Polyphenol modified iron metal wire light zeolite, preparation method and application thereof, modified carbon felt, and preparation method and application thereof
Through the hydrothermal synthesis of polyphenol modified iron mordenite and modified carbon felt, the problem of difficulty in reusing adsorbent materials in sewage treatment is solved, and efficient sewage treatment and material recycling is achieved, which is in line with the green and sustainable goals.
Patent Information
- Application Number
- CN202411304407.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing sewage treatment technology, the powder form of adsorbed materials is prone to loss of quantity when reused in environmental applications, making it difficult to achieve long-term and stable utilization of materials. The traditional synthesis methods are complex and expensive, and violate the green and sustainable goals.
Polyphenols are used to modify iron metal marronite and its modified carbon felt, and hydrothermal synthesis is carried out through the "acid co-hydrolysis" method, avoiding the use of templates and adhesives, achieving efficient sewage treatment, and the closeness between the material and the carbon felt The combination solves the problem of adsorbent recovery.
It has achieved efficient wastewater treatment, especially in ammonia nitrogen adsorption, which shows high adsorption performance and rapid adsorption kinetics. Add 0.5g/L polyphenol modified iron mercury or 50cm2/L modified carbon felt to the ammonia nitrogen in the wastewater within 1 h The adsorption capacity is as high as 35-40mg/g, and there is no secondary pollution.
Smart Images

Figure CN119016030A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sewage treatment, and in particular relates to a polyphenol-modified iron metal mordenite and a preparation method and application thereof, and a modified carbon felt and a preparation method and application thereof. Background Art
[0002] Zeolites have the advantages of abundant cavities, special crystal structure, low cost, good hydrothermal stability, etc., and have been widely used as catalysts and adsorbents in the environmental field. In particular, the framework of mordenite has a unidirectional 12-membered ring channel with a pore size of 0.58-0.70 nm, and has received widespread attention as an adsorbent. In order to further improve the adsorption performance of mordenite, a variety of methods have been proposed, such as adding organic templates to direct the regulation of topological structure, morphology and porosity. However, these methods have complex synthesis processes, are expensive, and have certain toxicity, which is contrary to the goal of achieving green and sustainable synthesis.
[0003] Tannic acid (TA), as a biodegradable natural plant polyphenol, is a benign reducing agent. Since TA contains abundant carboxyl and phenolic hydroxyl groups and has a high affinity for metal ions, TA can form complexes with metal ions. In addition, the phenolic hydroxyl groups on the surface of TA give it a certain reducing ability and improved electron transfer activity. Iron-based materials are widely applicable, non-toxic and cost-effective, and Fe-TA complexes can maintain the stability of iron ions under alkaline conditions. From the perspective of environment and economy, introducing Fe-TA to enhance the adsorption capacity of zeolite through low-temperature hydrothermal is an innovative and green way.
[0004] However, most reported adsorbent materials are developed in the form of powders, which may cause quantity loss when reused in environmental applications, making it difficult to maximize the utilization efficiency of adsorbent materials. Therefore, it is necessary to explore and develop effective strategies to achieve long-term and stable utilization of materials, thereby broadening the practical environmental applications of materials. Existing methods mainly combine powder materials with solid substrates, and the manufacturing methods are mainly divided into deposition methods and in-situ growth methods. Spraying and coating techniques are the most direct deposition methods. Although this method is relatively simple to operate, the adhesion of powder materials on the substrate is weak. The in-situ growth method uses hydrothermal or solvothermal methods to enable powder materials to grow directly on the substrate, which can significantly improve the structural stability of the material. Therefore, by in-situ directional growth and anchoring of materials on a conductive carbon felt (CF) substrate, the large surface area and superior stability of CF are utilized to improve practicality while obtaining high active sites and high conductivity, which becomes an effective way to achieve sustainable utilization of adsorbent materials.
[0005] In summary, developing an adsorption material with simple process, low price, green and high efficiency is a technical problem to be solved urgently in this field. Summary of the invention
[0006] The purpose of the present invention is to provide a polyphenol-modified iron metal mordenite and a preparation method and application thereof, a modified carbon felt and a preparation method and application thereof. The polyphenol-modified iron metal mordenite and modified carbon felt obtained by the preparation method provided by the present invention can achieve efficient treatment of sewage.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing polyphenol-modified iron metal mordenite, comprising the following steps:
[0009] The silicon source-containing acidic solution and the iron source are mixed to carry out a condensation reaction to obtain a condensation system;
[0010] The condensation system and plant polyphenols are mixed to carry out a complexation reaction to obtain a polyphenol-modified iron metal precursor solution;
[0011] The polyphenol-modified iron metal precursor solution and the aluminum source-containing alkaline solution are mixed and subjected to a hydrothermal reaction to obtain the polyphenol-modified iron metal mordenite.
