Porous titanium-based denitration catalyst as well as preparation method and application thereof
By designing a porous titanium-based denitrogenation catalyst, the problem of poor diffusion performance in the titanium-based catalyst is solved, the utilization rate of the catalyst and the conversion of nitrogen oxides are improved, the mechanical strength and stability are enhanced, and the efficient nitrogen oxide detachment is achieved remove.
Patent Information
- Application Number
- CN202411147307.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
The internal diffusion performance of titanium-based denitrification catalysts is poor, resulting in low catalyst utilization and low nitrogen oxide conversion. The existing technology lacks considerations to effectively solve the internal and external diffusion problems of pore structures.
Design a porous titanium-based denitrification catalyst, adjust the pore size to 2-3 μm by adding silicon oxide and alumina to the support, and adopting a specific preparation method, including dissolved in water, drying and calcining of the mixture, to form a high internal A catalyst for diffusion properties.
The internal utilization rate of the catalyst and the performance of catalytic reduction of nitrogen oxides are improved, the mechanical strength and service life are enhanced, and the conversion rate of NOx and the stability of the catalyst are significantly improved.
Smart Images

Figure CN119016041A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of environmental protection and industrial denitration, and in particular to a porous titanium-based denitration catalyst and a preparation method and application thereof. Background Art
[0002] Nitrogen oxides (NO) are one of the air pollutants x It not only causes environmental problems such as acid rain, photochemical smog and greenhouse effect, but also damages the human respiratory system and even induces cancer. x Among control technologies, the ammonia selective catalytic reduction of nitrogen oxides (NH3-SCR) technology has been widely used. The titanium-based catalyst with a reaction temperature window of 200-400°C is the core of the NH3-SCR denitrification process, but the internal utilization rate of the catalyst powder is low, which will lead to a large amount of raw materials being wasted, which indirectly increases the production cost of the catalyst.
[0003] The NH3-SCR denitration reaction on titanium-based catalysts involves a complex macroscopic reaction kinetic process. In practical applications, in addition to the intrinsic reaction kinetic process, external diffusion and internal diffusion will also affect the activity of the catalyst. At present, many researchers mainly focus on studying the intrinsic reaction kinetic process, and often ignore the influence of internal and external diffusion on the reaction, especially the influence of internal diffusion. However, on molded catalysts, the size of the internal diffusion efficiency will greatly affect the final catalyst activity and cannot be ignored. Especially at high temperature and high space velocity, the influence of internal diffusion on the reaction is more significant.
[0004] In previous studies, although various means were used to improve the overall denitrification activity of the catalyst, there was a lack of consideration of the internal and external diffusion issues of the pore structure. The pore size of traditional titanium-based denitrification catalysts is generally concentrated in the nanoscale, about 50nm, and its internal diffusion efficiency is low, resulting in low catalyst activity. Summary of the invention
[0005] The main purpose of the present invention is to provide a porous titanium-based denitration catalyst and a preparation method and application thereof, so as to solve the problem of low catalytic activity of the titanium-based denitration catalyst.
[0006] In order to achieve the above-mentioned purpose, according to the first aspect of the present invention, a porous titanium-based denitration catalyst is provided, comprising 30-65 parts of a carrier and 0.5-5 parts of an active component loaded thereon; wherein the carrier comprises titanium dioxide, silicon oxide and aluminum oxide, and the active component comprises at least one of vanadium pentoxide, tungsten oxide, manganese oxide, cerium oxide, copper oxide and iron oxide; the pore size of the porous titanium-based denitration catalyst is 2-3 μm.
[0007] The present invention can improve the internal utilization rate of the catalyst and improve the performance of the catalyst in catalyzing the selective reduction of nitrogen oxides by ammonia by designing the pore size of the porous titanium-based denitration catalyst. In addition, the present invention can ensure that the catalyst has good stability by selecting the weight of the carrier and the active component; by adding silicon oxide and aluminum oxide to the carrier, the mechanical strength can be further improved and the service life of the catalyst can be enhanced.
[0008] Furthermore, in the carrier, the mass ratio of titanium dioxide, silicon oxide and aluminum oxide is (250-270):(6-12):(6-12).
