Optical laminate and optical member comprising same
By stacking optical laminates with specific angles and materials in the phase difference plate, the problem of uneven phase difference after deformation of the phase difference plate is solved, and high performance display and uniform heat resistance over a wide wavelength range are achieved.
Patent Information
- Application Number
- CN202380033695.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-31
- Filing Date
- 2023-04-05
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, it is difficult to maintain uniformity of phase difference after deformation processing, resulting in a degradation of the display performance of the stereoscopic image display device, especially in a wide wavelength range, it is difficult to realize the high-performance λ/4-piece function.
By stacking λ/2 and λ/4 sheets in a specific material and angle along the thickness direction, ensure that the angle of the slow axis is between 24.6° to 30.6° and 90.5° to 96.5° and meet the specific refractive index relationship and stickiness The connection layer is distributed to reduce the uneven phase difference caused by deformation.
The uniformity of phase difference is achieved in a wide wavelength range, the display performance of the stereoscopic image display device is improved, the appearance of ghost images is avoided, and the heat resistance and uniformity of optical characteristics of the optical laminate are improved.
Smart Images

Figure CN119013593A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an optical layered body and an optical member including the same. Background Art
[0002] A member having an in-plane retardation Re(λ) of approximately λ / 2 at a wavelength λ is also called a λ / 2 plate, and a member having an in-plane retardation Re(λ) of approximately λ / 4 at a wavelength λ is also called a λ / 4 plate.
[0003] For example, Patent Document 1 describes a phase difference plate that provides in-plane retardation to transmitted light by laminating one λ / 2 plate and one λ / 4 plate on both surfaces of a glass plate.
[0004] Furthermore, Patent Document 2 describes a phase difference plate obtained by laminating two λ / 2 plates and one λ / 4 plate.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2003-344652;
[0008] Patent document 2: International Publication No. 2020 / 209354. Summary of the invention
[0009] Problem that the invention aims to solve
[0010] In order to make the phase difference plate that provides an in-plane retardation of λ / 4 to transmitted light function in a wide wavelength range (particularly in the visible light region), the technology of Patent Document 2 is used to laminate two λ / 2 plates and one λ / 4 plate to obtain a phase difference plate.
[0011] However, the phase difference plate can be used as a component of an image display device. In recent years, a high-performance phase difference plate capable of functioning as a λ / 4 plate in a wide wavelength range has been required in order to be incorporated into an optical system of a stereoscopic image display device that displays a stereoscopic image.
[0012] Here, in order to combine with an optical element (for example, a pancake lens) included in the optical system of an image display device such as a stereoscopic image display device, when the phase difference plate is deformed, the phase difference originally possessed by the phase difference plate may become uneven, affecting the quality of the image display device.
[0013] Particularly in a stereoscopic image display device, a slight reduction in the performance or quality of a phase difference plate may lead to a reduction in display performance (for example, display of an unexpected image (ghost image)).
[0014] In the techniques of Patent Documents 1 and 2, it is sometimes difficult to obtain a phase difference plate that reduces phase difference unevenness (phase difference spots) caused by deformation processing and can function as a λ / 4 plate that can be incorporated into a three-dimensional image display device to achieve excellent display performance.
[0015] Therefore, there is a need for: an optical layered body that reduces phase difference unevenness caused by deformation processing and can realize a stereoscopic image display device with excellent display performance; and an optical member including the optical layered body.
[0016] Solutions for solving problems
[0017] The present inventors conducted intensive studies to solve the above-mentioned problems and found that the above-mentioned problems can be solved by stacking two λ / 2 plates and one λ / 4 plate formed of specified materials in the thickness direction in such a way that their slow axes form a specified angle, thereby completing the present invention.
[0018] That is, the present invention provides the following solutions.
[0019] [1] An optical layered body comprising, in order, a first λ / 2 plate formed only of a material M1, a second λ / 2 plate formed only of a material M2, and a λ / 4 plate formed only of a material M3,
[0020] The angle between the slow axis of the first λ / 2 plate and the slow axis of the second λ / 2 plate is greater than or equal to 24.6° and less than or equal to 30.6°.
[0021] The angle between the slow axis of the first λ / 2 plate and the slow axis of the λ / 4 plate is greater than or equal to 90.5° and less than or equal to 96.5°.
[0022] The first λ / 2 plate satisfies any one of the following formulas (1a), (1b), and (1c):
[0023] nx1>ny1≈nz1(1a)
[0024] nx1>ny1>nz1(1b)
[0025] nx1>nz1>ny1(1c)
[0026] Here, nx1 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the first λ / 2 plate, ny1 represents the refractive index in the direction orthogonal to the direction of nx1 in the in-plane direction of the first λ / 2 plate, nz1 represents the refractive index in the thickness direction of the first λ / 2 plate,
[0027] The second λ / 2 plate satisfies any one of the following formulas (2a), (2b), and (2c):
[0028] nx2>ny2≈nz2(2a)
[0029] nx2>ny2>nz2(2b)
[0030] nx2>nz2>ny2(2c)
[0031] Here, nx2 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the second λ / 2 plate, ny2 represents the refractive index in the direction orthogonal to the direction of nx2 in the in-plane direction of the second λ / 2 plate, and nz2 represents the refractive index in the thickness direction of the second λ / 2 plate.
[0032] The λ / 4 plate satisfies any one of the following formulas (3a), (3b), and (3c):
[0033] nx3>ny3≈nz3(3a)
[0034] nx3>ny3>nz3(3b)
[0035] nx3>nz3>ny3(3c)
[0036] Here, nx3 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the λ / 4 plate, ny3 represents the refractive index in the direction orthogonal to the direction of nx3 in the in-plane direction of the λ / 4 plate, and nz3 represents the refractive index in the thickness direction of the λ / 4 plate.
[0037] The photoelastic coefficients of the material M1, the material M2, and the material M3 are each independently 10×10 - 13 cm 2 / dyn or below,
[0038] The material M1, the material M2, and the material M3 each contain more than 50 wt% of a specific polymer (P).
[0039] [2] The optical layered body according to [1], wherein
[0040] The first λ / 2 plate satisfies the above formula (1a) or formula (1b),
[0041] The second λ / 2 plate satisfies the above formula (2a) or formula (2b),
[0042] The λ / 4 plate satisfies the above formula (3a) or formula (3b).
[0043] [3] The optical layered body according to [1] or [2], wherein
[0044] The first λ / 2 plate satisfies the above formula (1c),
[0045] The second λ / 2 plate satisfies the above formula (2c),
[0046] The λ / 4 plate satisfies the above formula (3c).
[0047] [4] The optical layered body according to any one of [1] to [3], wherein
[0048] The NZ coefficient NZ1 of the first λ / 2 plate satisfies 0.0<NZ1<1.0,
[0049] The NZ coefficient NZ2 of the second λ / 2 plate satisfies 0.0<NZ2<1.0,
[0050] The NZ coefficient NZ3 of the above λ / 4 plate satisfies 0.0<NZ3<1.0,
[0051] Here,
[0052] NZ1 is represented by the following formula: NZ1 = (nx1-nz1) / (nx1-ny1),
[0053] NZ2 is represented by the following formula: NZ2 = (nx2-nz2) / (nx2-ny2),
[0054] NZ3 is represented by the following formula: NZ3 = (nx3-nz3) / (nx3-ny3),
[0055] nx1, ny1, nz1, nx2, ny2, nz2, nx3, ny3, and nz3 have the same meanings as above.
[0056] [5] The optical layered body according to any one of [1] to [4], wherein the polymer (P) is an alicyclic structure-containing polymer.
[0057] [6] The optical layered body according to any one of [1] to [5], comprising a first adhesive layer between the first λ / 2 plate and the second λ / 2 plate, and a second adhesive layer between the second λ / 2 plate and the λ / 4 plate.
[0058] [7] The optical layered body according to [6], wherein the optical layered body satisfies the following formula (4), formula (5), formula (6), and formula (7).
[0059] |I1―Ia1|≤0.02 (4)
[0060] |I2―Ia1|≤0.02 (5)
[0061] |I2―Ia2|≤0.02 (6)
[0062] |I3―Ia2|≤0.02 (7)
[0063] Here,
[0064] I1 represents the refractive index of the first λ / 2 plate,
[0065] I2 represents the refractive index of the second λ / 2 plate,
[0066] I3 represents the refractive index of the above-mentioned λ / 4 plate,
[0067] Ia1 represents the refractive index of the first adhesive layer,
[0068] Ia2 represents the refractive index of the second adhesive layer.
[0069] [8] An optical member comprising a transparent member and the optical layered body according to any one of [1] to [7] provided on the transparent member.
[0070] [9] The optical member according to [8], wherein the transparent member has a curved surface, and the optical layered body is provided on the curved surface of the transparent member.
[0071]
[10] The optical layered body according to any one of [1] to [7], wherein the optical layered body is used to be bonded to the curved surface of a transparent member having a curved surface.
[0072] Furthermore, the present invention provides the following solutions.
[0073] [2-1] An optical layered body comprising, in order, a first λ / 2 plate formed only of a material M1, a second λ / 2 plate formed only of a material M2, and a λ / 4 plate formed only of a material M3,
[0074] The angle between the slow axis of the first λ / 2 plate and the slow axis of the second λ / 2 plate is greater than or equal to 24.6° and less than or equal to 30.6°.
[0075] The angle between the slow axis of the first λ / 2 plate and the slow axis of the λ / 4 plate is greater than or equal to 90.5° and less than or equal to 96.5°.
[0076] The first λ / 2 plate satisfies the following formula (1a) or formula (1b),
[0077] nx1>ny1≈nz1(1a)
[0078] nx1>ny1>nz1(1b)
[0079] Here, nx1 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the first λ / 2 plate, ny1 represents the refractive index in the direction orthogonal to the direction of nx1 in the in-plane direction of the first λ / 2 plate, nz1 represents the refractive index in the thickness direction of the first λ / 2 plate,
[0080] The second λ / 2 plate satisfies the following formula (2a) or formula (2b),
[0081] nx2>ny2≈nz2(2a)
[0082] nx2>ny2>nz2(2b)
[0083] Here, nx2 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the second λ / 2 plate, ny2 represents the refractive index in the direction orthogonal to the direction of nx2 in the in-plane direction of the second λ / 2 plate, and nz2 represents the refractive index in the thickness direction of the second λ / 2 plate.
[0084] The λ / 4 plate satisfies the following formula (3a) or formula (3b),
[0085] nx3>ny3≈nz3(3a)
[0086] nx3>ny3>nz3(3b)
[0087] Here, nx3 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the λ / 4 plate, ny3 represents the refractive index in the direction orthogonal to the direction of nx3 in the in-plane direction of the λ / 4 plate, and nz3 represents the refractive index in the thickness direction of the λ / 4 plate.
[0088] The photoelastic coefficients of the material M1, the material M2, and the material M3 are each independently 10×10 - 13 cm 2 / dyn or below,
[0089] The material M1, the material M2, and the material M3 each contain more than 50 wt % of a specific polymer (P).
[0090] [2-2] The optical layered body according to [2-1], wherein the polymer (P) is an alicyclic structure-containing polymer.
[0091] [2-3] The optical layered body according to [2-1] or [2-2], comprising a first adhesive layer between the first λ / 2 plate and the second λ / 2 plate, and a second adhesive layer between the second λ / 2 plate and the λ / 4 plate.