[0012] Preferably, the silicon source-containing acidic solution comprises a silicon source, an acid and water; the silicon source comprises sodium silicate and / or ethyl orthosilicate; the acid comprises concentrated hydrochloric acid; the iron source comprises FeCl3·6H2O and / or Fe(NO3)3·9H2O;
[0013] The molar ratio of silicon in the silicon source to iron in the iron source is 1:0.25-0.5;
[0014] The condensation reaction temperature is room temperature and the time is 8 to 12 hours.
[0015] Preferably, the plant polyphenols include tannic acid and / or gallic acid; the molar ratio of the plant polyphenols to the iron in the iron source is 1:1-3;
[0016] The temperature of the complex reaction is room temperature, and the time is 8 to 12 hours.
[0017] Preferably, the aluminum source-containing alkaline solution comprises an aluminum source, an alkali and water; the aluminum source comprises Al2(SO4)3·18H2O and / or AlCl3; the alkali comprises NaOH and / or KOH;
[0018] The molar ratio of aluminum in the aluminum source to silicon in the silicon source is 6 to 10:1.
[0019] Preferably, the pH value of the aluminum source-containing alkaline solution is 12-13.
[0020] Preferably, the temperature of the hydrothermal reaction is 160-180° C., and the time is 12-24 hours.
[0021] The present invention also provides polyphenol-modified iron metal mordenite prepared by the preparation method described in the above technical scheme.
[0022] The present invention also provides a method for preparing the modified carbon felt, comprising the following steps:
[0023] A polyphenol-modified iron metal precursor solution is prepared according to the preparation method described in the above technical scheme;
[0024] The polyphenol-modified iron metal precursor solution, the aluminum source-containing alkaline solution and the carbon felt are mixed and subjected to a hydrothermal reaction to obtain the modified carbon felt.
[0025] The present invention also provides a modified carbon felt prepared by the preparation method described in the above technical solution, comprising carbon felt and polyphenol-modified iron metal mordenite in-situ grown on the surface and in the pores of the carbon felt.
[0026] The present invention also provides the use of the polyphenol-modified iron metal mordenite described in the above technical solution or the modified carbon felt described in the above technical solution in sewage treatment.
[0027] The present invention provides a preparation method of polyphenol-modified iron metal mordenite, comprising the following steps: mixing a silicon-containing acidic solution and an iron source, performing a condensation reaction, and obtaining a condensation system; mixing the condensation system and plant polyphenols, performing a complexation reaction, and obtaining a polyphenol-modified iron metal precursor solution; mixing the polyphenol-modified iron metal precursor solution and an aluminum-containing alkaline solution, performing a hydrothermal reaction, and obtaining the polyphenol-modified iron metal mordenite. The preparation method provided by the present invention is simple, and adopts the "acid co-hydrolysis" approach to synthesize the polyphenol-modified iron metal mordenite by hydrothermal method, without the need for a template or adhesive, and without the need for high-temperature calcination and post-treatment, thereby avoiding the energy consumption associated with calcination and the emission of waste gases such as carbon dioxide and nitrogen oxides.
[0028] The present invention also provides a method for preparing modified carbon felt. The modified carbon felt prepared by the present invention has surface hydroxyl groups modified, and the phenolic hydroxyl groups in polyphenols tend to be thermally oxidized into quinones, so that the material and the carbon felt are more closely combined during the hydrothermal reaction process, and the modified carbon felt solves the problem of adsorbent recovery well without secondary pollution.
[0029] The present invention also provides the use of the polyphenol-modified iron metal mordenite or the modified carbon felt in the above technical solution in sewage treatment. The polyphenol-modified iron metal mordenite or modified carbon felt provided by the present invention has an ordered microporous structure, exhibits high adsorption performance and rapid adsorption kinetics. The application example results show that the addition of 0.5 g / L polyphenol-modified iron metal mordenite or 50 cm 2 / L modified carbon felt has an adsorption capacity of up to 35-40 mg / g of ammonia nitrogen in sewage within 1 hour. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 SEM images of Fe-TA-MOR prepared in Example 1 and MOR prepared in Comparative Example 1, wherein a is MOR, b is Fe-TA-MOR, c is Fe-TA-MOR@CF prepared in Example 4, and d is XRD spectra of MOR and Fe-TA-MOR;
[0031] Figure 2 It is a graph showing the adsorption capacity of ammonia nitrogen by Fe-TA-MOR prepared in Example 2, MOR prepared in Comparative Example 2, and Fe-MOR prepared in Comparative Example 3;
[0032] Figure 3 This is a graph showing the adsorption capacity of Fe-TA-MOR prepared in Example 3 for ammonia nitrogen at different dosages;
[0033] Figure 4 This is the adsorption kinetics diagram of ammonia nitrogen by Fe-TA-MOR prepared in Example 3;
[0034] Figure 5 This is a graph showing the adsorption capacity of ammonia nitrogen for Fe-TA-MOR@CF prepared in Example 4, MOR@CF prepared in Comparative Example 4, and Fe-MOR@CF prepared in Comparative Example 5. DETAILED DESCRIPTION
[0035] The present invention provides a method for preparing polyphenol-modified iron metal mordenite, comprising the following steps:
[0036] The silicon source-containing acidic solution and the iron source are mixed to carry out a condensation reaction to obtain a condensation system;
[0037] The condensation system and plant polyphenols are mixed to carry out a complexation reaction to obtain a polyphenol-modified iron metal precursor solution;
[0038] The polyphenol-modified iron metal precursor solution and the aluminum source-containing alkaline solution are mixed and subjected to a hydrothermal reaction to obtain the polyphenol-modified iron metal mordenite.
