Display system, display method, display body, and method for manufacturing display body

By optimizing the optical component configuration in the display system, the problem of lightweight and high-fine VR goggle display system is solved, and the lightweight and high-fine display effect is achieved, reducing light leakage and improving the quality of image display .

CN119013605APending Publication Date: 2024-11-22NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027313.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-28
Filing Date
2023-03-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The display system of existing VR goggles is difficult to achieve lightweight and high-refinement, resulting in bulky equipment and insufficient image display performance.

Method used

A display system is adopted, which includes a display element, a reflective polarization member, a first lens portion, a half-reflective mirror, a first phase difference member and a second phase difference member. By optimizing the configuration and optical path design of these optical elements, the The slow axis angle of the first phase difference member and the second phase difference member is below 7° or 83° to 97°, and meets specific in-plane phase difference and ISC value requirements to achieve effective reflection and transmission of light.

Benefits of technology

The lightweight and high-fine display of VR goggles is realized, reducing light leakage, improving visual recognition and smoothness of image display.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013605A_ABST
    Figure CN119013605A_ABST
Patent Text Reader

Abstract

The invention provides a display system capable of realizing light weight and high definition of VR goggles. A display system according to an embodiment of the present invention is a display system for displaying an image to a user, the display system being provided with: a display element having a display surface for emitting light for displaying the image forward via a polarizing member; a reflection unit that is disposed in front of the display element, includes a reflective polarization member, and reflects light emitted from the display element; a first lens unit disposed on an optical path between the display element and the reflection unit; a half mirror that is disposed between the display element and the first lens unit, transmits the light emitted from the display element, and reflects the light reflected by the reflection unit toward the reflection unit; a first [lambda] / 4 member disposed on an optical path between the display element and the half mirror; and a second [lambda] / 4 member disposed on an optical path between the half mirror and the reflection unit, the second [lambda] / 4 member being disposed such that an angle formed by a slow axis of the first [lambda] / 4 member and a slow axis of the second [lambda] / 4 member is 7 DEG or less or 83 DEG to 97 DEG.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a display system, a display method, a display body and a method for manufacturing the display body. Background Art

[0002] Image display devices represented by liquid crystal display devices and electroluminescent (EL) display devices (e.g., organic EL display devices) are rapidly becoming popular. In image display devices, optical components such as polarization components and phase difference components are generally used to realize image display and improve image display performance (e.g., refer to Patent Document 1).

[0003] In recent years, new uses of image display devices have been developed. For example, goggles with displays (VR goggles) for realizing Virtual Reality (VR) have begun to be commercialized. Since the use of VR goggles in various scenarios has been studied, it is expected that they will be lightweight and highly refined. Lightweighting can be achieved, for example, by thinning the lenses used for VR goggles. On the other hand, it is also expected to develop optical components suitable for display systems using thin lenses.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-103286 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In view of the above circumstances, a main object of the present invention is to provide a display system that can achieve lightweight and high-definition VR goggles.

[0009] Solutions to the problem

[0010] According to one aspect of the present invention, the following display systems [1] to [8] are provided.

[0011] [1] A display system that displays an image to a user, the display system comprising: a display element having a display surface that emits light displaying the image forward via a polarizing member; a reflecting portion that is disposed in front of the display element, includes a reflective polarizing member, and reflects light emitted from the display element; a first lens portion that is disposed on an optical path between the display element and the reflecting portion; a half mirror that is disposed between the display element and the first lens portion, transmits light emitted from the display element, and reflects light reflected by the reflecting portion toward the reflecting portion; a first λ / 4 member that is disposed on an optical path between the display element and the half mirror; and a second λ / 4 member that is disposed on an optical path between the half mirror and the reflecting portion, wherein the first λ / 4 member and the second λ / 4 member are disposed in such a manner that an angle between the slow axis of the first λ / 4 member and the slow axis of the second λ / 4 member is less than 7° or between 83° and 97°.

[0012] [2] The display system according to [1], wherein the in-plane phase difference (a) of the first λ / 4 element and the in-plane phase difference (b) of the second λ / 4 element satisfy the following formula (I):

[0013] ((a)-(b)) / ((a)+(b) / 2)≤0.02(I).

[0014] [3] The display system according to [1] or [2], wherein the ISC values ​​of the first λ / 4 component and the second λ / 4 component are both 50 or less.

[0015] [4] The display system according to any one of [1] to [3], wherein the thickness of the first λ / 4 member and the second λ / 4 member are each 100 μm or less.

[0016] [5] The display system according to any one of [1] to [4], wherein the deviation in thickness of the first λ / 4 member and the second λ / 4 member is 1 μm or less.

[0017] [6] The display system according to any one of [1] to [5], wherein the ISC values ​​per unit thickness of the first λ / 4 member and the second λ / 4 member are each less than or equal to 1.

[0018] [7] A display system according to any one of [1] to [6], wherein the polarization direction of light emitted through the polarization component is substantially orthogonal to the reflection axis of the reflective polarization component, the angle formed by the absorption axis of the polarization component contained in the display element and the slow axis of the first λ / 4 component is 40° to 50°, and the angle formed by the slow axis of the first λ / 4 component and the slow axis of the second λ / 4 component is less than 7°.

[0019] [8] A display system according to any one of [1] to [6], wherein the polarization direction of light emitted through the polarization component is substantially parallel to the reflection axis of the reflective polarization component, the absorption axis of the polarization component included in the display element and the slow axis of the first λ / 4 component form an angle of 40° to 50°, and the slow axis of the first λ / 4 component and the slow axis of the second λ / 4 component form an angle of 83° to 97°.

[0020] According to another aspect of the present invention, the following display method [9] is provided.

[0021] [9] A display method, the method comprising: a step of causing light of a display image emitted via a polarization component to pass through a first λ / 4 component; a step of causing the light after passing through the first λ / 4 component to pass through a half-mirror and a first lens portion; a step of causing the light after passing through the half-mirror and the first lens portion to pass through a second λ / 4 component; a step of causing the light after passing through the second λ / 4 component to reflect toward the half-mirror at a reflection portion including a reflective polarization component; and a step of causing the light after reflecting at the reflection portion and the half-mirror to pass through the reflection portion through the second λ / 4 component, wherein the arrangement is such that the angle between the slow axis of the first λ / 4 component and the slow axis of the second λ / 4 component is less than 7° or between 83° and 97°.

[0022] According to another aspect of the present invention, there are provided the following display

[10] and a method for manufacturing the display

[11] .

[0023]

[10] A display comprising the display system according to any one of [1] to [8] above.

[0024]

[11] A method for manufacturing a display body, wherein the display body includes the display system according to any one of [1] to [8] above.

[0025] Effects of the Invention

[0026] According to the display system of the embodiment of the present invention, it is possible to realize lightweight and high-definition VR goggles. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram showing a schematic configuration of a display system according to one embodiment of the present invention.