[0092] [2-4] The optical layered body according to [2-3], wherein the optical layered body satisfies the following formula (4), formula (5), formula (6), and formula (7).
[0093] |I1―Ia1|≤0.02 (4)
[0094] |I2―Ia1|≤0.02 (5)
[0095] |I2―Ia2|≤0.02 (6)
[0096] |I3―Ia2|≤0.02 (7)
[0097] Here,
[0098] I1 represents the refractive index of the first λ / 2 plate,
[0099] I2 represents the refractive index of the second λ / 2 plate,
[0100] I3 represents the refractive index of the above-mentioned λ / 4 plate,
[0101] Ia1 represents the refractive index of the first adhesive layer,
[0102] Ia2 represents the refractive index of the second adhesive layer.
[0103] [2-5] An optical member including a transparent member and the optical layered body according to any one of [2-1] to [2-4] provided on the transparent member.
[0104] [2-6] The optical member according to [2-5], wherein the transparent member has a curved surface, and the optical layered body is provided on the curved surface of the transparent member.
[0105] [2-7] The optical layered body according to any one of [2-1] to [2-4], wherein the optical layered body is used to be bonded to the curved surface of a transparent member having a curved surface.
[0106] Effects of the Invention
[0107] According to the present invention, there can be provided: an optical layered body which reduces phase difference unevenness caused by deformation processing and can realize a stereoscopic image display device with excellent display performance; and an optical member including the optical layered body. BRIEF DESCRIPTION OF THE DRAWINGS
[0108] Figure 1 It is a cross-sectional view schematically showing the optical layered body according to the first embodiment of the present invention.
[0109] Figure 2 This is a schematic exploded perspective view of the optical layered body according to the first embodiment of the present invention.
[0110] Figure 3 It is a cross-sectional view schematically showing an optical layered body according to a second embodiment of the present invention.
[0111] Figure 4 It is a cross-sectional view schematically showing an optical member according to a third embodiment of the present invention. DETAILED DESCRIPTION
[0112] Hereinafter, the present invention will be described in detail by showing the embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and can be arbitrarily changed within the scope of the claims of the present invention and the scope equivalent thereto. The structural elements of the embodiments shown below can be appropriately combined. In addition, sometimes the same structural elements are marked with the same symbols in the drawings and their description is omitted.
[0113] In the following description, unless otherwise specified, "polarizer", "circular polarizer", "plate", "λ / 2 plate" and "λ / 4 plate" include not only rigid members but also flexible members such as resin films.
[0114] In the following description, unless otherwise specified, the slow axis of a film, layer or sheet means the slow axis within the plane of the film, layer or sheet.
[0115] In the following description, unless otherwise specified, the angle formed by the optical axis (slow axis, transmission axis, absorption axis, etc.) of each layer in a member having multiple layers means the angle when the layer is observed in the thickness direction.
[0116] In the following description, the λ / 2 plate refers to a plate having an in-plane retardation Re(λ) of approximately λ / 2 at a wavelength λ.
[0117] Furthermore, the λ / 4 plate refers to a plate in which the in-plane retardation Re(λ) at a wavelength λ is approximately λ / 4.
[0118] The in-plane retardation Re(λ) of the λ / 2 plate is preferably in the range of (λ / 2±35) nm, more preferably in the range of (λ / 2±15) nm, and ideally is λ / 2 nm.
[0119] The in-plane retardation Re(λ) of the λ / 4 plate is preferably in the range of (λ / 4±30) nm, more preferably in the range of (λ / 4±10) nm, and ideally is λ / 4 nm.
[0120] When λ is 550 nm, the in-plane retardation Re(550) of the λ / 2 plate is preferably 240 nm or more, more preferably 260 nm or more, and is preferably 310 nm or less, more preferably 290 nm or less.
[0121] When λ is 550 nm, the in-plane retardation Re(550) of the λ / 4 plate is preferably 110 nm or more, more preferably 130 nm or more, and is preferably 170 nm or less, more preferably 150 nm or less.
[0122] In the following description, unless otherwise specified, for the angular relationship between the direction of the optical axis (slow axis, transmission axis, absorption axis, etc.) in the plane of a certain product (optical laminate, circular polarizer, etc.) and the geometric direction (length direction and width direction of the film, etc.), the displacement in one direction is defined as positive and the displacement in the other direction is defined as negative, and the positive and negative directions are defined in common in the structural elements in the product. For example, in a certain circular polarizer, "the angle between the absorption axis of the circular polarizer and the slow axis of the first λ / 2 plate is A°, the angle between the slow axis of the first λ / 2 plate and the slow axis of the second λ / 2 plate is B°, and the angle between the slow axis of the first λ / 2 plate and the slow axis of the λ / 4 plate is C°" means the following two cases:
[0123] When the circular polarizer is observed from one side, the slow axis of the first λ / 2 plate is offset by A° clockwise from the absorption axis of the circular polarizer, the slow axis of the second λ / 2 plate is offset by B° clockwise from the slow axis of the first λ / 2 plate, and the slow axis of the λ / 4 plate is offset by C° clockwise from the slow axis of the first λ / 2 plate.
[0124] When the circular polarizer is observed from one side, the slow axis of the first λ / 2 plate is offset by A° counterclockwise from the absorption axis of the circular polarizer, the slow axis of the second λ / 2 plate is offset by B° counterclockwise from the slow axis of the first λ / 2 plate, and the slow axis of the λ / 4 plate is offset by C° counterclockwise from the slow axis of the first λ / 2 plate.
[0125] In the following description, unless otherwise specified, the front direction of a certain film refers to the normal direction of the principal surface of the film, specifically, the direction of the principal surface at a polar angle of 0° and an azimuth angle of 0°.
[0126] In the following description, unless otherwise specified, a material having positive intrinsic birefringence refers to a material having a refractive index in the stretching direction greater than a refractive index in the direction perpendicular thereto. In addition, unless otherwise specified, a material having negative intrinsic birefringence refers to a material having a refractive index in the stretching direction less than a refractive index in the direction perpendicular thereto. The value of intrinsic birefringence can be calculated based on the dielectric constant distribution.
[0127] Examples of materials having positive intrinsic birefringence include resins containing polymers having positive intrinsic birefringence. Examples of polymers having positive intrinsic birefringence include: polymers containing alicyclic structures; polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyarylene sulfides such as polyphenylene sulfide; polyvinyl alcohol; polycarbonate; polyarylate; cellulose ester; polyether sulfone; polysulfone; polyarylene sulfone; polyvinyl chloride; rod-shaped liquid crystal polymers, etc.
[0128] In the following description, unless otherwise stated, the in-plane retardation Re of the layer is a value represented by Re=(nx-ny)×d. In addition, unless otherwise stated, the retardation Rth in the thickness direction of the layer is a value represented by Rth=[{(nx+ny) / 2}-nz]×d. Furthermore, unless otherwise stated, the NZ coefficient NZ represents a value represented by NZ=Rth / Re+0.5, and can therefore be represented by NZ=(nx-nz) / (nx-ny). Here, nx represents the refractive index in the direction that provides the maximum refractive index in the direction perpendicular to the thickness direction of the layer (in-plane direction). Ny represents the refractive index in the direction orthogonal to the direction of nx in the above-mentioned in-plane direction of the layer. Nz represents the refractive index in the thickness direction of the layer. d represents the thickness of the layer. Unless otherwise stated, the measuring wavelength is 550nm.
[0129] In the following description, unless otherwise specified, the directions of the elements "parallel", "perpendicular" and "orthogonal" may include errors within the range of, for example, ±3°, ±2° or ±1°, within the range that does not impair the effects of the present invention.
[0130] In the following description, unless otherwise specified, adhesives include not only adhesives in a narrow sense (adhesives having a shear storage modulus of 1 MPa to 500 MPa at 23°C after irradiation with energy rays or heat treatment) but also adhesives having a shear storage modulus of less than 1 MPa at 23°C.
[0131] Therefore, the "adhesive layer" includes not only a layer of an adhesive in a narrow sense but also a layer of a tackifier.
[0132] "Substantially the same" also includes situations where they are completely identical.
[0133] [1. Optical laminate]
[0134] [1.1. First embodiment]
[0135] The optical layered body according to the first embodiment of the present invention includes a first λ / 2 plate, a second λ / 2 plate, and a λ / 4 plate in this order.
[0136] Figure 1 It is a cross-sectional view schematically showing the optical layered body according to the first embodiment of the present invention.
[0137] like Figure 1 As shown, the optical stack 100 includes a first λ / 2 plate 10 , a second λ / 2 plate 20 , and a λ / 4 plate 30 in this order along the thickness direction.
[0138] The optical layered body may include an arbitrary layer in addition to the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate. Examples of the arbitrary layer include an adhesive layer, a support, and a functional layer.
[0139] The optical layered body may include one or more retardation layers as arbitrary layers. As the retardation layer, for example, a retardation layer (posC) satisfying the following formula (8) can be mentioned.
[0140] nx4≈ny4<nz4 (8)
[0141] Here, nx4 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the layer, ny4 represents the refractive index in the direction orthogonal to the direction of nx4 in the above-mentioned in-plane direction of the layer, and nz4 represents the refractive index in the thickness direction of the layer.
[0142] A layer (posC) satisfying the formula (8) means that the layer is a so-called positive C plate.
[0143] In formula (8), nx4≈ny4 means that the value of nx4 is substantially the same as the value of ny4. Specifically, the value of |nx4-ny4| is usually 15 nm or less, preferably 10 nm or less, usually 0 nm or more, and may be 0 nm.
[0144] In addition, the phase difference layer (posC) functioning as a positive C plate can be arranged at any position of the optical laminate.
[0145] may be arranged between the first λ / 2 plate and the second λ / 2 plate; and / or
[0146] It may be arranged between the second λ / 2 plate and the λ / 4 plate; and / or
[0147] It may be arranged on the side of the first λ / 2 plate opposite to the second λ / 2 plate; and / or
[0148] It can be arranged on the side of the λ / 4 plate opposite to the second λ / 2 plate.
[0149] As an embodiment, it is particularly preferred that the optical stack includes three phase difference layers (posC) and is sequentially configured with a first λ / 2 plate, a first phase difference layer (posC), a second λ / 2 plate, a second phase difference layer (posC), a λ / 4 plate, and a third phase difference layer (posC).
[0150] When a phase difference layer that functions as a positive C plate is included in addition to the above-mentioned first λ / 2 plate, second λ / 2 plate, and λ / 4 plate, the optical stack can function well as a 1 / 4 wave plate in a wide wavelength range (especially the visible light region), and in particular can improve its function as a wide-band 1 / 4 wave plate in the inclined direction.
[0151] In this embodiment, the first λ / 2 plate 10 and the second λ / 2 plate 20 are in direct contact with each other without any layer interposed therebetween, and the second λ / 2 plate 20 and the λ / 4 plate 30 are in direct contact with each other without any layer interposed therebetween.
[0152] In another embodiment, any layer may be present between the first λ / 2 plate and the second λ / 2 plate.
[0153] Furthermore, any layer may be present between the second λ / 2 plate and the λ / 4 plate.
[0154] Figure 2 This is a schematic exploded perspective view of the optical layered body according to the first embodiment of the present invention.