[0039] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.
[0040] The present invention mixes a silicon source-containing acidic solution and an iron source to carry out a condensation reaction to obtain a condensation system.
[0041] In the present invention, the acidic solution containing silicon source preferably comprises silicon source, acid and water; the silicon source preferably comprises sodium silicate and / or ethyl orthosilicate; the acid preferably comprises concentrated hydrochloric acid; the mass concentration of the concentrated hydrochloric acid is preferably 36-38%; the water is preferably deionized water. In the present invention, the pH value of the acidic solution containing silicon source is preferably 2-3. In the present invention, the dosage ratio of the concentrated hydrochloric acid and water is preferably 3-5 drops: 20-30 mL. The present invention has no special limitation on the dosage ratio of the silicon source and water, as long as the silicon source can be evenly dispersed.
[0042] In the present invention, the silicon source-containing acidic solution is preferably obtained by mixing a silicon source, water and an acid; the mixing is preferably: dispersing the silicon source in water to obtain a silicon source solution, and then adding the acid to the silicon source solution. In the present invention, the acid is preferably added to the silicon source solution under vigorous stirring.
[0043] In the present invention, the iron source preferably includes FeCl3·6H2O and / or Fe(NO3)3·9H2O; the molar ratio of silicon in the silicon source to iron in the iron source is preferably 1:0.25-0.5, and more preferably 1:0.25.
[0044] In the present invention, the temperature of the condensation reaction is preferably room temperature, specifically 25°C; the time is preferably 8 to 12 hours, more preferably 12 hours; the condensation reaction is preferably carried out under stirring. The present invention has no special limitation on the stirring process, and a method familiar to those skilled in the art can be used.
[0045] After obtaining the condensation system, the present invention mixes the condensation system with plant polyphenols to carry out a complexation reaction to obtain a polyphenol-modified iron metal precursor solution.
[0046] In the present invention, the plant polyphenols preferably include tannic acid and / or gallic acid; the molar ratio of the plant polyphenols to the iron in the iron source is preferably 1:1-3, and more preferably 1:1.5. In the present invention, the introduction of plant polyphenols can increase the adhesion of the polyphenol-modified iron metal precursor solution without changing the framework structure, making it easier for the adsorbent material to form defects, increase roughness, and increase adsorption sites. The phenolic hydroxyl functional groups on the surface of plant polyphenols can be protonated under acidic conditions, increasing electrostatic attraction and enhancing adsorption capacity.
[0047] In the present invention, the complexation reaction is preferably carried out under stirring. In the present invention, the temperature of the complexation reaction is preferably room temperature, specifically 25° C.; the time is preferably 8 to 12 hours, more preferably 12 hours.
[0048] After obtaining the polyphenol-modified iron metal precursor solution, the present invention mixes the polyphenol-modified iron metal precursor solution with an alkaline solution containing an aluminum source, and performs a hydrothermal reaction to obtain the polyphenol-modified iron metal mordenite.
[0049] In the present invention, the aluminum source-containing alkaline solution preferably includes an aluminum source, an alkali and water; the aluminum source preferably includes Al2(SO4)3·18H2O and / or AlCl3; the alkali preferably includes NaOH and / or KOH; the water is preferably deionized water. In the present invention, the molar ratio of aluminum in the aluminum source to silicon in the silicon source is preferably 6 to 10:1, and more preferably 6:1.
[0050] In the present invention, the pH value of the aluminum source-containing alkaline solution is preferably 12 to 13; when the aluminum source is Al2(SO4)3·18H2O, the dosage ratio of Al2(SO4)3·18H2O to water is preferably 1.34 to 2.68 g:15 to 20 mL.
[0051] In the present invention, the aluminum source-containing alkaline solution is preferably obtained by mixing an aluminum source, water and an alkali; the mixing is preferably: adding an aluminum source to water to obtain an aluminum source solution, and then adding an alkali to the aluminum source solution for stirring to obtain a clarified aluminum source-containing alkaline solution. In the present invention, the stirring time is preferably 30 to 60 minutes. In the present invention, the pH value of the solution is adjusted by using an alkali to make the iron-polyphenol network more stable.
[0052] In the present invention, the mixing of the polyphenol-modified iron metal precursor solution and the aluminum source-containing alkaline solution is preferably carried out under stirring, and the stirring time is preferably 8 to 12 hours, and more preferably 12 hours.