[0028] Figure 2 (a) Yes Figure 1 A schematic diagram illustrating an example of the movement of light in the display system shown in FIG. Figure 1A schematic diagram illustrating an example of changes in the polarization state of light in the display system shown.

[0029] Figure 3 (a) Yes Figure 1 A schematic diagram illustrating an example of the movement of light in the display system shown in FIG. Figure 1 A schematic diagram illustrating an example of changes in the polarization state of light in the display system shown.

[0030] Figure 4 This is a diagram for explaining a method for measuring thickness variation.

[0031] Figure 5 This is a diagram for explaining the method of measuring the ISC value.

[0032] Explanation of symbols

[0033] 2 Display system

[0034] 4 Lens section

[0035] 12 Display components

[0036] 14 Reflection part

[0037] 16. First lens unit

[0038] 18 Half Mirror

[0039] 20 first phase difference member

[0040] 22. Second phase difference member

[0041] 24 Second lens unit DETAILED DESCRIPTION

[0042] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings, but the present invention is not limited to these embodiments. In order to explain more clearly, the drawings sometimes schematically show the width, thickness, shape, etc. of each part compared with the embodiments, but this is only an example and does not limit the interpretation of the present invention. In addition, with respect to the drawings, the same or equivalent elements are sometimes marked with the same symbols, and repeated descriptions are omitted.

[0043] (Definition of Terms and Symbols)

[0044] The definitions of terms and symbols in this specification are as follows.

[0045] (1) Refractive index (nx, ny, nz)

[0046] "nx" is the refractive index in the direction where the refractive index in the plane reaches the maximum (ie, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), and "nz" is the refractive index in the thickness direction.

[0047] (2) In-plane phase difference (Re)

[0048] "Re(λ)" is the in-plane phase difference measured at 23°C with light of wavelength λnm. For example, "Re(550)" is the in-plane phase difference measured at 23°C with light of wavelength 550nm. When the thickness of the layer (film) is d(nm), Re(λ) can be calculated by the formula: Re(λ) = (nx-ny)×d.

[0049] (3) Retardation in the thickness direction (Rth)

[0050] "Rth(λ)" is the phase difference in the thickness direction measured at 23°C with light of wavelength λnm. For example, "Rth(550)" is the phase difference in the thickness direction measured at 23°C with light of wavelength 550nm. When the thickness of the layer (film) is d(nm), Rth(λ) can be calculated by the formula: Rth(λ) = (nx-nz)×d.

[0051] (4) Nz coefficient

[0052] The Nz coefficient can be calculated by Nz=Rth / Re.

[0053] (5) Angle

[0054] In this specification, when an angle is mentioned, unless otherwise specified, the angle includes both clockwise and counterclockwise relative to the reference direction. Therefore, for example, "45°" means ±45°. In addition, in this specification, "substantially parallel" includes a range of 0°±10°, for example, within a range of 0°±5°, preferably within a range of 0°±3°, and more preferably within a range of 0°±1°. "Substantially orthogonal" includes a range of 90°±10°, for example, within a range of 90°±5°, preferably within a range of 90°±3°, and more preferably within a range of 90°±1°.

[0055] Figure 1 Schematic diagram showing a simplified structure of a display system according to an embodiment of the present invention. Figure 1, the configuration and shape of each component of the display system 2 are schematically shown. The display system 2 includes a display element 12, a reflector 14 including a reflective polarization member, a first lens unit 16, a half mirror 18, a first phase difference member 20, a second phase difference member 22, and a second lens unit 24. The reflector 14 is arranged on the display surface 12a side of the display element 12, that is, in front, and can reflect the light emitted from the display element 12. The first lens unit 16 is arranged on the optical path between the display element 12 and the reflector 14, and the half mirror 18 is arranged between the display element 12 and the first lens unit 16. The first phase difference member 20 is arranged on the optical path between the display element 12 and the half mirror 18, and the second phase difference member 22 is arranged on the optical path between the half mirror 18 and the reflector 14.

[0056] Components arranged in front of the half mirror (in the illustrated example, the half mirror 18 , the first lens portion 16 , the second phase difference member 22 , the reflection portion 14 , and the second lens portion 24 ) are sometimes collectively referred to as a lens portion (lens portion 4 ).

[0057] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12a for displaying images. Light emitted from the display surface 12a passes through a polarizing member (typically a polarizing film) that may be included in the display element 12 and then emitted as first linearly polarized light.

[0058] The first phase difference member 20 is a λ / 4 member capable of converting the first linearly polarized light incident on the first phase difference member 20 into the first circularly polarized light (hereinafter, the first phase difference member may be referred to as a first λ / 4 member). The first phase difference member 20 may be integrally provided with the display element 12 .

[0059] The in-plane phase difference Re (550) of the first phase difference member 20 may be, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm.

[0060] In one embodiment, the in-plane phase difference (a) of the first phase difference member 20 and the in-plane phase difference (b) of the second phase difference member 22 satisfy the following formula (I). In this case, it is possible to suppress display unevenness, display defects, etc., and appropriately perform high-definition image display. The in-plane phase differences (a) and (b) are, for example, the values ​​of Re (590).

[0061] ((a)-(b)) / ((a)+(b) / 2)≤0.02(I)

[0062] Preferably, ((a)-(b)) / ((a)+(b) / 2)≤0.015, and more preferably ((a)-(b)) / ((a)+(b) / 2)≤0.01.

[0063] The first phase difference member 20 preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measured light. The Re(450) / Re(550) of the first phase difference member 20 is, for example, less than 1, may be less than 0.95, further may be less than 0.90, and further may be less than 0.85. The Re(450) / Re(550) of the first phase difference member 20 is, for example, greater than 0.75.

[0064] In one embodiment, the first phase difference member 20 satisfies all of the conditions of Re(400) / Re(550)<0.85, Re(650) / Re(550)>1.03, and Re(750) / Re(550)>1.05. The first phase difference member 20 preferably satisfies at least one selected from 0.65<Re(400) / Re(550)<0.80 (preferably 0.7<Re(400) / Re(550)<0.75), 1.0<Re(650) / Re(550)<1.25 (preferably 1.05<Re(650) / Re(550)<1.20), and 1.05<Re(750) / Re(550)<1.40 (preferably 1.08<Re(750) / Re(550)<1.36), more preferably satisfies at least two of them, and further preferably satisfies all of them.

[0065] The refractive index characteristics of the first phase difference component 20 preferably show a relationship of nx>ny≥nz. Here, "ny=nz" includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, within the range that does not impair the effect of the present invention, ny<nz may sometimes be satisfied. The Nz coefficient of the first phase difference component 20 is preferably 0.9 to 3, more preferably 0.9 to 2.5, further preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0066] The ISC value of the first phase difference component 20 is, for example, less than 50, preferably less than 40, more preferably less than 30, and further preferably less than 20. By making the first phase difference component 20 satisfy such an ISC value, a display system with excellent visual recognition can be achieved. For example, by satisfying such an ISC value, the uniformity of the in-plane phase difference can be improved, as a result, light leakage in the reflective portion described later can be suppressed. The ISC value can be an indicator of smoothness or unevenness.