[0155] like Figure 2 As shown, the slow axis D1 of the first λ / 2 plate 10 and the slow axis D2 of the second λ / 2 plate form an angle θ 12 Angle θ 12 The range is usually 24.6° or more, preferably 25.6° or more, more preferably 26.6° or more, further preferably 27.1° or more, and is usually 30.6° or less, preferably 29.6° or less, more preferably 28.6° or less, further preferably 28.1° or less.
[0156] In addition, the slow axis D1 of the first λ / 2 plate 10 and the slow axis D3 of the λ / 4 plate 30 form an angle θ 13 Angle θ 13 The range is usually 90.5° or more, preferably 91.5° or more, more preferably 92.5° or more, further preferably 93.1° or more, and usually 96.5° or less, preferably 95.5° or less, more preferably 94.5° or less, further preferably 94.0° or less.
[0157] The first λ / 2 plate usually satisfies any one of the following formula (1a), formula (1b), and formula (1c).
[0158] nx1>ny1≈nz1(1a)
[0159] nx1>ny1>nz1(1b)
[0160] nx1>nz1>ny1(1c)
[0161] Here, nx1 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the above-mentioned first λ / 2 plate, ny1 represents the refractive index in the direction orthogonal to the direction of nx1 in the in-plane direction of the above-mentioned first λ / 2 plate, and nz1 represents the refractive index in the thickness direction of the above-mentioned first λ / 2 plate.
[0162] The second λ / 2 plate usually satisfies any one of the following formulas (2a), (2b), and (2c).
[0163] nx2>ny2≈nz2(2a)
[0164] nx2>ny2>nz2(2b)
[0165] nx2>nz2>ny2(2c)
[0166] Here, nx2 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the above-mentioned second λ / 2 plate, ny2 represents the refractive index in the direction orthogonal to the direction of nx2 in the in-plane direction of the above-mentioned second λ / 2 plate, and nz2 represents the refractive index in the thickness direction of the above-mentioned second λ / 2 plate.
[0167] The λ / 4 plate usually satisfies any one of the following formulas (3a), (3b), and (3c).
[0168] nx3>ny3≈nz3(3a)
[0169] nx3>ny3>nz3(3b)
[0170] nx3>nz3>ny3(3c)
[0171] Here, nx3 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the λ / 4 plate, ny3 represents the refractive index in the direction orthogonal to the direction of nx3 in the in-plane direction of the λ / 4 plate, and nz3 represents the refractive index in the thickness direction of the λ / 4 plate.
[0172] The sheet satisfying formula (1a), formula (2a) or formula (3a) is referred to as the so-called positive A plate, the sheet satisfying formula (1b), formula (2b) or formula (3b) is referred to as the so-called negative B plate, and the sheet satisfying formula (1c), formula (2c) or formula (3c) is referred to as the so-called Z plate.
[0173] In formula (1a), ny1≈nz1 means that the value of ny1 is substantially the same as the value of nz1. Specifically, the value of |ny1-nz1| is usually 15 nm or less, preferably 10 nm or less, and usually 0 nm or more, and may be 0 nm.
[0174] In formula (2a), ny2≈nz2 means that the value of ny2 is substantially the same as the value of nz2. Specifically, the value of |ny2-nz2| is usually 15 nm or less, preferably 10 nm or less, usually 0 nm or more, and may be 0 nm.
[0175] In formula (3a), ny3≈nz3 means that the value of ny3 is substantially the same as the value of nz3. Specifically, the value of |ny3-nz3| is usually 15 nm or less, preferably 10 nm or less, usually 0 nm or more, and may be 0 nm.
[0176] In one embodiment, the optical stack preferably has a first λ / 2 plate satisfying formula (1a) or (1b); and / or preferably has a second λ / 2 plate satisfying formula (2a) or (2b); and / or preferably has a λ / 4 plate satisfying formula (3a) or (3b).
[0177] More preferably, in the optical laminate, the first λ / 2 plate satisfies the formula (1a) or (1b), the second λ / 2 plate satisfies the formula (2a) or (2b), and the λ / 4 plate satisfies the formula (3a) or (3b).
[0178] This makes it possible to produce an optical layered body that functions particularly well as a λ / 4 plate in a wide wavelength range.
[0179] In another embodiment, the optical stack preferably has a first λ / 2 plate satisfying formula (1c); and / or preferably has a second λ / 2 plate satisfying formula (2c); and / or preferably has a λ / 4 plate satisfying formula (3c).
[0180] In the optical layered body, more preferably, the first λ / 2 plate satisfies the formula (1c), the second λ / 2 plate satisfies the formula (2c), and the λ / 4 plate satisfies the formula (3c).
[0181] This allows the optical layered body to function particularly well as a λ / 4 plate in a wide wavelength range and in all directions in the front direction and in the oblique direction.
[0182] The NZ coefficient NZ1 of the first λ / 2 plate preferably satisfies 0.0<NZ1≤1.0; and / or the NZ coefficient NZ2 of the second λ / 2 plate preferably satisfies 0.0<NZ2≤1.0; and / or the NZ coefficient NZ3 of the λ / 4 plate preferably satisfies 0.0<NZ3≤1.0. Thus, the optical laminate can function particularly well as a λ / 4 plate in a wide wavelength range.
[0183] More preferably, the NZ coefficient NZ1 of the first λ / 2 plate satisfies 0.0<NZ1≤1.0, the NZ coefficient NZ2 of the second λ / 2 plate satisfies 0.0<NZ2≤1.0, and the NZ coefficient NZ3 of the λ / 4 plate satisfies 0.0<NZ3≤1.0.
[0184] It is further preferred that the NZ coefficient NZ1 of the first λ / 2 plate satisfies 0.0<NZ1<1.0, the NZ coefficient NZ2 of the second λ / 2 plate satisfies 0.0<NZ2<1.0, and the NZ coefficient NZ3 of the λ / 4 plate satisfies 0.0<NZ3<1.0. Thus, the optical laminate can function particularly well as a λ / 4 plate in a wide wavelength range and in all directions in the front direction and further in the oblique direction.
[0185] The NZ coefficient NZ1 of the first λ / 2 plate is preferably greater than 0, more preferably 0.4 or more, further preferably 0.45 or more, preferably 1.0 or less, more preferably less than 1.0, further preferably 0.6 or less, and particularly preferably 0.55 or less.
[0186] The NZ coefficient NZ2 of the second λ / 2 plate is preferably greater than 0, more preferably 0.4 or more, further preferably 0.45 or more, preferably 1.0 or less, more preferably less than 1.0, further preferably 0.6 or less, and particularly preferably 0.55 or less.
[0187] The NZ coefficient NZ3 of the λ / 4 plate is preferably greater than 0, more preferably 0.4 or more, further preferably 0.45 or more, preferably 1.0 or less, more preferably less than 1.0, further preferably 0.6 or less, and particularly preferably 0.55 or less.
[0188] The NZ coefficient can be appropriately adjusted by adjusting the stretching conditions (stretching temperature, stretching ratio, etc.) of the resin film used to manufacture the first λ / 2 sheet, the second λ / 2 sheet, or the λ / 4 sheet, adjusting the NZ coefficient of the resin film, etc. The NZ coefficient of the resin film can be adjusted by a method of contacting the resin film with a solvent. The NZ coefficient of the resin film can be adjusted to less than 1 by contacting the resin film with a solvent. By stretching the resin film having the above-adjusted NZ coefficient, a stretched film having an NZ coefficient greater than 0 and less than 1 can be manufactured. As a method for manufacturing a stretched film having an NZ coefficient greater than 0 and less than 1, for example, the method described in International Publication No. 2021 / 107108 can be cited.
[0189] The first λ / 2 plate is usually formed of only the material M1 and contains only the material M1.
[0190] The second λ / 2 plate is usually formed of only the material M2 and contains only the material M2.
[0191] The λ / 4 plate is usually formed of only the material M3 and contains only the material M3.
[0192] As materials that can form a layer that satisfies the above-mentioned formula (1a), formula (1b), formula (1c), formula (2a), formula (2b), formula (2c), formula (3a), formula (3b), or formula (3c), a variety of materials are known, and these materials can be used as any of the materials M1 to M3.
[0193] The photoelastic coefficients of material M1, material M2, and material M3 are independent of each other and are usually 10×10 -13 cm 2 / dyn or less, preferably 8×10 -13 cm 2 / dyn or less, more preferably 6×10 -13 cm 2 / dyn or less, more preferably 5×10 -13 cm 2 / dyn or less, more preferably 4×10 -13 cm 2 / dyn or less, preferably close to 0cm 2 The absolute values of the photoelastic coefficients of the material M1, the material M2, and the material M3 are preferably independently 10×10 -13 cm 2 / dyn or less, more preferably 8×10 -13 cm 2 / dyn or less, more preferably 6×10 -13 cm 2 / dyn or less, more preferably 5×10 -13 cm 2 / dyn or less, more preferably 4×10 -13 cm 2 The photoelastic coefficients of the material M1, the material M2, and the material M3 are preferably 0 cm / s or less, respectively, independently of each other. 2 / dyn or above.
[0194] The angle θ of the optical layered body of this embodiment 12 The range and angle θ 13The range is within the above range, and the material M1, the material M2, and the material M3 each independently have a photoelastic coefficient within the above range. As a result, the optical laminate can function well as a λ / 4 plate in a wide wavelength range, and it is not easy to produce phase difference changes and uneven phase difference (phase difference spots) even if it is used in a state deformed from the initial shape. Therefore, the optical laminate can function well as a λ / 4 plate in a wide wavelength range even if it is processed along the curved surface of an optical component with a curved surface assembled in a stereoscopic image display device, etc. As a result, a stereoscopic image display device with excellent display characteristics can be manufactured from the optical laminate.
[0195] As a material having a photoelastic coefficient in the above range, various materials are known, and these materials can be used as any of the materials M1 to M3. Examples of the material having a photoelastic coefficient in the above range include materials containing alicyclic structure-containing polymers and polymethyl methacrylate.
[0196] The absolute value of the difference between the photoelastic coefficient C1 of the material M1 and the photoelastic coefficient C2 of the material M2, the absolute value of the difference between the photoelastic coefficient C2 of the material M2 and the photoelastic coefficient C3 of the material M3, and the absolute value of the difference between the photoelastic coefficient C1 of the material M1 and the photoelastic coefficient C3 of the material M3 are preferably 10×10 -13 cm 2 / dyn or less, more preferably 5×10 -13 cm 2 / dyn or less, more preferably 2×10 -13 cm 2 / dyn or less, usually 0cm 2 / dyn or more, ideally 0cm 2 / dyn.
[0197] Thus, when the optical stack is deformed, the in-plane retardation of the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate changes to the same extent or does not change, so when the optical stack is deformed, the phase difference change of the optical stack can be effectively suppressed.
[0198] The photoelastic coefficient of a material can be measured by the following method.
[0199] A film formed of the material is manufactured and cut into a rectangle of 100 mm×10 mm to obtain a test piece. A tensile load of 0 g, 100 g, 200 g, 300 g, 400 g, 500 g and 600 g is applied to the long side direction of the obtained test piece, and the delay in the in-plane direction at this time is measured. The above-mentioned delay in the in-plane direction is measured using an ellipsometer with a measurement wavelength of 550 nm. The thickness of the film is set to d, and the stress is calculated as the load per unit cross-sectional area of the film. The photoelastic coefficient can be derived as the ratio of the delay Re(550) in the in-plane direction to the thickness d, that is, the rate of change of Re(550) / d relative to the stress.
