 10 wt% HDPE Plastic B in VGO). The preparation of this blend was performed using a procedure similar to that described in Example 4. The mixture was heated to 350°F, held at that temperature for 1 hour, and then cooled to ambient temperature while stirring the entire time. The pressure was monitored during the heating period. The pressure built up to 4 psig at 350°F and then cooled back to 0 psig, indicating that there was no reaction between the plastic, VGO, and LCO. The slight pressure buildup near the target temperature was due to the evaporation of the light material in the LGO.
[0099] Example 7-2 was prepared via a method comparable to Example 7-1, except that diesel was used instead of LCO.
[0100] The final products, Examples 7-1 and 7-2, were light brown solids of waxy appearance at ambient temperature, which appeared homogeneous upon visual observation and did not contain any visible plastic residues. The blends of plastic, LCO (or diesel) and VGO were stable and no changes were observed over the 2 week observation period. Table 7 below summarizes a list of the samples prepared and their properties.
[0101] Table 7 Preparation of Stable Blends of Plastic, VGO and Second Petroleum Feed
[0102] Use of light petroleum secondary feedstock to improve physical properties
[0103] Example 8 - Direct Conversion of Plastics and VGO via FCC Using USY Catalyst
[0104] To study the effect of waste plastics and vacuum gas oil processing in a refinery FCC unit, laboratory tests of a fluid catalytic cracking (FCC) process were conducted using a stable blend of plastics and VGO (Examples 2-3, 2-9, 2-10) using an FCC catalyst containing USY zeolite. The catalyst was an equilibrium catalyst taken from a commercial FCC unit.
[0105] The FCC experiment was conducted on a C-type ACE (Advanced Cracking Evaluation) unit manufactured by Kayser Technology Inc. using a regenerated equilibrium catalyst (Ecat) from a refinery. The reactor was a fixed fluidized reactor using N2 as a fluidizing gas. The catalytic cracking experiment was conducted at atmospheric pressure and a reactor temperature of 975°F. The catalyst / oil ratio was varied between 5 and 8 by changing the amount of the catalyst. The gas products were collected and analyzed using a refinery gas analyzer (RGA) equipped with a GC with an FID detector. In-situ regeneration of the spent catalyst was performed at 1300°F in the presence of air, and the regenerated flue gas was sent through an IR chamber to determine the flue gas composition to calculate the coke yield. The liquid product was weighed and analyzed in the GC for simulated distillation (D2887) and C5 composition analysis. Using material balance, the yields of coke, dry gas components, LPG components, gasoline (C5-430°F), light cycle oil (LCO, 430-650°F), and heavy cycle oil (HCO, 650°F+) were determined. The results are summarized in Table 8 below.
[0106] Table 8 Evaluation of plastics co-fed to FCC with USY catalyst
[0107] *: Conversion rate – 430℉ + Distill to 430°F - Conversion rate
[0108] **: Octane number, (R+M) / 2, estimated from detailed hydrocarbon GC of FCC gasoline.
[0109] The results in Table 8 show that 5-10 wt% plastic co-feed produces only very minor changes to FCC unit performance, indicating that co-processing of up to 10 wt% plastic is readily feasible. Up to 20% may be run without any performance issues, but suitable equipment with good control is required to handle the increased viscosity and pour point.
[0110] Plastics are more easily cracked than VGO, so the conversion of the blend increases slightly. The addition of plastics in the FCC feed results in a very slight increase in coke yield, but there is no significant change in dry gas yield. A moderate increase in LPG and C3 and C4 olefin yields, as well as a slight reduction in LCO and HCO yields were observed. Gasoline yields are similar. Due to the paraffinic nature of the cracked products made from plastics, blends with plastics reduce the octane number by about 1-2 values. Due to the flexibility of refinery operations, these octane losses can be compensated by blending or by adjusting FCC process operations and catalyst / additive formulations. The hydrocarbon composition of all these co-feed products is well within the typical FCC gasoline range.