[0067] The deviation of the thickness of the first phase difference member 20 is preferably less than 1 μm, more preferably less than 0.8 μm, further preferably less than 0.6 μm, and further more preferably less than 0.4 μm. According to such a thickness deviation, for example, the above-mentioned ISC value can be well achieved. Here, the thickness deviation can be obtained by measuring the thickness of the first portion located in the surface of the phase difference member and the thickness of the position separated by a given interval (for example, 5 mm to 15 mm) from the first portion in any direction (for example, above, below, left and right).

[0068] The ISC value per unit thickness of the first phase difference member 20 is preferably 1 or less, more preferably 0.7 or less, and further preferably 0.5 or less. The ISC value per unit thickness can be obtained by, for example, dividing the ISC value by the thickness (unit: μm).

[0069] The first phase difference member 20 is formed of any appropriate material that can satisfy the above-mentioned characteristics. The first phase difference member 20 may be, for example, a stretched film of a resin film or an alignment fixing layer of a liquid crystal compound.

[0070] As the resin contained in the above-mentioned resin film, there can be cited: polycarbonate resin, polyester carbonate resin, polyester resin, polyvinyl acetal resin, polyarylate resin, cyclic olefin resin, cellulose resin, polyvinyl alcohol resin, polyamide resin, polyimide resin, polyether resin, polystyrene resin, acrylic resin, etc. These resins can be used alone or in combination (for example, blending, copolymerization). In the case where the first phase difference component 20 shows reverse dispersion wavelength characteristics, a resin film containing a polycarbonate resin or a polyester carbonate resin (hereinafter, sometimes referred to as a polycarbonate resin) can be suitably used.

[0071] As the above-mentioned polycarbonate resin, any appropriate polycarbonate resin can be used as long as the effect of the present invention can be obtained. For example, the polycarbonate resin contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, and structural units derived from at least one dihydroxy compound selected from alicyclic diols, alicyclic dimethanols, di, tri or polyethylene glycols and alkylene glycols or spirodiols. Preferably, the polycarbonate resin contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, structural units derived from alicyclic dimethanols and / or structural units derived from di, tri or polyethylene glycols; more preferably, it contains structural units derived from fluorene dihydroxy compounds, structural units derived from isosorbide dihydroxy compounds, and structural units derived from di, tri or polyethylene glycols. The polycarbonate resin may also contain structural units derived from other dihydroxy compounds as needed. It should be noted that the details of the polycarbonate resin that can be suitably used for the first phase difference component and the method for forming the first phase difference component are recorded in, for example, Japanese Patent Publication No. 2014-10291, Japanese Patent Publication No. 2014-26266, Japanese Patent Publication No. 2015-212816, Japanese Patent Publication No. 2015-212817, and Japanese Patent Publication No. 2015-212818, and the records in these publications are cited as references in this specification.

[0072] The orientation fixing layer of the above-mentioned liquid crystal compound is a layer in which the liquid crystal compound is oriented in a given direction within the layer and its orientation state is fixed. It should be noted that the "orientation fixing layer" is a concept that includes an orientation solidification layer obtained by solidifying the liquid crystal monomer as described later. In the first phase difference component, representatively, the rod-shaped liquid crystal compound is oriented (parallel orientation (homogeneous alignment)) in a state of being arranged along the slow axis direction of the first phase difference component. As rod-shaped liquid crystal compounds, for example, liquid crystal polymers and liquid crystal monomers can be cited. The liquid crystal compound is preferably capable of polymerization. If the liquid crystal compound is capable of polymerization, the orientation state of the liquid crystal compound can be fixed by polymerizing after orienting the liquid crystal compound.

[0073] The orientation fixing layer (liquid crystal orientation fixing layer) of the above-mentioned liquid crystal compound can be formed by the following method: an orientation treatment is applied to the surface of a given substrate, a coating liquid containing a liquid crystal compound is applied to the surface, and the liquid crystal compound is oriented along the direction corresponding to the above-mentioned orientation treatment to fix the orientation state. As an orientation treatment, any appropriate orientation treatment can be adopted. Specifically, mechanical orientation treatment, physical orientation treatment, and chemical orientation treatment can be cited. As specific examples of mechanical orientation treatment, friction treatment and stretching treatment can be cited. As specific examples of physical orientation treatment, magnetic field orientation treatment and electric field orientation treatment can be cited. As specific examples of chemical orientation treatment, inclined evaporation method and optical orientation treatment can be cited. The processing conditions of various orientation treatments can adopt any appropriate conditions according to the purpose.

[0074] The liquid crystal compound can be aligned by treating it at a temperature corresponding to the type of the liquid crystal compound at which it exhibits a liquid crystal phase. By such a temperature treatment, the liquid crystal compound is in a liquid crystal state and is aligned in the alignment treatment direction of the substrate surface.

[0075] In one embodiment, the alignment state is fixed by cooling the aligned liquid crystal compound as described above. When the liquid crystal compound is polymerizable or crosslinkable, the alignment state can be fixed by subjecting the aligned liquid crystal compound to polymerization or crosslinking treatment as described above.

[0076] As the above-mentioned liquid crystal compound, any appropriate liquid crystal polymer and / or liquid crystal monomer can be used. Liquid crystal polymer and liquid crystal monomer can be used alone or in combination. Specific examples of liquid crystal compounds and methods for making liquid crystal orientation fixing layers are described in, for example, Japanese Patent Publication No. 2006-163343, Japanese Patent Publication No. 2006-178389, and International Publication No. 2018 / 123551. The records of these publications are cited as references in this specification.

[0077] The thickness of the first phase difference member 20 is preferably 100 μm or less. Specifically, the thickness of the first phase difference member 20 composed of a stretched film of a resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, more preferably 10 μm to 60 μm, and further preferably 20 μm to 50 μm. In addition, the thickness of the first phase difference member 20 composed of a liquid crystal orientation fixing layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and further preferably 1 μm to 4 μm.

[0078] The half mirror 18 transmits the light emitted from the display element 12 and reflects the light reflected by the reflection portion 14 toward the reflection portion 14. The half mirror 18 is provided integrally with the first lens portion 16.

[0079] The second phase difference member 22 is a λ / 4 member (hereinafter, the second phase difference member may be referred to as a second λ / 4 member) that allows the light reflected by the reflection unit 14 and the half mirror 18 to pass through the reflection unit 14 including the reflective polarization member. It should be noted that the second phase difference member 22 may be integrally provided with the first lens unit 16.

[0080] The in-plane phase difference Re(550) of the second phase difference member 22 may be, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm.