[0200] The wavelength dispersion of the film can be evaluated by the value of D = Re (450) / Re (550). Here, Re (450) represents the retardation at a wavelength of 450 nm measured in the film plane direction, and Re (550) represents the retardation at a wavelength of 550 nm measured in the film plane direction.
[0201] The first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate preferably all have inverse wavelength dispersion. Here, a film having inverse wavelength dispersion means that the value of D=Re(450) / Re(550) of the film is 1 or less.
[0202] The value of Re(450) / Re(550) of the first λ / 2 plate is defined as D1, the value of Re(450) / Re(550) of the second λ / 2 plate is defined as D2, and the value of Re(450) / Re(550) of the λ / 4 plate is defined as D3.
[0203] Preferably, D1≤1, D2≤1, and D3≤1.
[0204] More preferably, D1<1. More preferably, D2<1. More preferably, D3<1.
[0205] Since the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate all have inverse wavelength dispersion, the optical layered body can function well as a λ / 4 plate in a wide wavelength range (particularly in the visible light region).
[0206] It is preferred that the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate have substantially the same wavelength dispersion as each other.
[0207] That they have substantially the same wavelength dispersion can be confirmed by the fact that D1 of the first λ / 2 plate, D2 of the second λ / 2 plate, and D3 of the λ / 4 plate are substantially the same.
[0208] D1 to D3 being substantially the same means that, when the maximum value among D1 to D3 is Dmax and the minimum value is Dmin, the value of Dmax-Dmin is preferably 0.3 or less, more preferably 0.2 or less, further preferably 0.1 or less, usually 0 or more, and ideally 0. By making the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate have substantially the same wavelength dispersion, the optical layered body can function well as a λ / 4 plate in a wide wavelength range.
[0209] It is preferred that the material M1, the material M2, and the material M3 all have positive intrinsic birefringence. By using materials having positive intrinsic birefringence, the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate can be easily made into plates satisfying the formula (1a), the formula (2a), the formula (3a), the formula (1b), the formula (2b), the formula (3b), the formula (1c), the formula (2c), or the formula (3c).
[0210] The material M1, the material M2, and the material M3 each contain a specific polymer (P) greater than 50% by weight, and further contain an arbitrary component as required. Examples of the specific polymer (P) contained in the material M1, the material M2, and the material M3 include: alicyclic structure-containing polymers such as cyclic olefin polymers; cellulose-based polymers such as triacetyl cellulose; polyimide; polyolefin; polyester; polyarylene sulfide; polyvinyl alcohol; polycarbonate; polyarylester; polyethersulfone; polysulfone; polyarylenesulfone; polyvinyl chloride, etc., and alicyclic structure-containing polymers are particularly preferred.
[0211] The specific polymer (P) may be a crystalline polymer with crystallinity or an amorphous polymer without crystallinity. "Crystalline polymer" refers to a polymer with a melting point Tm. Hereinafter, a resin containing a crystalline polymer is referred to as a crystalline resin. The melting point of a polymer with a melting point Tm can be observed using a differential scanning calorimeter (DSC).
[0212] The melting point Tm of a polymer can be measured by the following method. First, the polymer is melted by heating, and the molten polymer is quenched with dry ice. Then, the polymer can be used as a test body, and the glass transition temperature Tg and melting point Tm of the polymer can be measured using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min (heating mode).
[0213] The polymer containing an alicyclic structure is a polymer containing an alicyclic structure in a repeating unit. As the polymer containing an alicyclic structure, any one of a polymer containing an alicyclic structure in the main chain and a polymer containing an alicyclic structure in the side chain can be used. As the alicyclic structure, for example, a cycloalkane structure and a cycloolefin structure can be cited, and from the viewpoint of thermal stability, a cycloalkane structure is preferred. The number of carbon atoms contained in an alicyclic structure is preferably 4 or more, more preferably 5 or more, particularly preferably 6 or more, preferably 30 or less, more preferably 20 or less, and particularly preferably 15 or less.
[0214] In the alicyclic structure-containing polymer, the ratio of repeating units containing alicyclic structures is preferably 50 wt % or more, more preferably 70 wt % or more, and particularly preferably 90 wt % or more. When the ratio of repeating units containing alicyclic structures is within the above range, an optical laminate having excellent heat resistance can be obtained.
[0215] Examples of polymers containing alicyclic structures include (1) norbornene-based polymers, (2) monocyclic cyclic olefin polymers, (3) cyclic conjugated diene polymers, (4) vinyl alicyclic hydrocarbon polymers, and hydrogenated products thereof. Among these, cyclic olefin polymers and norbornene-based polymers are preferred, and norbornene-based polymers are particularly preferred. Examples of norbornene-based polymers include ring-opening polymers of monomers containing a norbornene structure, ring-opening copolymers of monomers containing a norbornene structure and other monomers capable of ring-opening copolymerization, and hydrogenated products thereof; addition polymers of monomers containing a norbornene structure, addition copolymers of monomers containing a norbornene structure and other monomers capable of copolymerization, and the like. Among these, hydrogenated ring-opening polymers of monomers containing a norbornene structure are particularly preferred from the viewpoint of transparency. The above-mentioned alicyclic structure-containing polymer can be selected from, for example, polymers disclosed in Japanese Patent Application Laid-Open No. 2002-321302 and polymers obtained by the production method disclosed in International Publication No. 2018 / 062067.
[0216] In one embodiment, the specific polymer (P) is preferably an amorphous alicyclic structure-containing polymer.
[0217] In another embodiment, the specific polymer (P) is preferably a crystalline alicyclic structure-containing polymer. As a crystalline alicyclic structure-containing polymer, a polymer having crystallinity as a ring-opening polymer of dicyclopentadiene and a polymer having crystallinity as a hydrogenated product of a ring-opening polymer of dicyclopentadiene are more preferably used. A polymer having crystallinity as a hydrogenated product of a ring-opening polymer of dicyclopentadiene is particularly preferred. Here, the ring-opening polymer of dicyclopentadiene refers to a polymer in which the ratio of the structural unit from dicyclopentadiene to all structural units is usually 50% by weight or more, preferably 70% by weight or more, more preferably 90% by weight or more, and further preferably 100% by weight.
[0218] The hydrogenated product of the ring-opening polymer of dicyclopentadiene preferably has a high proportion of syndiotactic diads. Specifically, the proportion of syndiotactic diads in the repeating unit in the hydrogenated product of the ring-opening polymer of dicyclopentadiene is preferably 51% or more, more preferably 70% or more, and particularly preferably 85% or more. A high proportion of syndiotactic diads indicates high syndiotactic stereoregularity. Therefore, there is a tendency that the higher the proportion of syndiotactic diads, the higher the melting point of the hydrogenated product of the ring-opening polymer of dicyclopentadiene.
[0219] The ratio of the syndiotactic diad can be determined based on the following examples. 13 The results were confirmed by C-NMR spectroscopy analysis.
[0220] The polymers (P) contained in the material M1, the material M2, and the material M3 may have the same weight average molecular weight or may be different polymers.
[0221] The polymer (P) contained in the material M1, the material M2, and the material M3 may be polymers having the same weight composition of the structural units contained therein, or may be polymers different from each other.
[0222] The ratio of the specific polymer (P) in the material M1, the ratio of the specific polymer (P) in the material M2, and the ratio of the specific polymer (P) in the material M3 are preferably greater than 50% by weight and less than 100% by weight, more preferably 70% by weight and less than 100% by weight, further preferably 90% by weight and less than 100% by weight, further preferably 95% by weight and less than 100% by weight, further preferably 97% by weight and less than 100% by weight. When the ratio of the polymer (P) is within the above range, the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate included in the optical laminate can be easily made into plates having substantially the same wavelength dispersion.
[0223] The material M1, the material M2, and the material M3 can be combined with the above-mentioned specific polymer (P) respectively, and further contain any component. As the arbitrary component, for example, stabilizers such as antioxidants, heat stabilizers, light stabilizers, weather stabilizers, ultraviolet absorbers, near infrared absorbers, plasticizers, solvents, etc. can be cited. These components can be used alone or in combination of two or more in any ratio.
[0224] The material M1, the material M2, and the material M3 preferably contain more than 50 wt% of the alicyclic structure-containing polymer as the specific polymer (P), more preferably 70 wt% or more, further preferably 90 wt% or more, further preferably 95 wt% or more or 97 wt% or more. Thus, the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate can be easily made into plates satisfying formula (1a), formula (2a), formula (3a), formula (1b), formula (2b), formula (3b), formula (1c), formula (2c), or formula (3c), respectively. In addition, the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate can be easily made into plates having substantially the same wavelength dispersion, respectively.
[0225] [1.2. Second embodiment]
[0226] The optical stack of the second embodiment of the present invention comprises a first λ / 2 sheet, a second λ / 2 sheet, and a λ / 4 sheet in sequence. Furthermore, the optical stack of the present embodiment comprises a first adhesive layer between the first λ / 2 sheet and the second λ / 2 sheet, and a second adhesive layer between the second λ / 2 sheet and the λ / 4 sheet.
[0227] Figure 3 It is a cross-sectional view schematically showing an optical layered body according to a second embodiment of the present invention.
[0228] like Figure 3 As shown, the optical laminate 200 includes a first λ / 2 sheet 10, a second λ / 2 sheet 20, and a λ / 4 sheet 30 in order along the thickness direction. A first adhesive layer 12 is provided between the first λ / 2 sheet 10 and the second λ / 2 sheet 20 in direct contact with the main surface of the first λ / 2 sheet and the main surface of the second λ / 2 sheet. A second adhesive layer 23 is provided between the second λ / 2 sheet 20 and the λ / 4 sheet 30 in direct contact with the main surface of the second λ / 2 sheet 20 and the main surface of the λ / 4 sheet 30.
[0229] In the optical stack 200, the angle θ between the slow axis of the first λ / 2 plate 10 and the slow axis of the second λ / 2 plate is 12 The angle θ formed by the slow axis of the first λ / 2 plate 10 and the slow axis of the λ / 4 plate 30 is 13 and the angle θ in the optical laminate 100. 12 and angle θ13 In the same range.
[0230] The first adhesive layer 12 and the second adhesive layer 23 can be formed of an adhesive. Examples of adhesives used to form the adhesive layers include acrylate adhesives, polyurethane adhesives, polyurethane acrylate adhesives, epoxy adhesives, epoxy acrylate adhesives, polyolefin adhesives, ethylene vinyl alcohol adhesives, vinyl chloride adhesives, chloroprene rubber adhesives, cyanoacrylate adhesives, polyamide adhesives, polystyrene adhesives, polyvinyl butyral adhesives, and polyvinyl alcohol adhesives.
[0231] A commercially available adhesive sheet can be used as the adhesive layer, and examples of commercially available products include an adhesive sheet "CS9621" (refractive index: 1.477) manufactured by Nitto Denko Corporation.
[0232] The optical layered body 200 preferably satisfies the following formula (4), formula (5), formula (6), and formula (7).