[0111] Example 9: Properties of Waste Plastic Samples and Blend Formulations
[0112] Four waste plastic samples were purchased for blend preparation and their properties are summarized in Table 9. FT-IR was used to determine the general properties of the plastics. In addition to determining the main polymer species, the FT-IR data revealed that all of these recycled plastics contained varying amounts of calcium carbonate and talc. In order to assess the amount of potentially recoverable hydrocarbons, each sample was calcined at 1000°F for 3 hours under N2. The recoverable hydrocarbons were assumed to be equal to the % loss on ignition (LOI). The inorganic residues from the calcination were analyzed using ICP analysis. Using the LOI values and ICP analysis, the weight % of impurities in the original plastics were assessed and reported in Table 9 below. The most common impurities in waste plastics are Ca, Mg, Si, and Ti, which can come from plastic consumer product manufacturing, such as calcium carbonate, silica, and talc, which are commonly used filler materials. Al, Fe, P, and Zn are also present in large quantities.
[0113] Table 9 Properties of waste plastics
[0114] Thermogravimetric analysis (TGA) of waste plastic samples was performed to verify the thermal stability of plastic materials at temperatures well above the melt preparation temperature. Fig.10 The TGA results shown in show that the waste plastic sample is stable up to 700°F.
[0115] Blends of the above waste plastic samples and VGO were prepared using the procedure in Example 4, except that the dissolution temperature was 400° F. After 10 wt% plastic was dissolved, some solid precipitation was observed, which may be from filler materials, and the blends generally exhibited very high viscosities, which may be due to the presence of solids. For the dissolution of 5 wt% plastic, the blends were filtered to remove the solid filler materials, where a significant drop in viscosity was observed.
[0116] Table 10 Preparation of stable blends of waste plastics and VGO
[0117] Example 10: Direct conversion of waste plastic and VGO blends via FCC using USY catalyst
[0118] To study the impact of processing waste plastics and vacuum gas oil in a refinery FCC unit, laboratory tests of a fluid catalytic cracking (FCC) process were conducted on a stable blend of waste plastics and VGO using an FCC catalyst containing USY zeolite. The plastics used were waste plastic #1 (Plastic E) and waste plastic #2 (Plastic F). A base case with only VGO feed (Example 10-1) was compared to two blend runs; a 5 / 95% blend containing Plastic E / VGO (Example 10-2) and a 5 / 95 wt% blend of Plastic F / VGO (Example 10-3). The catalyst was an equilibrium catalyst taken from a commercial FCC unit.
[0119] Table 11 Evaluation of waste plastics co-fed to FCC with USY catalyst
[0120] *: Conversion rate – 430℉ + Distill to 430°F - Conversion rate
[0121] **: Octane number, (R+M) / 2, estimated from detailed hydrocarbon GC of FCC gasoline.
[0122] The results in Table 11 show that 5 wt% waste plastic co-feed only resulted in minor changes in FCC unit performance, indicating that co-processing of 5 wt% waste plastic is readily feasible.
[0123] Waste plastics are easier to crack than VGO, so the conversion of the blend increases slightly. The waste plastics added in the FCC feed cause a very slight increase in coke yield, but the dry gas yield changes very little. A moderate increase in LGP, C3 and C4 olefin yields and a slight reduction in LCO and HCO yields are observed. Gasoline yield is similar. Due to the paraffinic nature of the cracked products made of plastics, the blend with plastics reduces the octane number by about 1-1.5 values. Due to the flexibility of refinery operations, this octane loss can be easily compensated by blending or by adjusting FCC process operations and catalyst / additive formulations. The hydrocarbon composition of all co-feed products is well within the typical FCC gasoline range.
[0124] As used herein, the phrases "comprising / containing / including" are intended to be open ended transitions, meaning that the recited elements are included but not necessarily that other unnamed elements are excluded. The phrase "consisting essentially of is intended to indicate the exclusion of other elements having any essential importance to the composition. The phrase "consisting of is intended to be transitional, meaning that all elements other than the recited elements are excluded, except for only trace amounts of impurities.