[0053] In the present invention, the temperature of the hydrothermal reaction is preferably 160-180° C., more preferably 180° C.; the time of the hydrothermal reaction is preferably 12-24 h, more preferably 12 h; and the hydrothermal reaction is preferably carried out in a reactor.
[0054] After the hydrothermal reaction is completed, the present invention also preferably includes naturally cooling, washing and drying the obtained hydrothermal reaction system in sequence; after the natural cooling, the temperature of the hydrothermal reaction system is preferably below 60°C; the washing is preferably carried out alternately using water and ethanol in sequence, and the number of times the water and ethanol are washed independently is preferably 3 times; the drying temperature is preferably 60°C, and the time is preferably 12 hours.
[0055] The present invention adopts the "acid co-hydrolysis" approach to prepare polyphenol-modified iron metal mordenite through hydrothermal synthesis, without the need for templates or adhesives, high-temperature calcination and post-treatment, thus avoiding the energy consumption associated with calcination and the emission of waste gases such as carbon dioxide and nitrogen oxides.
[0056] The present invention also provides polyphenol-modified iron metal mordenite prepared by the preparation method described in the above technical solution. In the present invention, the particle size of the polyphenol-modified iron metal mordenite is preferably 10 to 15 μm.
[0057] The present invention also provides a method for preparing the modified carbon felt, comprising the following steps:
[0058] A polyphenol-modified iron metal precursor solution is prepared according to the preparation method described in the above technical scheme;
[0059] The polyphenol-modified iron metal precursor solution, the aluminum source-containing alkaline solution and the carbon felt are mixed and subjected to a hydrothermal reaction to obtain the modified carbon felt.
[0060] In the present invention, before the mixing, the carbon felt is preferably pretreated; the pretreatment preferably includes acid leaching, cleaning and drying in sequence. In the present invention, the acid leaching solution preferably includes sulfuric acid and nitric acid; the mass concentration of the sulfuric acid is preferably 98.0%, and the mass concentration of the nitric acid is preferably 68%; the volume ratio of the sulfuric acid and the nitric acid is preferably 1:3; the acid leaching is preferably carried out under the condition of water bath heating; the temperature of the acid leaching is preferably 80°C; and the time is preferably 3 to 4 hours. In the present invention, the cleaning is preferably ultrasonic cleaning and water washing in sequence; the solvent used for the ultrasonic cleaning is preferably ethanol; the time of the ultrasonic cleaning is preferably 30 to 40 minutes; the water used for the water washing is preferably deionized water; the number of water washings is preferably 2 to 3 times. In the present invention, the drying temperature is preferably 60 to 65°C; the time is preferably 6 to 8 hours; the drying is preferably carried out in a vacuum drying oven.
[0061] In the present invention, the size of the carbon felt is preferably 2-5 cm×2-5 cm×0.1-0.3 cm.
[0062] In the present invention, the conditions of the hydrothermal reaction are consistent with the conditions of the hydrothermal reaction defined in the above technical solution, and will not be repeated here.
[0063] After the hydrothermal reaction is completed, the present invention also preferably includes naturally cooling the obtained hydrothermal reaction system in sequence, washing and drying the obtained carbon felt; after the natural cooling, the temperature of the hydrothermal reaction system is preferably below 60°C; the washing is preferably carried out alternately using water and ethanol in sequence, and the number of times the water and ethanol are washed independently is preferably 3 times; the drying temperature is preferably 60°C, and the time is preferably 6h.
[0064] The present invention also provides a modified carbon felt prepared by the preparation method described in the above technical solution, comprising carbon felt and polyphenol-modified iron metal mordenite in-situ grown on the surface and in the pores of the carbon felt.
[0065] In the present invention, the content of the polyphenol-modified iron metal mordenite on the modified carbon felt is preferably 0.001 to 0.005 g / cm 2 .
[0066] The present invention also provides the use of the polyphenol-modified iron metal mordenite described in the above technical solution or the modified carbon felt described in the above technical solution in sewage treatment.
[0067] In the present invention, when the polyphenol-modified iron metal mordenite or the modified carbon felt described in the above technical solution is used for sewage treatment, the addition amount of the polyphenol-modified iron metal mordenite is preferably 0.1-1.0 g / L, and the addition amount of the modified carbon felt is preferably 25-100 cm 2 / L.
[0068] In the present invention, the sewage treatment is preferably carried out at a constant temperature, specifically preferably at 25°C; the sewage treatment is preferably accompanied by an oscillation reaction, and the oscillation reaction time is preferably 0.5 to 1 hour. The present invention can fully adsorb ammonia nitrogen or heavy metal ions in the sewage by the polyphenol-modified iron metal mordenite or modified carbon felt through the oscillation reaction accompanied by sewage treatment.
[0069] The modified carbon felt provided by the invention has no secondary pollution and can solve the problem of adsorbent recovery.
[0070] To further illustrate the present invention, a polyphenol-modified iron metal mordenite and its preparation method and application, a modified carbon felt and its preparation method and application provided by the present invention are described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0071] Example 1
[0072] 6.34 g of sodium silicate and 30 mL of deionized water were mixed, and 3 drops of concentrated hydrochloric acid were added under vigorous stirring to obtain an acidic solution containing a silicon source with a pH value of 3.