[0233] |I1―Ia1|≤0.02 (4)
[0234] |I2―Ia1|≤0.02 (5)
[0235] |I2―Ia2|≤0.02 (6)
[0236] |I3―Ia2|≤0.02 (7)
[0237] Here, I1 represents the refractive index of the first λ / 2 plate 10, I2 represents the refractive index of the second λ / 2 plate 20, I3 represents the refractive index of the λ / 4 plate 30, Ia1 represents the refractive index of the first adhesive layer 12, and Ia2 represents the refractive index of the second adhesive layer 23. I1, I2, I3, Ia1, and Ia2 are all refractive indices at a measurement wavelength of 550 nm.
[0238] When the optical layered body 200 satisfies the equations (4) to (7), reflection can be reduced at the interface between the layers of the optical layered body 200. Therefore, the generation of an unintended image in an optical system in which the optical layered body 200 is incorporated can be effectively suppressed.
[0239] The refractive index I1 of the first λ / 2 plate 10 is preferably 1.40 or more, more preferably 1.50 or more, and is preferably 1.60 or less, more preferably 1.55 or less.
[0240] The preferred range of the refractive index I2 of the second λ / 2 plate 20 can be the same as the preferred range of the refractive index I1.
[0241] The preferred range of the refractive index I3 of the λ / 4 plate 30 can be the same as the preferred range of the refractive index I1.
[0242] The refractive index Ia1 of the first adhesive layer 12 is preferably 1.40 or more, more preferably 1.50 or more, and is preferably 1.60 or less, more preferably 1.55 or less.
[0243] The preferred range of the refractive index Ia2 of the second adhesive layer 23 can be the same as the preferred range of the refractive index Ia1.
[0244] The refractive index of each layer of the optical layered body 200 (ie, the first λ / 2 plate 10 , the second λ / 2 plate 20 , the λ / 4 plate 30 , the first adhesive layer 12 , and the second adhesive layer 23 ) can be measured by the following method.
[0245] First, a refractive index film thickness measuring device (e.g., "prism coupler" manufactured by Metricon Corporation) is used to measure the refractive index of each layer of the optical laminate 200 at measuring wavelengths of 405 nm, 532 nm, and 633 nm. The refractive index at a measuring wavelength of 550 nm is calculated by substituting the measured values obtained at the measuring wavelengths of 405 nm, 532 nm, and 633 nm into the Cauchy dispersion equation for fitting.
[0246] When the refractive index of a layer has anisotropy, the average refractive index can be determined as the refractive index of the layer by the following method.
[0247] The refractive index at a wavelength of 550 nm is measured in the extrusion direction, the in-plane direction perpendicular to the extrusion direction, and the thickness direction of the layer, respectively. Then, the average refractive index of the layer at a wavelength of 550 nm can be obtained as the refractive index of the layer by averaging the refractive indices in the extrusion direction, the in-plane direction perpendicular to the extrusion direction, and the thickness direction.
[0248] [1.3. Characteristics of optical laminate]
[0249] The optical layered body can function as a λ / 4 plate.
[0250] When the optical laminate and the linear polarizer are combined as a circular polarizing plate, nearly ideal circularly polarized light having an ellipticity close to or equal to 1 in a wide wavelength range (particularly in the visible light region of 450 nm to 650 nm) can be obtained.
[0251] The ellipticity of circularly polarized light obtained by the circularly polarizing plate including the optical laminate is preferably 0.80 or more, more preferably 0.85 or more, and ideally 1 in the front direction and at a measurement wavelength of 550 nm.
[0252] The ellipticity of circularly polarized light obtained by the circularly polarizing plate including the optical laminate is preferably 0.7 or more, more preferably 0.8 or more, and ideally 1 in the tilt direction at a polar angle of 45° and at a measurement wavelength of 550 nm.
[0253] The ellipticity of the circularly polarized light obtained at 450nm, 550nm, and 650nm by the circular polarizer containing the optical laminate is preferably a difference (Max-Min) between the maximum value Max and the minimum value Min in the front direction or the inclined direction of the polar angle 45° of 0.20 or less, more preferably 0.10 or less, and ideally 0.
[0254] The difference in ellipticity E between the directions of circularly polarized light in the oblique direction obtained by the circularly polarizing plate including the optical laminate is max -E min Small. The difference in ellipticity E max -E min The small size means that the optical layered body included in the circularly polarizing plate can function as a λ / 4 plate nearly uniformly in a wide wavelength range and in all directions in the oblique direction.
[0255] E max -E min The value of is preferably 0.4 or less, more preferably 0.3 or less, further preferably 0.2 or less, and ideally 0.
[0256] Here, E max -E min The value of can be obtained as follows.
[0257] In the azimuth angle range of 0° to 360° at 450 nm, the largest ellipticity among the ellipticities calculated every 5° along the azimuth direction is set as E(450) max , set the minimum ellipticity to E(450) min Similarly, the maximum ellipticity at 550nm is set to E(550) max , set the minimum ellipticity to E(550) min Similarly, the maximum ellipticity at 650nm is set to E(650) max , set the minimum ellipticity to E(650) min , find their respective values. max 、E(550) max 、E(650) max The maximum ellipticity is set to E max , E(450) min 、E(550) min 、E(650) min The smallest ellipticity is set to Emin , we can find E max -E min The value of .
[0258] The optical layered body is excellent in heat resistance.
[0259] Specifically, the optical layered body has a small change in phase difference due to heat.
[0260] When the in-plane retardation of the optical layered body at a wavelength of 550 nm before a heat resistance test of the optical layered body being heated at 85°C for 500 hours is defined as Reb(550), and the in-plane retardation of the optical layered body at a wavelength of 550 nm after the heat resistance test is defined as Rea(550), the absolute value |Reb(550)-Rea(550)| is preferably less than 10 nm, more preferably less than 5 nm, further preferably less than 3 nm, further preferably less than 3 nm, and the closer to 0 nm, the more preferred, and it may also be greater than 0.5 nm.
[0261] The reason why the optical layered body of the present embodiment has a small phase difference fluctuation due to heat is presumed as follows, but the reason does not limit the present invention.
[0262] For the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate included in the optical stack, the material M1, the material M2, and the material M3 forming them contain a specific polymer (P) greater than 50% by weight. It can be considered that since the polymer (P) contained is common in the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate, when the optical stack is heated, the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate contained therein each have the same behavior of phase difference change caused by heating. It can be considered that under the angular relationship of the slow axis of the first λ / 2 plate, the slow axis of the second λ / 2 plate, and the slow axis of the λ / 4 plate in the optical stack of this embodiment, the phase difference change in the first λ / 2 plate and the second λ / 2 plate and the phase difference change in the λ / 4 plate cancel each other, and the phase difference change caused by heat of the entire optical stack becomes smaller than the phase difference change caused by heat of the λ / 4 plate when it is a single layer.
[0263] [2. Method for producing an optical laminate]
[0264] The above-mentioned optical laminate can be manufactured by any method. For example, by preparing a long strip of a first λ / 2 sheet having a slow axis in the conveying direction or the width direction, a long strip of a second λ / 2 sheet having a slow axis in a direction (inclined direction) other than the conveying direction and the width direction, and a long strip of a λ / 4 sheet having a slow axis in the inclined direction, and bonding them together in a manner that the length directions are aligned and overlap in the thickness direction via a layer of an arbitrary and appropriate adhesive, a long strip of an optical laminate can be manufactured.
[0265] Furthermore, a single-piece optical layered body can be manufactured by laminating the single-piece first λ / 2 plate, second λ / 2 plate, and λ / 4 plate so that their slow axis directions form an angular relationship with the optical layered body and overlapping them in the thickness direction.
[0266] The method for producing the first λ / 2 sheet, the second λ / 2 sheet, and the λ / 4 sheet is not particularly limited, and examples thereof include a method of obtaining an extruded film by a melt extrusion method and stretching the extruded film.
[0267] The obtained extruded film can be stretched directly or stretched after any process. As an example of any process, a process of contacting the extruded film with a solvent can be cited. By contacting the extruded film with a solvent, the NZ coefficient of the extruded film can be changed.
[0268] Examples of solvents in contact with the extruded film include hydrocarbon solvents such as toluene, limonene, and decalin; and carbon disulfide. In the case where the extruded film is formed of a resin containing a crystalline polymer, a hydrocarbon solvent is preferably used as the solvent from the viewpoint that the crystalline polymer is not easily dissolved. The solvent may be one or more. Examples of methods for contacting the extruded film with the solvent include a spray method of spraying the solvent on the film; a coating method of coating the solvent on the film; and an immersion method of immersing the film in the solvent.
[0269] [3. Application of optical laminate]
[0270] [3.1. Circular polarizer]
[0271] The optical layered body can be preferably used as a component of a circular polarizing plate.
[0272] The circularly polarizing plate can include the above-mentioned optical layered body and a linear polarizer.
[0273] The circularly polarizing plate including the optical layered body can convert linearly polarized light in a wide wavelength range into circularly polarized light.
[0274] The circular polarizer having the above optical laminate preferably includes a linear polarizer, a first λ / 2 plate, a second λ / 2 plate, and a λ / 4 plate in order along the thickness direction. The angle between the absorption axis of the linear polarizer and the slow axis of the first λ / 2 plate is preferably 2° or more, more preferably 4° or more, preferably 12° or less, and more preferably 10° or less.
[0275] Alternatively, the angle formed by the transmission axis of the linear polarizer and the slow axis of the first λ / 2 plate is preferably 29° or more, more preferably 31° or more, and is preferably 40° or less, more preferably 38° or less.
[0276] Examples of the linear polarizer included in the circularly polarizing plate are not particularly limited, and examples thereof include an absorption-type polarizer and a reflection-type polarizer.
[0277] As an example of the absorption-type polarizer, there is mentioned a polarizer which can be produced by a production method including a step of adsorbing a dichroic dye on a polyvinyl alcohol-based resin film.
[0278] Examples of reflective polarizers include: a polarizer that is a laminate of thin films with different birefringence; a wire grid polarizer; and a polarizer that is a laminate of a layer having cholesteric regularity and a λ / 4 plate, the cholesteric regularity having the function of separating left and right circularly polarized light.
[0279] [3.2. Image display device]
[0280] The optical laminate can be preferably used as a component of an image display device. For example, a circular polarizer including an optical laminate can be preferably used as a component of a flexible image display device or a component of a stereoscopic image display device because the optical properties thereof are less changed by deformation.
[0281] Examples of image display devices include organic electroluminescent image display devices and liquid crystal image display devices.
[0282] [4. Optical components]
[0283] (Third Embodiment)
[0284] An optical member according to a third aspect of the present invention includes a transparent member and the optical layered body provided on the transparent member.
[0285] Figure 4 Schematically showing a cross-sectional view of an optical component according to a third embodiment of the present invention. The optical component 1000 includes a transparent component 40 and an optical laminate 100. In the present embodiment, the transparent component 40 and the optical laminate 100 are in direct contact with each other without passing through any layer such as an adhesive layer, but in another embodiment, the optical laminate 100 may be disposed on the transparent component 40 via any layer (for example, a third adhesive layer). In the present specification, "on a transparent component" includes not only a case where a layer is directly disposed on a transparent component, but also a case where a layer is indirectly disposed on a transparent component via any layer.
[0286] The transparent member 40 is usually a member having a total transmittance of 80% or more in the visible light region. The total transmittance is usually 100% or less, but may be 100%.
[0287] In this embodiment, the transparent member 40 is lens-shaped and has a curved surface 40U, and the optical laminate 100 is provided on the curved surface 40U. As described above, in another embodiment, the optical laminate 100 may be provided on the curved surface 40U of the transparent member 40 via an arbitrary layer (for example, an adhesive layer).