[0081] The second phase difference member 22 preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measured light. The Re(450) / Re(550) of the second phase difference member 22 is, for example, less than 1, may be less than 0.95, further may be less than 0.90, and further may be less than 0.85. The Re(450) / Re(550) of the second phase difference member 22 is, for example, greater than 0.75.

[0082] In one embodiment, the second phase difference member 22 satisfies all of the conditions of Re(400) / Re(550)<0.85, Re(650) / Re(550)>1.03, and Re(750) / Re(550)>1.05. The second phase difference member 22 preferably satisfies at least one selected from 0.65<Re(400) / Re(550)<0.80 (preferably 0.7<Re(400) / Re(550)<0.75), 1.0<Re(650) / Re(550)<1.25 (preferably 1.05<Re(650) / Re(550)<1.20), and 1.05<Re(750) / Re(550)<1.40 (preferably 1.08<Re(750) / Re(550)<1.36), more preferably satisfies at least two, and further preferably satisfies all of them.

[0083] The refractive index characteristics of the second phase difference component 22 preferably show a relationship of nx>ny≥nz. Here, "ny=nz" includes not only the case where ny and nz are completely equal, but also the case where they are substantially equal. Therefore, within the range that does not impair the effect of the present invention, ny<nz may sometimes be achieved. The Nz coefficient of the second phase difference component 22 is preferably 0.9 to 3, more preferably 0.9 to 2.5, further preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.

[0084] The ISC value of the second phase difference component 22 is, for example, less than 50, preferably less than 40, more preferably less than 30, and further preferably less than 20. By making the second phase difference component 22 satisfy such an ISC value, a display system with excellent visual recognition can be achieved. For example, by satisfying such an ISC value, the uniformity of the in-plane phase difference can be improved, as a result, light leakage in the reflective portion described later can be suppressed. The ISC value can be an indicator of smoothness or unevenness.

[0085] The variation in thickness of the second phase difference member 22 is preferably 1 μm or less, more preferably 0.8 μm or less, further preferably 0.6 μm or less, and further more preferably 0.4 μm or less. With such a variation in thickness, for example, the above-mentioned ISC value can be well achieved.

[0086] The ISC value per unit thickness of the second phase difference member 22 is preferably 1 or less, more preferably 0.7 or less, and even more preferably 0.5 or less.

[0087] The second phase difference member 22 is formed of any appropriate material that can satisfy the above characteristics. The second phase difference member 22 can be, for example, a stretched film of a resin film or an orientation fixing layer of a liquid crystal compound. For the second phase difference member 22 composed of a stretched film of a resin film or an orientation fixing layer of a liquid crystal compound, the same description as the first phase difference member 20 can be applied. The first phase difference member 20 and the second phase difference member 22 can be members of the same composition (forming material, thickness, optical properties, etc.), or they can be members of different compositions.

[0088] The thickness of the second phase difference member 22 is preferably 100 μm or less. Specifically, the thickness of the second phase difference member 22 composed of the stretched film of the resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, more preferably 10 μm to 60 μm, and further preferably 20 μm to 50 μm. In addition, the thickness of the second phase difference member 22 composed of the liquid crystal orientation fixing layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and further preferably 1 μm to 4 μm.

[0089] In addition to the reflective polarization component, the reflective part 14 may also include an absorptive polarization component. The absorptive polarization component may be arranged in front of the reflective polarization component. The reflection axis of the reflective polarization component and the absorption axis of the absorptive polarization component may be arranged substantially parallel to each other, and the transmission axis of the reflective polarization component and the transmission axis of the absorptive polarization component may be arranged substantially parallel to each other. In the case where the reflective part 14 includes the absorptive polarization component, the reflective part 14 may include a laminate having the reflective polarization component and the absorptive polarization component.

[0090] The above-mentioned reflective polarizing component can allow polarized light (representatively linear polarized light) parallel to its transmission axis to pass through while maintaining its polarization state, and reflect light in other polarization states. The orthogonal transmittance (Tc) of the reflective polarizing component can be, for example, 0.01% to 3%. The single transmittance (Ts) of the reflective polarizing component can be, for example, 43% to 49%, and can be preferably 45% to 47%. The polarization degree (P) of the reflective polarizing component can be, for example, 92% to 99.99%. As a reflective polarizing component, it is typically composed of a film with a multilayer structure (sometimes referred to as a reflective polarizing film). Commercially available products of reflective polarizing films include, for example, the trade names "DBEF" and "APF" manufactured by 3M Company and the trade name "APCF" manufactured by Nitto Denko Corporation.

[0091] The absorption-type polarizing member may typically include a resin film containing a dichroic substance (sometimes referred to as an absorption-type polarizing film). The thickness of the absorption-type polarizing film is, for example, 1 μm to 20 μm, 2 μm to 15 μm, 12 μm to 10 μm, 8 μm to 8 μm, or 5 μm to 5 μm.

[0092] The absorption-type polarizing film may be produced by a single-layer resin film or by using a laminate of two or more layers.

[0093] In the case of a single-layer resin film, for example, a hydrophilic polymer film such as a polyvinyl alcohol (PVA) film, a partially formalized PVA film, or a partially saponified ethylene-vinyl acetate copolymer film can be subjected to dyeing treatment using a dichroic substance such as iodine or a dichroic dye, stretching treatment, etc., thereby obtaining an absorption-type polarizing film. Among them, an absorption-type polarizing film obtained by dyeing a PVA film with iodine and uniaxially stretching the film is preferred.

[0094] The dyeing using iodine can be performed by, for example, immersing the PVA film in an iodine aqueous solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching can be performed after the dyeing treatment or while dyeing. In addition, the dyeing can also be performed after the stretching. The PVA film can be subjected to swelling treatment, cross-linking treatment, cleaning treatment, drying treatment, etc. as needed.