[0073] 0.1 g of FeCl3·6H2O was added to the acidic solution containing silicon source so that the molar ratio of silicon to iron was 1:0.25. The mixture was stirred at 25°C for 12 h to completely condense sodium silicate and FeCl3·6H2O to obtain a condensation system.
[0074] 0.31 g of tannic acid (TA) was added to the condensation system to make the molar ratio of tannic acid to iron 1:2, and stirring was continued at 25°C for 12 h to construct a polyphenol-iron metal network and obtain a polyphenol-modified iron metal precursor solution.
[0075] 1.34 g of Al2(SO4)3·18H2O and 20 mL of deionized water were mixed, 1 g of NaOH was added and stirred for 30 min to adjust the pH value of the solution to 12, and a clear alkaline solution containing an aluminum source was obtained.
[0076] The polyphenol-modified iron metal precursor solution and the aluminum source-containing alkaline solution were mixed and stirred for 2 hours, wherein the molar ratio of aluminum to silicon was 6:1, and then transferred to a reactor for hydrothermal synthesis at 160°C for 12 hours. After naturally cooling to below 60°C, the solution was washed alternately with deionized water and ethanol for 3 times and then dried at 60°C for 12 hours to obtain the polyphenol-modified iron metal silk zeolite Fe-TA-MOR.
[0077] Example 2
[0078] 9.05 g of sodium silicate and 40 mL of deionized water were mixed, and 3 drops of concentrated hydrochloric acid were added under vigorous stirring to obtain an acidic solution containing a silicon source with a pH value of 3.
[0079] 0.1 g of FeCl3·6H2O was added to the acidic solution containing silicon source so that the molar ratio of silicon to iron was 1:0.25. The mixture was stirred at 25°C for 12 h to completely condense sodium silicate and FeCl3·6H2O to obtain a condensation system.
[0080] 0.42 g of tannic acid (TA) was added to the condensation system to make the molar ratio of tannic acid to iron 1:1.5, and stirring was continued at 25°C for 8 h to construct a polyphenol-iron metal network to obtain a polyphenol-modified iron metal precursor solution.
[0081] 2.68 g of Al2(SO4)3·18H2O and 20 mL of deionized water were mixed, 2 g of NaOH was added and stirred for 60 min to adjust the pH value of the solution to 13, and a clear alkaline solution containing an aluminum source was obtained.
[0082] The polyphenol-modified iron metal precursor solution and the aluminum source-containing alkaline solution were mixed and stirred for 1 hour, wherein the molar ratio of aluminum to silicon was 10:1, and then transferred to a reactor for hydrothermal synthesis at 180°C for 12 hours. After naturally cooling to below 60°C, the solution was washed alternately with deionized water and ethanol for 3 times and then dried at 60°C for 12 hours to obtain the polyphenol-modified iron metal silk zeolite Fe-TA-MOR.
[0083] Example 3
[0084] 6.34 g of sodium silicate and 40 mL of deionized water were mixed, and 5 drops of concentrated hydrochloric acid were added under vigorous stirring to obtain an acidic solution containing a silicon source with a pH value of 2.
[0085] 0.2 g of FeCl3·6H2O was added to the acidic solution containing silicon source so that the molar ratio of silicon to iron was 1:0.5. The mixture was stirred at 25°C for 10 h to completely condense sodium silicate and FeCl3·6H2O to obtain a condensation system.
[0086] 0.42 g of tannic acid (TA) was added to the condensation system to make the molar ratio of tannic acid to iron 1:3, and stirring was continued at 25°C for 10 h to construct a polyphenol-iron metal network to obtain a polyphenol-modified iron metal precursor solution.
[0087] 2.68 g of Al2(SO4)3·18H2O was dissolved in 15 mL of deionized water, and 2 g of NaOH was added and stirred for 60 min to adjust the pH value of the solution to 13, thereby obtaining a clear alkaline solution containing an aluminum source.
[0088] The polyphenol-modified iron metal precursor solution and the aluminum source-containing alkaline solution were mixed and stirred for 1 hour, wherein the molar ratio of aluminum to silicon was 8:1, and then transferred to a reactor for hydrothermal synthesis at 180°C for 24 hours. After naturally cooling to below 60°C, the solution was washed alternately with deionized water and ethanol for 3 times and then dried at 60°C for 12 hours to obtain the polyphenol-modified iron metal silk zeolite Fe-TA-MOR.
[0089] Example 4
[0090] 6.34 g of sodium silicate and 30 mL of deionized water were mixed, and 3 drops of concentrated hydrochloric acid were added under vigorous stirring to obtain an acidic solution containing a silicon source with a pH value of 3.
[0091] 0.1 g of FeCl3·6H2O was added to the acidic solution containing silicon source so that the molar ratio of silicon to iron was 1:0.25. The mixture was stirred at 25°C for 12 h to completely condense sodium silicate and FeCl3·6H2O to obtain a condensation system.