[0288] In another embodiment, the transparent member included in the optical member may have any shape other than a lens shape (eg, a flat plate shape, a prism shape, a corrugated plate shape).
[0289] In another embodiment, the optical member may include an optical layered body of any embodiment such as the optical layered body 200 instead of the optical layered body 100 .
[0290] The optical component may include a transparent component, a first λ / 2 plate, a second λ / 2 plate, and a λ / 4 plate in sequence along the thickness direction, or may include a transparent component, a λ / 4 plate, a second λ / 2 plate, and a first λ / 2 plate in sequence along the thickness direction, but the optical component preferably includes a transparent component, a first λ / 2 plate, a second λ / 2 plate, and a λ / 4 plate in sequence along the thickness direction.
[0291] As described above, the optical laminate reduces the phase difference change caused by deformation from the initial shape. Therefore, even if the optical laminate is arranged on the curved surface of a transparent component with a curved surface, it is not easy to produce uneven phase difference (phase difference spot). As a result, an optical component with excellent uniformity of desired optical properties can be obtained.
[0292] The optical component can be applied to a pancake optical system that can be included in a stereoscopic image display device, for example. Examples of pancake optical systems are not particularly limited, and include optical systems described in "Official journal of the CIOMP2047-7538" and optical systems described in International Publication No. 2020 / 209354 (Patent Document 2).
[0293] Example
[0294] The present invention will be described in detail below with reference to the following examples. However, the present invention is not limited to the following examples, and can be arbitrarily modified and implemented without departing from the scope of the claims of the present invention and its equivalent scope.
[0295] In the following description, "%" and "parts" indicating amounts are based on weight unless otherwise specified. In addition, unless otherwise specified, the operations described below are performed at room temperature (20°C ± 15°C) and normal pressure (1 atm).
[0296] [Evaluation method]
[0297] (Method for measuring hydrogenation rate of polymer)
[0298] The hydrogenation rate of the polymer was determined by using o-dichlorobenzene-d4 as solvent at 145°C. 1 The measurement was carried out by H-NMR measurement.
[0299] (Method for measuring glass transition temperature Tg and melting point Tm)
[0300] The glass transition temperature Tg and melting point Tm of the polymer are measured as follows. First, the polymer is melted by heating, and the molten polymer is quenched with dry ice. Next, the polymer is used as a test body, and the glass transition temperature Tg and melting point Tm of the polymer are measured using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min (heating mode).
[0301] (Method for determining the ratio of syndiotactic diads in polymer)
[0302] The ratio of syndiotactic diads in the polymer was determined as follows. The polymer was subjected to inverse-gated decoupling at 200° C. using o-dichlorobenzene-d4 as a solvent. 13 C-NMR measurement. 13 In the results of C-NMR measurement, the peak of 127.5 ppm of o-dichlorobenzene-d4 was used as the reference shift, and the signal of 43.35 ppm from the isotactic diad and the signal of 43.43 ppm from the syndiotactic diad were identified. Based on the intensity ratio of these signals, the ratio of the syndiotactic diad in the polymer was obtained.
[0303] (thickness)
[0304] The thickness of each layer was measured using a film thickness measurement system (“F20” manufactured by Filmetrics, Inc.).
[0305] (Photoelastic coefficient)
[0306] The photoelastic coefficient is measured by the method described below.
[0307] The material to be measured is supplied to an extruder, extruded from a T-die onto a casting drum in a sheet form through a polymer filter, and cooled to obtain an extruded film having a thickness of 40 μm (in the case of a norbornene-based resin (“ZEONOR1430” manufactured by Zeon Corporation of Japan)), a thickness of 35 μm (in the case of a crystalline resin containing a hydrogenated product of a ring-opening polymer of dicyclopentadiene), or a thickness of 16 μm (in the case of a polycarbonate resin (“Iupilon E2000” manufactured by Mitsubishi Engineering-Plastics Corporation)).
[0308] The obtained extruded film was cut into a rectangle of 100 mm × 10 mm to obtain a test piece. The cutting was performed in such a way that the long side of the test piece was parallel to the conveying direction of the film. A tensile load of 0 g, 100 g, 200 g, 300 g, 400 g, 500 g and 600 g was applied at 25°C in the long side direction of the obtained test piece, and the delay in the in-plane direction at this time was measured. The above-mentioned delay in the in-plane direction was measured using an ellipsometer with a measurement wavelength of 550 nm. The thickness of the film was set to d, and the stress was calculated as the load per unit cross-sectional area of the film. The photoelastic coefficient was derived as the ratio of the delay Re(550) in the in-plane direction to the thickness d, that is, the rate of change of Re(550) / d relative to the stress.
[0309] (Determination of refractive index)
[0310] The refractive index of the film was measured at 25° C. using a refractive index film thickness measuring device (“prism coupler” manufactured by Metricon Corporation) at measuring wavelengths of 405 nm, 532 nm, and 633 nm. The refractive index at a measuring wavelength of 550 nm was calculated by substituting the measured values obtained at the measuring wavelengths of 405 nm, 532 nm, and 633 nm into the Cauchy dispersion equation for fitting.
[0311] The refractive index at the wavelength of 550 nm was measured in the extrusion direction, the in-plane direction perpendicular to the extrusion direction, and the thickness direction of the sample film. Then, the average refractive index of the film at a wavelength of 550 nm was obtained as the average of the refractive indices in the extrusion direction, the in-plane direction perpendicular to the extrusion direction, and the thickness direction, and was used as the refractive index of the film.
[0312] In addition, the in-plane retardation Re and the retardation Rth in the thickness direction of the film were measured. Based on these values, the NZ coefficient NZ of the film was calculated by the formula: NZ=Rth / Re+0.5.
[0313] (Heat resistance of optical laminate) Re change after treatment at 85°C for 500 hours
[0314] A 50 mm x 50 mm square sample is cut out from the optical laminate. The cutting is performed in such a way that each side of the sample is parallel to the width direction or the length direction of the long strip of the optical laminate. For the cut sample of the optical laminate, a phase difference meter ("AxoScan" manufactured by Axometrics) is used to measure the in-plane delay (Reb(550)) at a wavelength of 550 nm. Then, after the sample is allowed to stand in a thermostat at 85°C for 500 hours, it is taken out from the thermostat and the phase difference (Rea(550)) at a wavelength of 550 nm is measured. The heat resistance is evaluated by calculating the absolute value of the difference in phase difference before and after the heat resistance test.
[0315] When |Reb(550)-Rea(550)| was less than 3 nm, the in-plane retardation Re change was evaluated as "small", and when |Reb(550)-Rea(550)| was greater than 3 nm, the in-plane retardation Re change was evaluated as "large".
[0316] (Phase difference spots during curved surface processing)
[0317] A set of metal molds having a concave or convex surface with a curvature radius of 125 mm is prepared. The optical laminates of the examples and comparative examples are sandwiched between two sheets of fluororesin (Teflon (registered trademark)) films as release films and are set in a metal mold. The flat optical laminate is processed into a shape having a curved surface by heat pressing at 110°C for 1 minute. The obtained optical laminate having a curved surface is arranged between two polarizing plates and observed by backlighting. At this time, the observation is performed while one of the two polarizing plates is rotated arbitrarily. The optical laminate in which color spots are observed in the surface is evaluated as having phase difference spots "present", and the optical laminate in which color spots are not observed is evaluated as having phase difference spots "absent". The optical laminate in which color spots are not observed shows that the phase difference changes that may occur when processed into a shape having a curved surface are reduced.
[0318] (Calculation method of ellipticity based on simulation)
[0319] The optical laminates manufactured in each embodiment and comparative example were modeled using "LCD Master" manufactured by SHINTECH Co., Ltd. as simulation software. In the simulation model, as a circular polarizer, the structure of the optical laminates of the embodiment and comparative example was set to be attached to the linear polarizer. Therefore, in the model, the polarizer, the first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate of the optical laminate were sequentially arranged in the thickness direction, and the absorption axis direction of the linear polarizer and the slow axis of the first λ / 2 plate of the optical laminate were set to form an angle θ shown in Tables 1 and 2. 01structure. Then, in the above model, the ellipticity of the light transmitted in the front direction and the inclined direction of the polar angle 45° when the circular polarizer is irradiated with light from a D65 light source is calculated. Here, in the front direction, at a polar angle of 0°, calculations are performed every 5° in the azimuth direction within the range of 0° to 360°, and the average of the calculated values is used as the ellipticity in the front direction. Ellipticity refers to the value obtained by dividing the amplitude of the short axis in circular or elliptically polarized light by the amplitude of the long axis, and can take values of 0 to 1. The closer it is to 1, the closer it is to a perfect circle, and the better performance it shows as a circular polarizer. The ellipticity is calculated at wavelengths of 450nm, 550nm, and 650nm. In addition, in order to evaluate the reduction of color shift, the value (Max-Min) obtained by subtracting the minimum ellipticity from the maximum ellipticity among the ellipticities at 450nm, 550nm, and 650nm is calculated. The smaller the value, the closer the characteristics of the circular polarizer are to uniformity over a wide wavelength range.
[0320] Next, at a polar angle of 45°, calculations are performed every 5° in the azimuth direction within the range of 0° to 360°, and the average of the calculated values is used as the ellipticity in the tilt direction. The ellipticity in the tilt direction is calculated at wavelengths of 450nm, 550nm, and 650nm. In addition, in order to evaluate the reduction of color shift, the value (Max-Min) obtained by subtracting the minimum ellipticity from the maximum ellipticity among the ellipticities at 450nm, 550nm, and 650nm is calculated. The smaller the value, the closer the characteristics of the circular polarizer are to uniformity over a wide wavelength range.
[0321] Furthermore, in the range of azimuth angles of 0° to 360° at 450 nm, the largest ellipticity among the ellipticities calculated every 5° along the azimuth direction is set as E(450) max , set the minimum ellipticity to E(450) min Similarly, the maximum ellipticity at 550nm is set to E(550) max , set the minimum ellipticity to E(550) min Similarly, the maximum ellipticity at 650nm is set to E(650) max , set the minimum ellipticity to E(650) min , find their respective values. max 、E(550) max 、E(650) max The maximum ellipticity is set to E max , E(450) min 、E(550) min 、E(650) min The smallest ellipticity is set to E min , calculate E max -Emin . E max -E min The smaller the value of is, the more the degree of reduction of the color shift in each direction of the tilt direction is equal between each direction and between each wavelength measured, and the more uniform the characteristics of the circular polarizer when observed from the tilt direction are between each direction and between each wavelength measured. That is, it means that the optical laminate included in the circular polarizer can function well as a λ / 4 plate in each direction of the tilt direction and in a wide wavelength range.
[0322] (Visual evaluation of performance of circular polarizing plate)
[0323] An absorption-type linear polarizer manufactured by stretching a long polyvinyl alcohol resin film dyed with iodine was prepared.
[0324] The linear polarizer and the optical laminate obtained in each example and comparative example were bonded together in such a manner that the linear polarizer and the first λ / 2 plate of the optical laminate were opposite to each other via an optically isotropic adhesive ("CS9621" manufactured by Nitto Denko Corporation) to obtain a circular polarizing plate. The bonding was performed in such a manner that the absorption axis direction of the linear polarizer and the slow axis of the first λ / 2 plate of the optical laminate formed an angle θ shown in Tables 1 and 2. 01 The obtained circular polarizing plate sequentially comprises a linear polarizer, a first λ / 2 plate, a second λ / 2 plate, and a λ / 4 plate.