[0095] As a laminate made using the above-mentioned two or more layers, there can be cited a laminate of a resin substrate and a PVA-type resin layer (PVA-type resin film) laminated on the resin substrate, or a laminate of a resin substrate and a PVA-type resin layer formed by coating on the resin substrate. The absorption-type polarizing film obtained by using a laminate of a resin substrate and a PVA-type resin layer formed by coating on the resin substrate can be made by the following method: for example, a PVA-type resin solution is applied to a resin substrate, dried to form a PVA-type resin layer on the resin substrate, and a laminate of a resin substrate and a PVA-type resin layer is obtained; the laminate is stretched and dyed to make the PVA-type resin layer into an absorption-type polarizing film. In this embodiment, it is preferred to form a polyvinyl alcohol-type resin layer containing a halide and a polyvinyl alcohol-type resin on one side of the resin substrate. Stretching typically includes immersing the laminate in a boric acid aqueous solution for stretching. In addition, stretching can further include stretching the laminate in a gas atmosphere at a high temperature (for example, above 95°C) before stretching in a boric acid aqueous solution as needed. In addition, in the present embodiment, it is preferred that the laminate is subjected to a drying shrinkage treatment in which the laminate shrinks by more than 2% in the width direction by heating while being conveyed in the length direction. Representatively, the manufacturing method of the present embodiment includes sequentially performing an auxiliary stretching treatment in a gas atmosphere, a dyeing treatment, a stretching treatment in an aqueous solution, and a drying shrinkage treatment on the laminate. By introducing auxiliary stretching, the crystallinity of the PVA can be improved even when the PVA is coated on the thermoplastic resin, and high optical properties can be achieved. In addition, by simultaneously improving the orientation of the PVA in advance, it is possible to prevent problems such as the reduction of the orientation and dissolution of the PVA when immersed in water in the subsequent dyeing process and the stretching process, and high optical properties can be achieved. In addition, when the PVA-type resin layer is immersed in a liquid, the orientation disorder of the polyvinyl alcohol molecules and the reduction of the orientation can be suppressed compared to the case where the PVA-type resin layer does not contain a halide. Thus, the optical properties of the absorption-type polarizing film obtained by the treatment process of immersing the laminate in a liquid such as a dyeing treatment and a stretching treatment in an aqueous solution can be improved. Further, the laminate is shrunk in the width direction by drying and shrinking treatment, thereby improving the optical properties. The obtained laminate of resin substrate / absorption type polarizing film can be used directly (that is, the resin substrate can be used as a protective layer of absorption type polarizing film), or the resin substrate can be peeled off from the laminate of resin substrate / absorption type polarizing film, and any appropriate protective layer corresponding to the purpose can be stacked on the peeling surface or on the side opposite to the peeling surface. The details of the manufacturing method of such an absorption type polarizing film are recorded in, for example, Japanese Patent Publication No. 2012-73580 and Japanese Patent No. 6470455. The records of these publications as a whole are cited in this specification as a reference.

[0096] The orthogonal transmittance (Tc) of the absorption type polarization component (absorption type polarizing film) is preferably 0.5% or less, more preferably 0.1% or less, and further preferably 0.05% or less. The single transmittance (Ts) of the absorption type polarization component (absorption type polarizing film) is, for example, 41.0% to 45.0%, and preferably 42.0% or more. The polarization degree (P) of the absorption type polarization component (absorption type polarizing film) is, for example, 99.0% to 99.997%, and preferably 99.9% or more.

[0097] In one embodiment (embodiment I), the first phase difference member 20 and the second phase difference member 22 are configured so that the angle between their slow axes is less than 7°, preferably less than 6°, more preferably less than 5°, further preferably less than 4°, and further more preferably less than 3°. In addition, the absorption axis of the polarization member included in the display element 12 and the reflection axis of the reflective polarization member included in the reflection part 14 can be arranged approximately parallel to each other (in other words, the polarization direction of the light emitted through the polarization member included in the display element 12 and the reflection axis of the reflective polarization member included in the reflection part 14 can be approximately orthogonal to each other). The angle between the absorption axis of the polarization member included in the display element 12 and the slow axis of the first phase difference member 20 is, for example, 40° to 50°, can be 42° to 48°, or can be about 45°. The angle between the absorption axis of the polarization member included in the display element 12 and the slow axis of the second phase difference member 22 is, for example, 40° to 50°, can be 42° to 48°, or can be about 45°. By adjusting the axial relationship of each member to such a state, light leakage in the reflection portion can be effectively suppressed.

[0098] Below, refer to Figure 1 and Figure 2 The display system of the above-mentioned embodiment I is described. Figure 2 (a) is a schematic diagram for explaining the movement of light in the display system of Embodiment 1. Figure 2 (b) is a schematic diagram for explaining the change in polarization state of light caused by passing through or being reflected by each component in the display system. Figure 2 In the figure, the solid arrow marked on the display element 12 indicates the absorption axis direction of the polarization component included in the display element 12, the arrows marked on the first phase difference component 20 and the second phase difference component 22 indicate the slow axis direction, the solid arrow marked on the reflective polarization component 14a included in the reflection part 14 indicates the reflection axis direction, and the dotted arrows indicate the transmission axis direction of each polarization component.

[0099] The light L emitted from the display element 12 as the first linearly polarized light via the polarizing member is converted into the first circularly polarized light by the first λ / 4 member 20. The first circularly polarized light is reflected by the half mirror 18 and the first lens portion 16 (at Figure 2The second linear polarized light passes through the reflecting portion 14 (not shown in the figure), and is converted into a second linear polarized light having a polarization direction orthogonal to the first linear polarized light by the second λ / 4 element 22. The polarization direction of the second linear polarized light is the same direction (substantially parallel) as the reflection axis of the reflective polarizing element 14a included in the reflecting portion 14. Thus, the second linear polarized light incident on the reflecting portion 14 is reflected toward the half mirror 18 by the reflective polarizing element 14a.

[0100] The second linearly polarized light reflected by the reflecting portion 14 is converted into the second circularly polarized light by the second λ / 4 member 22. The rotation direction of the second circularly polarized light is the same as the rotation direction of the first circularly polarized light. The second circularly polarized light emitted from the second λ / 4 member 22 is reflected by the half mirror 18 after passing through the first lens portion 16, and is converted into the third circularly polarized light rotating in the opposite direction to the second circularly polarized light. The third circularly polarized light reflected by the half mirror 18 passes through the first lens portion 16, and is converted into the third linearly polarized light by the second λ / 4 member 22. The polarization direction of the third linearly polarized light is orthogonal to the polarization direction of the second linearly polarized light and in the same direction (approximately parallel) as the transmission axis of the reflective polarization member 14a. Thus, the third linearly polarized light can be transmitted through the reflective polarization member 14a. Although not shown, when the reflective portion includes an absorptive polarizer, the reflective polarizer 14a is arranged so that its absorption axis is substantially parallel to the reflection axis of the reflective polarizer 14a. Therefore, the third linear polarized light transmitted through the reflective polarizer 14a can directly transmit through the absorptive polarizer.

[0101] The light transmitted through the reflecting portion 14 enters the user's eye 26 after passing through the second lens portion 24. As described above, in the display system of Embodiment 1, the first linearly polarized light emitted from the display element 12 via the polarizing member is transmitted through the λ / 4 member a total of four times and then transmitted through the reflecting portion 14. However, by configuring the first phase difference member 20 and the second phase difference member 22 so that the angle formed by the slow axis is 7° or less, it is possible to appropriately suppress light leakage in the reflecting portion 14. As a result, it is possible to appropriately suppress light that should be reflected or absorbed in the reflecting portion 14 from being visually recognized as a ghost by the user.

[0102] exist Figure 2 In the figure, when observed from the side of the display element 12, the slow axes of the first phase difference member 20 and the second phase difference member 22 are arranged at an angle of 45° counterclockwise relative to the absorption axis of the polarization member included in the display element 12, but the same description as above can also be applied when they are arranged at an angle of 45° clockwise.