[0092] 0.31 g of tannic acid (TA) was added to the condensation system, wherein the molar ratio of tannic acid to iron was 1:2, and stirring was continued at 25°C for 12 h to construct a polyphenol-iron metal network and obtain a polyphenol-modified iron metal precursor solution.
[0093] 1.34 g of Al2(SO4)3·18H2O was dissolved in 20 mL of deionized water, 1 g of NaOH was added and stirred for 30 min to adjust the pH value of the solution to 12, and a clear alkaline solution containing an aluminum source was obtained.
[0094] A carbon felt with a size of 2cm×2cm×0.2cm was immersed in a mixture of sulfuric acid and nitric acid (wherein the mass concentration of sulfuric acid was 98.0%, the mass concentration of nitric acid was 68%; the volume ratio of sulfuric acid to nitric acid was 1:3), and acid-immersed at 80°C for 3h; the carbon felt after acid immersion was ultrasonically cleaned with ethanol for 30min, and then washed with water 3 times; the washed carbon felt was dried at 60°C for 6h to obtain a pretreated carbon felt.
[0095] The polyphenol-modified iron metal precursor solution and the aluminum source alkaline solution were mixed and stirred for 2 hours, and then transferred to a reactor with the pretreated carbon felt for hydrothermal synthesis at 180°C for 12 hours. After naturally cooling to below 60°C, the obtained carbon felt was washed alternately with deionized water and ethanol for 3 times, and the drying temperature was 60°C for 6 hours to obtain the polyphenol-modified iron metal silk zeolite in-situ grown modified carbon felt Fe-TA-MOR@CF, wherein the content of polyphenol-modified iron metal silk zeolite on the modified carbon felt was 0.001 g / cm 2 .
[0096] Comparative Example 1
[0097] The silicon source acidic solution and aluminum source alkaline solution prepared in Example 1 were mixed and stirred for 2 hours, transferred to a reactor for hydrothermal synthesis at 160° C. for 12 hours, naturally cooled to below 60° C., and washed alternately with deionized water and ethanol for 3 times. The drying temperature was 60° C. and the drying time was 12 hours to obtain mordenite MOR.
[0098] Comparative Example 2
[0099] The silicon-containing acidic solution and the aluminum-containing alkaline solution prepared in Example 2 were mixed and stirred for 1 hour, transferred to a reactor for hydrothermal synthesis at 180°C for 12 hours, naturally cooled to below 60°C, and then washed alternately with deionized water and ethanol for 3 times. The drying temperature was 80°C and the drying time was 8 hours to obtain mordenite MOR.
[0100] Comparative Example 3
[0101] The condensation system prepared in Example 2 and the aluminum source alkaline solution were mixed and stirred for 1 hour, transferred to a reactor for hydrothermal synthesis at 180°C for 12 hours, naturally cooled to below 60°C, and washed alternately with deionized water and ethanol for 3 times. The drying temperature was 80°C and the drying time was 8 hours to obtain iron metal silk zeolite Fe-MOR.
[0102] Comparative Example 4
[0103] The silicon-containing acidic solution and the aluminum-containing alkaline solution prepared in Example 4 were mixed and stirred for 2 hours, and transferred to a reactor with the pretreated carbon felt for hydrothermal synthesis at 180°C for 12 hours. After naturally cooling to below 60°C, the obtained carbon felt was washed alternately with deionized water and ethanol for 3 times at a drying temperature of 60°C and a drying time of 6 hours to obtain mordenite in-situ grown modified carbon felt MOR@CF.
[0104] Comparative Example 5
[0105] The condensation system prepared in Example 4 and the alkaline solution containing an aluminum source were mixed and stirred for 2 hours, and transferred to a reactor with the pretreated carbon felt for hydrothermal synthesis at 180°C for 12 hours. After naturally cooling to below 60°C, the obtained carbon felt was washed alternately with deionized water and ethanol for 3 times at a drying temperature of 60°C and a drying time of 6 hours to obtain iron metal silk zeolite in situ grown modified carbon felt Fe-MOR@CF.
[0106] Application Example 1
[0107] The mordenite MOR prepared in Comparative Example 2, the iron metal mordenite Fe-MOR prepared in Comparative Example 3, and the polyphenol-modified iron metal mordenite Fe-TA-MOR prepared in Example 2 were used for adsorption of ammonia nitrogen in sewage.
[0108] Due to the presence of ammonia nitrogen (NH4 + -N) has an average concentration of about 40 mgN / L. Therefore, the present invention uses NH4Cl dried to constant weight to prepare 40 mL of a 40 mgN / L ammonia nitrogen solution and places it in a centrifuge tube. 40 mg of adsorbent is added and the solution is shaken in a constant temperature shaker at 25°C for 1 hour to allow the ammonia nitrogen to be fully adsorbed by the adsorbent. The residual ammonia nitrogen concentration is determined by sampling and Nessler's reagent spectrophotometry.