[0325] An Apple "iPad" (registered trademark) was prepared as an image display device. A circular polarizer was bonded to the image display device via an adhesive ("CS9621" manufactured by Nitto Denko Corporation). The image display device was made to display a white screen and observed from the front. At this time, a polarizer was arranged between the image display device and the observer's eyes, and the observation was performed while the polarizer was rotated. The brightness and color shift of the image were confirmed, and the case where the brightness was low or the color shift was confirmed was evaluated as "poor", and the case where neither was confirmed was evaluated as "good".
[0326] (Stereoscopic images show whether there are ghost images in the optical system)
[0327] The optical laminates obtained in the embodiments and comparative examples of two sheets (set as optical laminate (1) and optical laminate (2)) are assembled into a head-mounted display having a pancake optical system. The assembly is performed in a manner that includes, in sequence, a display, a first linear polarizer, an optical laminate (1), a beam splitter as a half-mirror, an optical laminate (2), a polarization beam splitter (DBEF (registered trademark)), and a second linear polarizer. In addition, the direction of the absorption axis of the first linear polarizer and the slow axis of the first λ / 2 plate included in the optical laminate (1) form an angle θ shown in Tables 1 and 2 01In this manner, the absorption axis direction of the first linear polarizer and the slow axis of the first λ / 2 plate included in the optical laminate (2) form an angle θ shown in Tables 1 and 2. 01 way.
[0328] The head mounted display in which the two optical laminates were assembled was made to display an image, and the presence of an unwanted image (ghost image) was visually confirmed. The case where a ghost image was confirmed was evaluated as "presence", the case where a ghost image was slightly confirmed was evaluated as "slightly presence", and the case where a ghost image was almost not confirmed was evaluated as "no".
[0329] [Wave plate and bonding layer]
[0330] The wave plates and adhesive layers used in the respective examples and comparative examples are as follows.
[0331] [COP(λ / 2)1]
[0332] COP(λ / 2)1 as a half-wave plate was manufactured by the following operation and used.
[0333] The particles of norbornene resin ("ZEONOR1430" manufactured by Zeon Co., Ltd., Japan) were dried at 100°C for 5 hours. After drying, the particles were supplied to an extruder, extruded from a T-die onto a casting drum in a sheet form via a polymer filter, and cooled to obtain an unstretched film with a thickness of 80 μm. The unstretched film was supplied to a roller longitudinal stretching machine, and a longitudinal uniaxial stretching treatment was performed along the length direction of the film at a temperature of 139°C and a magnification of 2.0 times to obtain a 1 / 2 wavelength film (λ / 2 sheet) with a thickness of 56 μm. The in-plane retardation Re of the obtained 1 / 2 wavelength film is 275 nm, and the thickness direction retardation Rth is 138 nm. The refractive index shows the relationship of nx>ny=nz.
[0334] [COP(λ / 2)2]
[0335] COP(λ / 2)2 as a half-wave plate was manufactured by the following operation and used.
[0336] (1) Production of crystalline resin containing hydrogenated product of ring-opening polymer of dicyclopentadiene
[0337] After the metal pressure-resistant reactor was fully dried and purged with nitrogen, 154.5 parts of cyclohexane, 42.8 parts of a 70% cyclohexane solution of dicyclopentadiene (endomorph content of 99% or more) (30 parts of dicyclopentadiene), and 1.9 parts of 1-hexene were added to the metal pressure-resistant reactor and heated to 53°C.
[0338] Dissolve 0.014 parts of tetrachlorotungsten benzimide (tetrahydrofuran) complex in 0.70 parts of toluene to prepare a solution. Add 0.061 parts of 19% diethoxyethylaluminum / n-hexane solution to the solution and stir for 10 minutes to prepare a catalyst solution. Add the catalyst solution to a pressure-resistant reactor to initiate a ring-opening polymerization reaction. After that, react for 4 hours while maintaining 53°C to obtain a solution of a ring-opening polymer of dicyclopentadiene. The number average molecular weight (Mn) and weight average molecular weight (Mw) of the obtained ring-opening polymer of dicyclopentadiene are 8750 and 28100, respectively, and the molecular weight distribution (Mw / Mn) obtained therefrom is 3.21.
[0339] 0.037 parts of 1,2-ethylene glycol as a terminator was added to 200 parts of the obtained solution of the ring-opening polymer of dicyclopentadiene, and the mixture was heated to 60°C and stirred for 1 hour to terminate the polymerization reaction. At this time, 1 part of a hydrotalcite-like compound ("Kyoward (registered trademark) 2000" manufactured by Kyowa Chemical Industry Co., Ltd.) was added, heated to 60°C, and stirred for 1 hour. Thereafter, 0.4 parts of a filter aid ("Radio Light (registered trademark) #1500" manufactured by Showa Chemical Industry Co., Ltd.) was added, and the adsorbent and the solution were separated by filtration using a PP pleated cartridge filter ("TCP-HX" manufactured by ADVANTEC Toyo Co., Ltd.).
[0340] 100 parts of cyclohexane were added to 200 parts (polymer amount: 30 parts) of the filtered solution of the ring-opening polymer of dicyclopentadiene, and 0.0043 parts of carbonylchlorohydrotris(triphenylphosphine)ruthenium were added, and a hydrogenation reaction was carried out at a hydrogen pressure of 6 MPa and 180° C. for 4 hours. Thus, a reaction solution containing a hydrogenated product of the ring-opening polymer of dicyclopentadiene was obtained. In the reaction solution, the hydrogenated product was precipitated to form a slurry solution.
[0341] The hydride contained in the reaction solution was separated from the solution using a centrifugal separator and dried under reduced pressure at 60° C. for 24 hours to obtain 28.5 parts of a crystalline hydrogenated ring-opening polymer of dicyclopentadiene. The hydrogenation rate of the hydrogenated product was 99% or more, the glass transition temperature Tg was 93° C., the melting point (Tm) was 262° C., and the ratio of the syndiotactic diad was 89%.
[0342] 1.1 parts of an antioxidant (tetrakis [methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl) propionate] methane, manufactured by BASF Japan, "Irganox (registered trademark) 1010") were mixed into 100 parts of the obtained hydrogenated product of the ring-opening polymer of dicyclopentadiene, and then introduced into a twin-screw extruder having four die holes with an inner diameter of 3 mm (product name "TEM-37B", manufactured by Toshiba Machine Co., Ltd.). The mixture of the hydrogenated product of the ring-opening polymer of dicyclopentadiene and the antioxidant was formed into a strand shape by hot melt extrusion molding, and then chopped with a strand pelletizer to obtain a crystalline resin in the form of particles. The crystalline resin is a resin having a positive intrinsic birefringence value.
[0343] The operating conditions of the twin-screw extruder are as follows.
[0344] ·Barrel setting temperature = 270~280℃
[0345] Die head set temperature = 250℃
[0346] Screw speed = 145 rpm
[0347] (2) Film production
[0348] The crystalline resin pellets produced in (1) above are dried at 100°C for 5 hours. After drying, the pellets are supplied to an extruder, extruded from a T-die onto a casting drum in a sheet form through a polymer filter, and cooled to obtain an unstretched resin film with a thickness of 35 μm. The unstretched resin film is passed through a bathtub filled with toluene as a solvent so that toluene is in contact with the resin film. The contact time with the solvent is 7 seconds. The resin film in contact with the solvent is heated in an oven heated to 110°C for about 1 minute to obtain a solvent-treated resin film. Then, the resin film is supplied to a roller-type longitudinal stretching machine, and a longitudinal uniaxial stretching treatment is performed at a temperature of 130°C and a magnification of 1.5 times along the length direction of the film to obtain a 1 / 2 wavelength film (λ / 2 sheet) with a thickness of 34 μm. The in-plane retardation Re of the obtained 1 / 2 wavelength film is 275 nm, and the thickness direction retardation Rth is 0 nm. The refractive index shows the relationship of nx>nz>ny.
[0349] [COP(λ / 4)1]
[0350] COP(λ / 4)1 as a quarter wave plate was manufactured by the following operation and used.
[0351] In the manufacture of COP(λ / 2)1, the extrusion conditions are changed. Except for the above matters, the same operation as the manufacture of COP(λ / 2)1 is carried out to obtain an unstretched film with a thickness of 40μm. The unstretched film is supplied to a roller longitudinal stretching machine, and a longitudinal uniaxial stretching treatment is carried out along the length direction of the film at a temperature of 139°C and a magnification of 2.0 times to obtain a 1 / 4 wavelength film (λ / 4 sheet) with a thickness of 28μm. The in-plane retardation Re of the obtained 1 / 4 wavelength film is 138nm, and the thickness direction retardation Rth is 69nm. The refractive index shows the relationship of nx>ny=nz.
[0352] [COP(λ / 4)2]
[0353] COP(λ / 4)2 as a quarter wave plate was manufactured by the following operation and used.
[0354] In the manufacture of COP(λ / 2)1, the extrusion conditions are changed. Except for the above matters, the same operation as the manufacture of COP(λ / 2)1 is carried out to obtain an unstretched film with a thickness of 40μm. The unstretched film is supplied to a roller longitudinal stretching machine, and a longitudinal uniaxial stretching treatment is carried out along the length direction of the film at a temperature of 139°C and a magnification of 2.0 times to obtain a 1 / 4 wavelength film (λ / 4 sheet) with a thickness of 28μm. The in-plane retardation Re of the obtained 1 / 4 wavelength film is 141nm, and the thickness direction retardation Rth is 70nm. The refractive index shows the relationship of nx>ny=nz.
[0355] [COP(λ / 4)3]
[0356] COP(λ / 4)3 as a quarter wave plate was manufactured by the following operation and used.
[0357] In the manufacture of COP(λ / 2)2, the extrusion conditions are changed. Except for the above matters, the same operation as the manufacture of COP(λ / 2)2 is carried out to obtain an unstretched resin film with a thickness of 18μm. The unstretched resin film is passed through a bathtub filled with toluene as a solvent, so that toluene is in contact with the resin film. The contact time with the solvent is 7 seconds. The resin film in contact with the solvent is heated in an oven at 110°C for about 1 minute to obtain a solvent-treated resin film. Then, the resin film is supplied to a roller-type longitudinal stretching machine, and a longitudinal uniaxial stretching treatment is performed along the length direction of the film at a temperature of 130°C and a magnification of 1.5 times to obtain a 1 / 4 wavelength film (λ / 4 sheet) with a thickness of 15μm. The in-plane retardation Re of the obtained 1 / 4 wavelength film is 138nm, and the thickness direction retardation Rth is 0nm. The refractive index shows the relationship of nx>nz>ny.
[0358] [PC(λ / 2)]
[0359] PC (λ / 2) as a half-wave plate was manufactured by the following operation and used.