[0103] In another embodiment (embodiment II), the first phase difference member 20 and the second phase difference member 22 are configured so that the angle between their slow axes is 83° to 97°, preferably 84° to 96°, more preferably 85° to 95°, further preferably 86° to 94°, and further more preferably 87° to 93°. In addition, the absorption axis of the polarization member included in the display element 12 and the reflection axis of the reflective polarization member included in the reflection part 14 can be configured approximately orthogonal to each other (in other words, the polarization direction of the light emitted through the polarization member included in the display element 12 and the reflection axis of the reflective polarization member included in the reflection part 14 can be approximately parallel to each other). The angle between the absorption axis of the polarization member included in the display element 12 and the slow axis of the first phase difference member 20 is, for example, 40° to 50°, can be 42° to 48°, or can be about 45°. The angle between the absorption axis of the polarizing member included in the display element 12 and the slow axis of the second phase difference member 22 is, for example, 40° to 50°, 42° to 48°, or about 45°. By adjusting the axis relationship of each member to such a state, light leakage in the reflection part can be appropriately suppressed.

[0104] Below, refer to Figure 1 and Figure 3 The display system of the above-mentioned embodiment II is described. Figure 3 (a) is a schematic diagram for explaining the movement of light in the display system of Embodiment II. Figure 3 (b) is a schematic diagram for explaining the change in polarization state of light caused by passing through or being reflected by each component in the display system. Figure 3 In the figure, the solid arrow marked on the display element 12 indicates the absorption axis direction of the polarization component included in the display element 12, the arrows marked on the first phase difference component 20 and the second phase difference component 22 indicate the slow axis direction, the solid arrow marked on the reflective polarization component 14a included in the reflection part 14 indicates the reflection axis direction, and the dotted arrows indicate the transmission axis direction of each polarization component.

[0105] The light L emitted from the display element 12 as the first linearly polarized light via the polarizing member is converted into the first circularly polarized light by the first λ / 4 member 20. The first circularly polarized light is reflected by the half mirror 18 and the first lens portion 16 (at Figure 3 The second linear polarized light passes through the reflective portion 14 (not shown in the figure), and is converted into a second linear polarized light having a polarization direction parallel to the first linear polarized light by the second λ / 4 element 22. The polarization direction of the second linear polarized light is the same direction (substantially parallel) as the reflection axis of the reflective polarizing element 14a included in the reflective portion 14. Thus, the second linear polarized light incident on the reflective portion 14 is reflected toward the half mirror 18 by the reflective polarizing element 14a.

[0106] The second linearly polarized light reflected by the reflecting portion 14 is converted into the second circularly polarized light by the second λ / 4 member 22. The rotation direction of the second circularly polarized light is the same as the rotation direction of the first circularly polarized light. The second circularly polarized light emitted from the second λ / 4 member 22 is reflected by the half mirror 18 after passing through the first lens portion 16, and is converted into the third circularly polarized light rotating in the opposite direction to the second circularly polarized light. The third circularly polarized light reflected by the half mirror 18 passes through the first lens portion 16, and is converted into the third linearly polarized light by the second λ / 4 member 22. The polarization direction of the third linearly polarized light is orthogonal to the polarization direction of the second linearly polarized light and in the same direction (approximately parallel) as the transmission axis of the reflective polarization member 14a. Thus, the third linearly polarized light can be transmitted through the reflective polarization member 14a. Although not shown, when the reflective portion includes an absorptive polarizer, the reflective polarizer 14a is arranged so that its absorption axis is substantially parallel to the reflection axis of the reflective polarizer 14a. Therefore, the third linear polarized light transmitted through the reflective polarizer 14a can directly transmit through the absorptive polarizer.

[0107] The light transmitted through the reflection part 14 enters the user's eye 26 after passing through the second lens part 24. As described above, in the display system of Embodiment II, the first linear polarized light emitted from the display element 12 via the polarizing member is transmitted through the λ / 4 member a total of four times and then transmitted through the reflection part 14, but by configuring the first phase difference member 20 and the second phase difference member 22 so that the angle formed by the slow axis is 83° to 97° or less, it is possible to appropriately suppress the leakage of light in the reflection part 14, and as a result, it is possible to appropriately suppress the light that should be reflected or absorbed in the reflection part 14 from being visually recognized as an afterimage by the user.

[0108] exist Figure 3 In the figure, when observed from the side of the display element 12, the slow axes of the first phase difference member 20 and the second phase difference member 22 are respectively arranged at an angle of 45° counterclockwise and 45° clockwise relative to the absorption axis of the polarization member included in the display element 12, but the same description as above can also be applied when they are arranged at an angle of 45° clockwise and 45° counterclockwise.

[0109] Example

[0110] Hereinafter, the present invention will be specifically described in conjunction with embodiments, but the present invention is not subject to any limitation of these embodiments. It should be noted that the test and evaluation methods in the embodiments etc. are as follows. Wherein, when recorded as "parts", as long as there is no special record, then "parts by weight" is represented, and when recorded as "%", as long as there is no special record, then "% by weight" is represented.

[0111] (1) Thickness

[0112] The thickness of 10 μm or less was measured using a scanning electron microscope (manufactured by JEOL Ltd., product name “JSM-7100F”). The thickness exceeding 10 μm was measured using a digital micrometer (manufactured by Anritsu Co., Ltd., product name “KC-351C”).

[0113] (2) In-plane phase difference Re(λ)

[0114] The sample was prepared by cutting a square shape of 50 mm in width and 50 mm in length from the center and both ends of the λ / 4 member in the width direction so that one side was parallel to the width direction of the member. The in-plane phase difference of the sample at various wavelengths at 23°C was measured using a Mueller matrix polarimeter (Axoscan, manufactured by Axometrics).

[0115] (3) Single-body transmittance and polarization degree of polarizing film

[0116] The single transmittance Ts, parallel transmittance Tp, and orthogonal transmittance Tc of the polarizing film were measured using a spectrophotometer (L.O.Tsuka Electronics Co., Ltd., "LPF-200"). The above Ts, Tp, and Tc are Y values ​​obtained by measuring the 2-degree field of view (C light source) of JIS Z8701 and correcting for visibility. Based on the obtained Tp and Tc, the polarization degree of the polarizing film was calculated using the following formula.

[0117] Polarization degree (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0118] (4) Single-unit transmittance and polarization degree of the laminate

[0119] The single transmittance Ts, parallel transmittance Tp, and orthogonal transmittance Tc of the λ / 4 component 1 side surface of the laminate produced in the examples and comparative examples were measured using a spectrophotometer (manufactured by Otsuka Electronics Co., Ltd., "LPF-200") when linear polarized light whose polarization direction is orthogonal to the absorption axis direction of the absorption-type polarizing film was incident. The above Ts, Tp, and Tc are Y values ​​obtained by measuring with a 2-degree field of view (C light source) of JIS Z8701 and correcting for visibility. The polarization degree of the laminate was calculated from the obtained Tp and Tc using the formula described in (3) above.