[0125] All patents and publications mentioned herein are hereby incorporated by reference, without being inconsistent with this document. It should be understood that some of the above-mentioned structures, functions and operations of the above-mentioned embodiments are not necessary for practicing the present invention, and are included in the specification only for the integrity of one or more exemplary embodiments. In addition, it should be understood that the specific structures, functions and operations set forth in the above-mentioned patents and publications can be practiced in conjunction with the present invention, but they are not necessary for the practice of the present invention. Therefore, it should be understood that the present invention can be practiced in other ways as specifically described without actually departing from the spirit and scope of the present invention as defined by the appended claims.
Claims
1. A blend of a petroleum feedstock and 1-20 wt% plastic, based on the weight of the blend, wherein the plastic comprises polyethylene and / or polypropylene, and the plastic in the blend comprises finely dispersed micron-sized particles having an average particle size of 10 microns to less than 100 microns.
2. The blend according to claim 1, wherein the amount of plastic in the blend is 1-10 wt% of the blend.
3. The blend of claim 1, wherein the plastic comprises low density polyethylene.
4. The blend of claim 1, wherein the plastic comprises high density polyethylene.
5. The blend of claim 4, wherein the blend comprises 1-10 wt% high density polyethylene.
6. The blend according to claim 1, wherein the plastic comprises polypropylene having an average molecular weight Mw of 5,000 to 150,000.
7. The blend of claim 1, wherein the plastic comprises polypropylene having an average molecular weight Mw of 150,000 to 400,000.
8. The blend of claim 7, wherein the blend comprises 1-10 wt% polypropylene.
9. The blend of claim 1, wherein the plastic comprises a mixture of polyethylene and polypropylene.
10. The blend of claim 1, wherein the plastic is a waste plastic mixture comprising polyethylene and polypropylene.
11. The blend of claim 1 wherein the finely divided particles have an average particle size of 10 to 50 microns.
12. The blend of claim 1 wherein the finely divided particles have an average particle size of 10 to less than 100 microns.
13. The blend of claim 1, wherein the petroleum feedstock in the blend comprises vacuum gas oil, atmospheric gas oil, reformate, light cycle oil, heavy fuel oil, a refinery hydrocarbon stream containing toluene, xylene, heptane or benzene, coker naphtha, C5-C6 isomerized paraffin naphtha, FCC naphtha, hydrocracker bottoms, gasoline, jet fuel, diesel or mixtures thereof.
14. The blend of claim 1, wherein the petroleum feedstock in the blend comprises gas oil or heavy reformate.
15. The blend of claim 13, wherein the blend comprises light cycle oil, gasoline, or diesel.
16. The blend of claim 14, wherein the blend comprises light cycle oil, gasoline, or diesel.
17. The blend of claim 13, wherein the blend comprises benzene, toluene, xylene, or heptane.
18. The blend of claim 14, wherein the blend comprises benzene, toluene, xylene, or heptane.
19. The blend of claim 1 wherein the temperature of the blend is above the melting point of the plastic and is a hot homogeneous liquid blend.
20. The blend of claim 19 further comprising a petroleum feedstock added to the blend.
21. A method for preparing a blend of plastic and petroleum, comprising: (a) mixing together a petroleum feed and a plastic comprising polyethylene and / or polypropylene and, while mixing, heating the mixture to a temperature above the melting point of the plastic but less than 500°F; and (b) cooling the plastic melt and petroleum feedstock liquid blend to a temperature below the melting point of the plastic.
22. The method of claim 21, wherein the cooling in (b) is carried out with continuous stirring.
23. The method of claim 21, wherein the heating is conducted at a temperature of 250-450°F and the residence time at the final heating temperature is 5-240 minutes.
24. The method of claim 21, wherein cooling is continued until ambient temperature is reached.
25. The method of claim 21, wherein the plastic is a waste plastic mixture comprising polyethylene and polypropylene.
Citation Information
Patent Citations
Spherical polymer particles are produced by melting a thermoplastic, adding a molecular liquid phase dispersing agent, forming droplets, cooling and liquid phase separation.
DE10122492A1
Suspension of a waste plastic and a vacuum gas oil, its preparation and use in fcc
EP3878926A1
Process For Co-Conversion Of Waste Plastics And Hydrocarbon Feedstock
US20220041940A1
Process for preparing a free-flowing, modified polypropylene powder
US5093399A
Method for conversion of waste plastics to lube oil
US6150577A