[0109] Application Example 2
[0110] The polyphenol-modified iron metal mordenite Fe-TA-MOR prepared in Example 3 was used to adsorb ammonia nitrogen in sewage.
[0111] 40 mL of 40 mg N / L ammonia nitrogen solution was prepared using NH4Cl dried to constant weight and placed in a centrifuge tube. 10, 20, 40, 80, and 200 mg of adsorbent were added respectively, and the mixture was shaken in a constant temperature shaker at 25°C for 1 h.
[0112] Use NH4Cl dried to constant weight to prepare 40mgN / L ammonia nitrogen solution (10mL) and place it in a centrifuge tube. Add 10mg of adsorbent and shake in a constant temperature shaker at 25℃ for 5, 10, 15, 30, 60, 120, and 180 minutes. Take samples and determine the residual ammonia nitrogen concentration by Nessler's reagent spectrophotometry.
[0113] Application Example 3
[0114] The Fe-TA-MOR@CF prepared in Example 4, the MOR@CF prepared in Comparative Example 4, and the Fe-MOR@CF prepared in Comparative Example 5 were used to adsorb ammonia nitrogen in sewage.
[0115] Prepare 40 mL of 40 mg N / L ammonia nitrogen solution using NH4Cl dried to constant weight and place in a centrifuge tube. Add 50 cm 2 / L of MOR@CF, Fe-MOR@CF and Fe-TA-MOR@CF were shaken in a constant temperature shaker at 25℃ for 1h.
[0116] Application Example 4
[0117] The polyphenol-modified iron metal mordenite Fe-TA-MOR prepared in Example 3 was used to adsorb heavy metal strontium (Sr). 10 mL of 10 mg / L SrCl2 solution was prepared and placed in a centrifuge tube, and the adsorbent dosage was 1.2 g / L. The mixture was shaken in a constant temperature shaker at 25°C for 1 h. The residual Sr was determined by inductively coupled plasma spectrometry (ICP). 2+ concentration.
[0118] Performance Testing
[0119] (1) The Fe-TA-MOR prepared in Example 1 and the MOR prepared in Comparative Example 1 were characterized by SEM and XRD. Figure 1 As shown, Figure 1 a and b are SEM images of MOR and Fe-TA-MOR. Figure 1 c is a physical picture of Fe-TA-MOR@CF obtained in Example 4. Figure 1 d is the XRD spectra of MOR and Fe-TA-MOR.
[0120] Depend on Figure 1 It can be seen that the Fe-TA-MOR prepared in Example 1 and the MOR prepared in Comparative Example 1 are flower-like microspheres composed of prismatic crystals with a size of 10 to 15 μm. Compared with MOR, Fe-TA-MOR is modified with polyphenols, and the prism size becomes larger, the flower-like microspheres are more uniform, the surface becomes rough, and the adsorption sites increase, which is conducive to the adsorption of ammonia nitrogen. According to the standard card comparison, MOR is orthorhombic zeolite, and the diffraction peaks at 2θ=15.84°, 25.99° and 30.58° correspond to (211), (400) and (332) crystal planes, respectively (JCPDS41-1478). After Fe and TA doping, the new diffraction peak at 2θ=44.67° indicates the presence of iron (JCPDS06-0696), proving the successful synthesis of Fe-TA-MOR.
[0121] (2) The adsorption capacity of ammonia nitrogen by the mordenite MOR, the iron-containing mordenite Fe-MOR and the iron-containing mordenite Fe-TA-MOR modified by polyphenol in Application Example 1 is as follows: Figure 2 As shown by Figure 2 It can be seen that under the conditions of 1 g / L adsorbent dosage and 40 mg / L initial ammonia nitrogen concentration, the adsorption capacities of the silk zeolite MOR prepared in Comparative Example 2, the iron-containing silk zeolite Fe-MOR prepared in Comparative Example 3, and the polyphenol-modified iron metal silk zeolite Fe-TA-MOR prepared in Example 2 are 17.0 mg / g, 4.3 mg / g, and 28.5 mg / g, respectively. Among them, Fe-TA-MOR has the largest adsorption capacity for ammonia nitrogen, indicating that silk zeolite itself has a certain adsorption capacity for ammonia nitrogen (equivalent to commercial artificial zeolite). The "acid co-hydrolysis" approach is adopted, and the doped Fe exists in the framework structure and microporous channels, in which isolated Fe occupies part of the microporous channels, making them narrower and unable to effectively adsorb ammonia nitrogen, but improving the conductivity of MOR. In addition, at high temperature, TA and the isolated iron elements in the microporous channels are complexed to form channels with different pore sizes, which improves the adsorption performance of ammonia nitrogen.