[0120] (5) Thickness deviation

[0121] The λ / 4 member was cut into a size of 100 mm × 100 mm as a measurement sample. Figure 4As shown, the thickness was measured at a total of five points including the center of the sample and four points each 10 mm away from the center in the upper, lower, left and right directions, and the difference between the maximum value and the minimum value was taken as the thickness deviation.

[0122] (6) ISC value

[0123] The ISC value of the λ / 4 member was measured using EyeScale-4W manufactured by ISYSTEM Co., Ltd. Specifically, the in-plane unevenness was calculated as the ISC value in the ISC measurement mode of the 3CCD image sensor based on the manual of the measuring device.

[0124] Figure 5 This is a diagram for explaining the method of measuring the ISC value, and is a simplified diagram showing the arrangement of the light source, λ / 4 member, screen, and CCD camera as viewed from above. Figure 5 As shown in FIG. 1 , a light source L, a λ / 4 member M, and a screen S are arranged in this order, and a transmission image projected onto the screen S is measured using a CCD camera C. It should be noted that the λ / 4 member M is attached to an alkali-free glass plate (1737 manufactured by Corning Incorporated) and is provided for measurement in a state where the glass plate is placed on the light source L side.

[0125] The arrangement was made such that the distance from the light source L to the λ / 4 member M in the X-axis direction was 10 to 60 cm. The arrangement was made such that the distance from the light source L to the screen S in the X-axis direction was 70 to 130 cm. The arrangement was made such that the distance from the CCD camera C to the λ / 4 member M in the Y-axis direction was 3 to 30 cm. The arrangement was made such that the distance from the CCD camera C to the screen S in the X-axis direction was 70 to 130 cm.

[0126] [Manufacturing Example 1: Preparation of λ / 4 Member]

[0127] In a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and a reflux condenser controlled at 100° C., 29.60 parts by weight (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by weight (0.200 mol) of isosorbide (ISB), 42.28 parts by weight (0.139 mol) of spiroglycol (SPG), 63.77 parts by weight (0.298 mol) of diphenyl carbonate (DPC), and 1.19×10-6 parts by weight of calcium acetate monohydrate as a catalyst were charged. 2 Weight parts (6.78×10- 5mol). After the reactor was replaced with nitrogen under reduced pressure, it was heated by a heat medium and stirring was started when the internal temperature reached 100°C. The internal temperature reached 220°C 40 minutes after the start of the temperature rise, and the pressure was reduced while controlling to maintain the temperature, so that it reached 13.3kPa after 90 minutes after reaching 220°C. The phenol vapor produced as a by-product during the polymerization reaction was introduced into a 100°C reflux condenser, so that a certain amount of monomer components contained in the phenol vapor was returned to the reactor, and the uncondensed phenol vapor was introduced into a 45°C condenser for recovery. After nitrogen was introduced into the first reactor to temporarily restore it to atmospheric pressure, the reaction liquid after oligomerization in the first reactor was transferred to the second reactor. Next, the temperature rise and pressure reduction in the second reactor were started, so that it reached an internal temperature of 240°C and a pressure of 0.2kPa after 50 minutes. Then, the polymerization was carried out until the given stirring power was reached. When the predetermined power was reached, nitrogen gas was introduced into the reactor to restore the pressure, and the produced polyester carbonate resin was extruded into water, and the strands were cut to obtain pellets.

[0128] After the obtained polyester carbonate resin (pellets) was vacuum dried at 80°C for 5 hours, a long strip of resin film with a thickness of 130 μm was produced using a film-making device equipped with a single screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder setting temperature: 250°C), a T-die (width 200 mm, setting temperature: 250°C), a chilled roll (setting temperature: 120-130°C) and a winder. The obtained long strip of resin film was stretched in the width direction at a stretching temperature of 140°C and a stretching ratio of 2.7 times. Thus, a phase difference film (λ / 4 component) with a thickness of 47 μm, Re(590) of 143 nm, and an Nz coefficient of 1.2 was obtained. The Re(450) / Re(550) of the λ / 4 component is 0.856. In addition, the ISC value and thickness deviation of the λ / 4 component are shown in Table 1.

[0129] [Table 1]

[0130]

[0131] [Manufacturing Example 2: Preparation of Polarizing Film]

[0132] As the thermoplastic resin substrate, a long amorphous polyethylene terephthalate copolymer film (thickness: 100 μm) having a Tg of about 75° C. was used, and one surface of the resin substrate was subjected to a corona treatment.

[0133] To 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (degree of polymerization 4200, degree of saponification 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Mitsubishi Chemical Corporation, trade name "GOHSENX Z410") in a ratio of 9:1, 13 parts by weight of potassium iodide were added, and the resulting mixture was dissolved in water to prepare a PVA aqueous solution (coating solution).

[0134] The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60° C., thereby forming a PVA-based resin layer with a thickness of 13 μm, thereby producing a laminate.

[0135] The obtained laminate was uniaxially stretched to 2.4 times in the longitudinal direction (length direction) in an oven at 130° C. (auxiliary stretching treatment in an atmosphere).

[0136] Next, the laminate was immersed in an insolubilization bath (boric acid aqueous solution prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).

[0137] Next, the film was immersed in a dyeing bath (an iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 relative to 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single body transmittance (Ts) of the final absorption-type polarizing film reached the desired value (dyeing treatment).

[0138] Next, the sample was immersed in a crosslinking bath (boric acid aqueous solution containing 3 parts by mass of potassium iodide and 5 parts by mass of boric acid per 100 parts by mass of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment).

[0139] Then, the laminate was immersed in an aqueous boric acid solution (boric acid concentration 4 wt%, potassium iodide concentration 5 wt%) at a liquid temperature of 70°C, and simultaneously uniaxially stretched (stretching treatment in aqueous solution) in the longitudinal direction (length direction) between rollers with different circumferential speeds so that the total stretching ratio reached 5.5 times.

[0140] Then, the laminated body was immersed in a cleaning bath (an aqueous solution containing 4 parts by weight of potassium iodide per 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment).

[0141] Thereafter, the laminate was dried in an oven maintained at about 90° C. and brought into contact with a SUS heating roll maintained at a surface temperature of about 75° C. (drying shrinkage treatment). The shrinkage rate in the width direction of the laminate due to the drying shrinkage treatment was 5.2%.

[0142] In this manner, an absorption-type polarizing film having a thickness of about 5 μm was formed on the resin substrate.

[0143] A cycloolefin resin film (thickness: 25 μm) as a protective layer was attached to the surface of the obtained absorption-type polarizing film (the surface opposite to the resin substrate) via an ultraviolet curing adhesive. Specifically, the curing adhesive was applied so that the total thickness reached about 1 μm, and the film was attached using a roller press. Then, UV rays were irradiated from the cycloolefin resin film side to cure the adhesive. Next, the resin substrate was peeled off.