[0360] In the manufacture of COP(λ / 2)1, particles of polycarbonate resin ("IUPILONE2000" manufactured by Mitsubishi Engineering-Plastics Corporation, glass transition temperature 151°C) are used instead of particles of norbornene-based resin, and the extrusion conditions are changed. Except for the above matters, the same operation as the manufacture of COP(λ / 2)1 is carried out to obtain an unstretched film with a thickness of 32 μm. The unstretched film is supplied to a roller-type longitudinal stretching machine, and a longitudinal uniaxial stretching treatment is performed along the length direction of the film at a temperature of 155°C and a magnification of 1.5 times to obtain a 1 / 2 wavelength film (λ / 2 sheet) with a thickness of 26 μm. The in-plane retardation Re of the obtained 1 / 2 wavelength film is 275 nm, and the thickness direction retardation Rth is 138 nm. The refractive index shows the relationship of nx>ny=nz.
[0361] [PC(λ / 4)]
[0362] PC (λ / 4) as a quarter wave plate was manufactured by the following operation and used.
[0363] In the manufacture of COP(λ / 2)1, particles of polycarbonate resin ("IUPILONE2000" manufactured by Mitsubishi Engineering-Plastics Corporation, glass transition temperature 151°C) are used instead of particles of norbornene-based resin, and the extrusion conditions are changed. Except for the above matters, the same operation as the manufacture of COP(λ / 2)1 is carried out to obtain an unstretched film with a thickness of 16 μm. The unstretched film is supplied to a roller-type longitudinal stretching machine, and a longitudinal uniaxial stretching treatment is performed along the length direction of the film at a temperature of 155°C and a magnification of 1.5 times to obtain a 1 / 4 wavelength film (λ / 4 sheet) with a thickness of 13 μm. The in-plane retardation Re of the obtained 1 / 4 wavelength film is 138 nm, and the thickness direction retardation Rth is 69 nm. The refractive index shows the relationship of nx>ny=nz.
[0364] [Adhesive layer 1]
[0365] As the adhesive layer 1, an adhesive sheet "CS9621" manufactured by Nitto Denko Corporation (a layer of acrylic adhesive, a refractive index of 1.477) was used.
[0366] [Adhesive layer 2]
[0367] The adhesive layer 2 is produced by the following operation and used.
[0368] (Preparation of Adhesive Layer 2)
[0369] 210 parts of ethyl acetate as a solvent, 70 parts of phenoxyethyl acrylate, 20 parts of butyl acrylate, 3 parts of hydroxyethyl acrylate, and 0.3 parts of benzoyl peroxide were added to a reaction container having a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer, and polymerization treatment was performed in a nitrogen stream to obtain a solution of a copolymer having an adhesiveness of about 30% by weight in solid content. In this solution, 3 parts of a multifunctional isocyanate crosslinking agent were uniformly mixed per 100 parts of the solid content to prepare a solution of an acrylic adhesive composition. Next, the solution was applied to a partition, dried at 130°C for 5 minutes, and a layer of an adhesive having a thickness of 50 μm was formed on the partition to prepare an adhesive layer 2. The refractive index of the adhesive layer 2 was measured, and the refractive index at 550 nm was 1.535.
[0370] [Examples 1, 3 to 6, 7, Comparative Examples 1 to 6] Production of Optical Laminated Body
[0371] The first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate shown in Tables 1 and 2 were prepared.
[0372] The first λ / 2 sheet and the second λ / 2 sheet are bonded together via the adhesive layer 2 to obtain an intermediate laminate. The λ / 4 sheet is bonded to the surface of the second λ / 2 sheet of the intermediate laminate via the adhesive layer 2 to obtain an optical laminate. The first λ / 2 sheet and the second λ / 2 sheet are bonded together at an angle θ 12 and the angle θ between the first λ / 2 plate and the λ / 4 plate 13 The angles were set to the angles shown in Tables 1 and 2. The obtained optical layered body was evaluated by the above-mentioned method.
[0373] [Example 2]
[0374] The first λ / 2 plate, the second λ / 2 plate, and the λ / 4 plate shown in Tables 1 and 2 were prepared.
[0375] An optical layered body was obtained in the same manner as in Example 1 except that the adhesive layer 1 was used instead of the adhesive layer 2. The obtained optical layered body was evaluated by the above-mentioned method.
[0376] [Comparative Example 7]
[0377] Evaluation was performed using COP(λ / 4)2 instead of the optical layered body.
[0378] [result]
[0379] The results are shown in the table below.
[0380] In the following table, the abbreviations have the following meanings.
[0381] “θ 01”: Angle between the absorption axis of the linear polarizer and the slow axis of the first λ / 2 plate
[0382] “θ 02 ”: Angle between the absorption axis of the linear polarizer and the slow axis of the second λ / 2 plate
[0383] “θ 03 ”: Angle between the absorption axis of the linear polarizer and the slow axis of the λ / 4 plate
[0384] “θ 12 ”: Angle between the slow axis of the first λ / 2 plate and the slow axis of the second λ / 2 plate
[0385] “θ 13 ”: Angle between the slow axis of the first λ / 2 plate and the slow axis of the λ / 4 plate
[0386] "Re": In-plane retardation (nm)
[0387] “Rth”: Thickness retardation (nm)
[0388] "NZ1", "NZ2" and "NZ3": NZ coefficients of the first λ / 2 plate, the second λ / 2 plate and the λ / 4 plate, respectively [Table 1]
[0389] Table 1
[0390]
[0391] [Table 2]
[0392] Table 2
[0393]
[0394] According to the above results, the optical laminate of the embodiment has no phase difference unevenness (phase difference spot) and excellent heat resistance when processed along the curved surface. In addition, the results of ellipticity simulation show that the optical laminate of the embodiment can function well as a λ / 4 plate in a wide visible light region of at least 450nm to 650nm.
[0395] In particular, the optical laminate of Example 7 showed Ema x -Emi n The value of is significantly low, and it can function nearly uniformly as a λ / 4 plate in a wide wavelength range and in all directions in the tilt direction.
[0396] Furthermore, the optical layered bodies of the examples showed that, when incorporated in a stereoscopic image display optical system, ghost images were not observed or were very slight even if observed, and that the optical layered bodies were applicable to optical systems requiring high performance.
[0397] On the other hand, it can be seen that the optical laminate of the comparative example cannot fully function as a λ / 4 plate, the visual evaluation of the circular polarizer is poor and / or there are phase difference spots during curved surface processing. Furthermore, it can be seen that when the optical laminate of the comparative example is assembled into a stereoscopic image display optical system, ghost images can be observed, and it is sometimes not suitable for an optical system requiring high performance.
[0398] Description of Reference Numerals
[0399] 10: first λ / 2 piece;
[0400] 12: first bonding layer;
[0401] 20: second λ / 2 plate;
[0402] 23: second adhesive layer;
[0403] 30: λ / 4 piece;
[0404] 40: transparent component;
[0405] 40U: curved surface;
[0406] 100: optical laminate;
[0407] 200: optical laminate;
[0408] 1000: optical components;
[0409] D1, D2, D3: slow axis.
Claims
1. An optical laminate comprising, in order, a first λ / 2 plate formed only of a material M1, a second λ / 2 plate formed only of a material M2, and a λ / 4 plate formed only of a material M3, The angle formed by the slow axis of the first λ / 2 plate and the slow axis of the second λ / 2 plate is greater than or equal to 24.6° and less than or equal to 30.6°, The angle formed by the slow axis of the first λ / 2 plate and the slow axis of the λ / 4 plate is greater than or equal to 90.5° and less than or equal to 96.5°. The first λ / 2 plate satisfies any one of the following formulas (1a), (1b), and (1c): nx1>ny1≈nz1(1a) nx1>ny1>nz1(1b) nx1>nz1>ny1(1c) Here, nx1 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the first λ / 2 plate, ny1 represents the refractive index in the direction orthogonal to the direction of nx1 in the in-plane direction of the first λ / 2 plate, nz1 represents the refractive index in the thickness direction of the first λ / 2 plate, The second λ / 2 plate satisfies any one of the following formulas (2a), (2b), and (2c): nx2>ny2≈nz2(2a) nx2>ny2>nz2(2b) nx2>nz2>ny2(2c) Here, nx2 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the second λ / 2 plate, ny2 represents the refractive index in the direction orthogonal to the direction of nx2 in the in-plane direction of the second λ / 2 plate, nz2 represents the refractive index in the thickness direction of the second λ / 2 plate, The λ / 4 plate satisfies any one of the following formulas (3a), (3b), and (3c), nx3>ny3≈nz3(3a) nx3>ny3>nz3(3b) nx3>nz3>ny3(3c) Here, nx3 represents the refractive index in the direction providing the maximum refractive index in the in-plane direction of the λ / 4 plate, ny3 represents the refractive index in the direction orthogonal to the direction of nx3 in the in-plane direction of the λ / 4 plate, and nz3 represents the refractive index in the thickness direction of the λ / 4 plate. The photoelastic coefficients of the material M1, the material M2, and the material M3 are each independently 10×10 -13 cm 2 Below / dyn, The material M1, the material M2, and the material M3 each contain more than 50 wt% of a specific polymer (P).
2. The optical layered body according to claim 1, wherein: The first λ / 2 plate satisfies the formula (1a) or (1b), The second λ / 2 plate satisfies the formula (2a) or (2b), The λ / 4 plate satisfies the formula (3a) or the formula (3b).
3. The optical layered body according to claim 1, wherein: The first λ / 2 plate satisfies the formula (1c), The second λ / 2 plate satisfies the formula (2c), The λ / 4 plate satisfies the formula (3c).
4. The optical laminate according to claim 1, wherein: The NZ coefficient NZ1 of the first λ / 2 plate satisfies 0.0<NZ1<1.0, The NZ coefficient NZ2 of the second λ / 2 plate satisfies 0.0<NZ2<1.0, The NZ coefficient NZ3 of the λ / 4 plate satisfies 0.0<NZ3<1.0, Here, NZ1 is represented by the following formula: NZ1 = (nx1-nz1) / (nx1-ny1), NZ2 is represented by the following formula: NZ2 = (nx2-nz2) / (nx2-ny2), NZ3 is represented by the following formula: NZ3 = (nx3-nz3) / (nx3-ny3), nx1, ny1, nz1, nx2, ny2, nz2, nx3, ny3, and nz3 have the same meanings as above.
5. The optical layered body according to claim 1, wherein: The polymer (P) is a polymer containing an alicyclic structure.
6. The optical layered body according to claim 1, wherein: The optical layered body includes a first adhesive layer between the first λ / 2 plate and the second λ / 2 plate, and includes a second adhesive layer between the second λ / 2 plate and the λ / 4 plate.
7. The optical layered body according to claim 6, wherein: The optical laminate satisfies the following formula (4), formula (5), formula (6), and formula (7), |I1―Ia1|≤0.02 (4) |I2―Ia1|≤0.02 (5) |I2―Ia2|≤0.02 (6) |I3―Ia2|≤0.02 (7) Here, I1 represents the refractive index of the first λ / 2 plate, I2 represents the refractive index of the second λ / 2 plate, I3 represents the refractive index of the λ / 4 plate, Ia1 represents the refractive index of the first adhesive layer, Ia2 represents the refractive index of the second adhesive layer. 8 . An optical member comprising a transparent member and the optical layered body according to claim 1 provided on the transparent member.
9. The optical component according to claim 8, wherein The transparent member has a curved surface, and the optical laminate is provided on the curved surface of the transparent member.
10. The optical layered body according to any one of claims 1 to 7, wherein The optical layered body is to be bonded to a curved surface of a transparent member having a curved surface.