[0122] (3) The adsorption capacity of Fe-TA-MOR prepared in Example 3 of Application Example 2 for ammonia nitrogen at dosages of 0.25, 0.5, 1, 2, and 5 g / L (corresponding to 10, 20, 40, 80, and 200 mg of adsorbent added) is shown in Figure 2. Figure 3 As shown by Figure 3 It can be seen that with the increase in the amount of adsorbent added, the ammonia nitrogen removal rate gradually increased to nearly 90%. The intersection of the adsorption capacity and the removal rate shows that the optimal dosage is 0.85g / L. In subsequent experiments, both the removal rate and the adsorption capacity were taken into consideration, and 1g / L was selected for subsequent experiments.
[0123] The adsorption kinetics of ammonia nitrogen by Fe-TA-MOR prepared in Example 3 of Application Example 2 is shown in FIG. Figure 4 As shown by Figure 4 It can be seen that the adsorption of ammonia nitrogen by Fe-TA-MOR can be divided into three stages: rapid adsorption (0-10 min), slow adsorption (10-60 min) and easing adsorption (60-180 min), which conforms to the quasi-second-order kinetic model.
[0124] (4) The adsorption capacity images of ammonia nitrogen for Fe-TA-MOR@CF prepared in Example 4 of Application Example 3, MOR@CF prepared in Comparative Example 4, and Fe-MOR@CF prepared in Comparative Example 5 are shown in FIG. Figure 5 As shown. Figure 5It can be seen that the adsorption capacity of MOR@CF, Fe-MOR@CF and Fe-TA-MOR@CF for ammonia nitrogen are 21.1 mg / g, 1.3 mg / g and 35.5 mg / g, respectively, which is 25% higher than that of directly adding adsorbent. It is speculated that this is because the surface hydroxyl groups of carbon felt are modified, and the phenolic hydroxyl groups in TA tend to be thermally oxidized into quinones, which makes the material more tightly combined with carbon felt during the hydrothermal reaction. In addition, the modified carbon felt solves the problem of adsorbent recovery well without secondary pollution.
[0125] (5) The Fe-TA-MOR prepared in Example 3 of Application Example 4 was used to adsorb heavy metal strontium (Sr) at an initial concentration of 10 mg / L. 2+ The residual concentrations were 0.63 (adsorbent dosage was 1 g / L) and 0.30 mg / L (adsorbent dosage was 2 g / L), and the corresponding removal rates were 94% and 97%, respectively.
[0126] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing polyphenol-modified iron metal mordenite, characterized in that: The following steps are involved: The silicon source-containing acidic solution and the iron source are mixed to carry out a condensation reaction to obtain a condensation system; The condensation system and plant polyphenols are mixed to carry out a complexation reaction to obtain a polyphenol-modified iron metal precursor solution; The polyphenol-modified iron metal precursor solution and the aluminum source-containing alkaline solution are mixed and subjected to a hydrothermal reaction to obtain the polyphenol-modified iron metal mordenite.
2. The preparation method according to claim 1, characterized in that: The silicon source-containing acidic solution includes a silicon source, an acid and water; the silicon source includes sodium silicate and / or ethyl orthosilicate; the acid includes concentrated hydrochloric acid; the iron source includes FeCl3·6H2O and / or Fe(NO3)3·9H2O; The molar ratio of silicon in the silicon source to iron in the iron source is 1:0.25-0.5 The condensation reaction temperature is room temperature and the time is 8 to 12 hours.
3. The preparation method according to claim 1, characterized in that: The plant polyphenols include tannic acid and / or gallic acid; the molar ratio of the plant polyphenols to the iron in the iron source is 1:1-3; The temperature of the complex reaction is room temperature, and the time is 8 to 12 hours.
4. The preparation method according to claim 2, characterized in that: The aluminum source-containing alkaline solution comprises an aluminum source, an alkali and water; the aluminum source comprises Al2(SO4)3·18H2O and / or AlCl3; the alkali comprises NaOH and / or KOH; The molar ratio of aluminum in the aluminum source to silicon in the silicon source is 6 to 10:
1.
5. The preparation method according to claim 1 or 4, characterized in that: The pH value of the aluminum source-containing alkaline solution is 12-13.
6. The preparation method according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 160-180° C. and the time is 12-24 hours.
7. The polyphenol-modified iron metal mordenite prepared by the preparation method according to any one of claims 1 to 6.
8. A method for preparing modified carbon felt, characterized in that: The following steps are involved: A polyphenol-modified iron metal precursor solution is prepared according to the preparation method of claim 1; The polyphenol-modified iron metal precursor solution, the aluminum source-containing alkaline solution and the carbon felt are mixed and subjected to a hydrothermal reaction to obtain the modified carbon felt.
9. The modified carbon felt prepared by the preparation method according to claim 8, characterized in that: The invention comprises a carbon felt and a polyphenol-modified iron metal mordenite in-situ grown on the surface and in the pores of the carbon felt.
10. Use of the polyphenol-modified iron metal mordenite according to claim 7 or the modified carbon felt according to claim 9 in sewage treatment.
Citation Information
Cited By
Controllable preparation method of molecular welding zeolite coating with high adsorption capacity in extreme environment
CN119592111A