[0144] Thus, a polarizing film having a structure of cycloolefin resin film / absorption type polarizing film was obtained. The single body transmittance (Ts) of the polarizing film was 43.4%, and the polarization degree was 99.993%.

[0145] [Examples 1 to 3 and Comparative Examples 1 to 2]

[0146] Four sheets of the λ / 4 members obtained in Manufacturing Example 1 were stacked in order as λ / 4 member 1, λ / 4 member 2, λ / 4 member 3 and λ / 4 member 4 according to the axial relationship shown in Table 2, and the polarizing film obtained in Manufacturing Example 2 was stacked on the side of λ / 4 member 4 to produce a laminate (the angles shown in Table 2 are the axial angles of each member based on the absorption axis direction of the absorption-type polarizing film when the laminate is observed from the λ / 4 member 1 side, "+" means clockwise and "-" means counterclockwise). The stacking of each member was performed by bonding via an acrylic adhesive layer (manufactured by Nitto Denko Corporation, thickness 5 μm).

[0147] The single body transmittance, orthogonal transmittance and polarization degree of the obtained laminate are shown in Table 2. It should be noted that the laminate produced in the above-mentioned examples and comparative examples is a simple evaluation model of the display system of the above-mentioned embodiment I of the present invention. Specifically, the light incident on the laminate from the λ / 4 component 1 side and emitted from the polarizing film side can be set as the following light for evaluation: In the display system of the embodiment of the present invention, the first linear polarized light emitted from the display element to the front through the polarizing component is transmitted through the first phase difference component and the second phase difference component in sequence, and then is reflected by the reflection part and the half-reflecting mirror and further transmitted through the second phase difference component twice, and then is transmitted through the reflection part and emitted to the front.

[0148] [Table 2]

[0149]

[0150] As shown in Table 2, a display system that is configured so that the angle between the slow axes of the first phase difference member (1st λ / 4 member) and the second phase difference member (2nd λ / 4 member) is 7° or less can achieve a high degree of polarization. According to such a display system, light leakage can be appropriately suppressed.

[0151] [Example 4 and Comparative Example 3]

[0152] Four sheets of the λ / 4 members obtained in Manufacturing Example 1 were stacked in order as λ / 4 member 1, λ / 4 member 2, λ / 4 member 3 and λ / 4 member 4 according to the axial relationship shown in Table 3, and the polarizing film obtained in Manufacturing Example 2 was stacked on the side of λ / 4 member 4 to produce a laminate (the angles shown in Table 3 are the axial angles of each member based on the absorption axis direction of the absorption-type polarizing film when the laminate is observed from the λ / 4 member 1 side, "+" means clockwise and "-" means counterclockwise). The stacking of each member was performed by bonding via an acrylic adhesive layer (manufactured by Nitto Denko Corporation, thickness 5 μm).

[0153] The single body transmittance, orthogonal transmittance and polarization degree of the obtained laminate are shown in Table 3. It should be noted that the laminates produced in the above Examples and Comparative Examples are simplified evaluation models of the display system according to the above Embodiment II of the present invention.

[0154] [Table 3]

[0155]

[0156] As shown in Table 3, a display system in which the first phase difference member (1st λ / 4 member) and the second phase difference member (2nd λ / 4 member) are configured so that the angle between their slow axes is 83° to 97° can be achieved. According to such a display system, light leakage can be appropriately suppressed.

[0157] The present invention is not limited to the above-described embodiments, and various modifications are possible. For example, the above-described embodiments may be replaced with substantially the same configuration, a configuration that exhibits the same effects, or a configuration that achieves the same purpose.

[0158] Industrial Applicability

[0159] The display system according to the embodiment of the present invention can be used for a display body such as VR goggles, for example.

Claims

1. A display system, which is a display system for displaying images to a user, The display system comprises: A display element having a display surface for emitting light displaying an image forward via a polarizing member; a reflector, which is disposed in front of the display element, includes a reflective polarizing member, and reflects light emitted from the display element; A first lens portion, which is disposed on an optical path between the display element and the reflective portion; a half mirror disposed between the display element and the first lens portion, transmitting light emitted from the display element and reflecting light reflected from the reflection portion toward the reflection portion; a first λ / 4 member disposed on an optical path between the display element and the half mirror; as well as a second λ / 4 member disposed on an optical path between the half mirror and the reflecting portion, The first λ / 4 member is arranged so that the angle formed by the slow axis of the first λ / 4 member and the slow axis of the second λ / 4 member is 7° or less or 83° to 97°.

2. The display system according to claim 1, wherein: The in-plane phase difference (a) of the first λ / 4 element and the in-plane phase difference (b) of the second λ / 4 element satisfy the following formula (I): ((a)-(b)) / ((a)+(b) / 2)≤0.02(I).

3. The display system according to claim 1, wherein: The ISC values ​​of the first λ / 4 member and the second λ / 4 member are each 50 or less.

4. The display system according to claim 1, wherein: The thickness of the first λ / 4 member and the second λ / 4 member are each 100 μm or less.

5. The display system according to claim 1, wherein: The deviation in thickness of the first λ / 4 member and the second λ / 4 member is 1 μm or less.

6. The display system according to claim 1, wherein: The ISC values ​​per unit thickness of the first λ / 4 member and the second λ / 4 member are each 1 or less.

7. The display system according to claim 1, wherein: The polarization direction of the light emitted through the polarization element is substantially orthogonal to the reflection axis of the reflective polarization element. The angle between the absorption axis of the polarization member included in the display element and the slow axis of the first λ / 4 member is 40° to 50°. An angle formed between a slow axis of the first λ / 4 member and a slow axis of the second λ / 4 member is 7° or less.

8. The display system according to claim 1, wherein: The polarization direction of the light emitted through the polarization element is substantially parallel to the reflection axis of the reflective polarization element. The angle between the absorption axis of the polarization member included in the display element and the slow axis of the first λ / 4 member is 40° to 50°. The angle formed by the slow axis of the first λ / 4 member and the slow axis of the second λ / 4 member is 83° to 97°.

9. A display method, the method comprising: a step of allowing the light of the display image emitted through the polarization member to pass through the first λ / 4 member; A step of allowing the light that has passed through the first λ / 4 member to pass through a half mirror and a first lens portion; a step of allowing the light that has passed through the half mirror and the first lens portion to pass through a second λ / 4 member; a step of reflecting the light after passing through the second λ / 4 member toward the half mirror at a reflecting portion including a reflective polarization member; and a step of allowing the light reflected by the reflecting portion and the half mirror to pass through the reflecting portion via the second λ / 4 member, The first λ / 4 member is arranged so that the angle formed by the slow axis of the first λ / 4 member and the slow axis of the second λ / 4 member is 7° or less or 83° to 97°. 10 . A display comprising the display system according to claim 1 . 11 . A method for manufacturing a display comprising the display system according to claim 1 .