[0009] According to a second aspect of the present invention, there is provided a method for preparing the porous titanium-based denitration catalyst according to the first aspect of the present invention, comprising the following steps:
[0010] dissolving the active ingredient in water to obtain an active agent;
[0011] Mixing a pore structure modifier, a titanium source, a silicon source, an aluminum source, and a binder to obtain a first mixture;
[0012] adding an active agent to the first mixture to obtain a second mixture;
[0013] mixing the second mixture with a lubricant to obtain a third mixture;
[0014] The third mixture is dried and calcined to obtain a porous titanium-based denitration catalyst.
[0015] Furthermore, the active component is at least one of a vanadium source, a tungsten source, a manganese source, a cerium source, a copper source, and an iron source.
[0016] Furthermore, the pore structure modifier is at least one of plastic, rosin, and sawdust.
[0017] Furthermore, the binder is at least one of hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxymethyl cellulose and polyethylene oxide.
[0018] Furthermore, the lubricant is at least one of glycerol, palm oil and paraffin oil.
[0019] Furthermore, the titanium source is at least one of tetrabutyl titanate, titanyl sulfate, and titanium oxide.
[0020] Furthermore, the aluminum source is at least one of aluminum chloride and aluminum oxide.
[0021] Furthermore, the silicon source is at least one of silicon chloride and silicon oxide.
[0022] Furthermore, the vanadium source is at least one of ammonium metavanadate and vanadium pentoxide.
[0023] Furthermore, the tungsten source is at least one of ammonium metatungstate and tungsten oxide.
[0024] Furthermore, the manganese source is at least one of manganese nitrate, manganese sulfate, potassium permanganate and manganese oxide.
[0025] Furthermore, the cerium source is at least one of cerium nitrate and cerium oxide.
[0026] Furthermore, the copper source is at least one of copper nitrate, copper sulfate and copper oxide.
[0027] Furthermore, the iron source is at least one of ferric nitrate, ferrous sulfate and ferric oxide.
[0028] Furthermore, the pore structure modifier is wood chips; preferably, the particle size of the wood chips is 40-100 meshes.
[0029] Furthermore, the ratio of the mass of sawdust to the total mass of the titanium source, silicon source and aluminum source is 1:(1.5-3.1), and the sawdust is at least one of pine sawdust, poplar sawdust, fir sawdust and birch sawdust.
[0030] Furthermore, taking the total mass fraction of the raw materials for preparing the porous titanium-based denitration catalyst as 100%, the mass fraction of the binder is 1%-12%, and the mass fraction of the lubricant is 0.5%-12%.
[0031] Furthermore, the drying conditions are: 30-100°C, 1-36h; the calcination conditions are: 200-1000°C, 1-15h.
[0032] According to the third aspect of the present invention, there is provided a use of the porous titanium-based denitration catalyst according to the first aspect of the present invention or the porous titanium-based denitration catalyst prepared by the preparation method of the second aspect of the present invention in catalytic reduction of nitrogen oxides.
[0033] By applying the technical solution of the present invention, the components of the porous titanium-based denitrification catalyst are selected, and its mechanical strength is improved by adding silicon oxide and aluminum oxide. By designing its particle size and pore size, the internal diffusion performance of the porous titanium-based catalyst can be improved, the utilization rate of the catalyst can be increased, and its catalytic reduction performance of nitrogen oxides can be enhanced. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 is a cross-sectional view of the porous titanium-based denitration catalyst in Example 1;
[0035] Figure 2 It is a cross-sectional view of the titanium-based denitration catalyst in Comparative Example 1;
[0036] Figure 3 is a relationship diagram between the logarithmic differential volume and pore size of the porous titanium-based denitration catalyst in Example 1;
[0037] Figure 4 is a relationship diagram between the logarithmic differential volume and pore size of the titanium-based denitration catalyst in Comparative Example 1;
[0038] Figure 5 For Example 1 and Comparative Example 1 at 10000h -1 Comparison of SCR activity curves at airspeed;
[0039] Figure 6 It is a comparison diagram of the SCR activity curves of Example 1 and Comparative Example 1 at different space velocities. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0041] As described in the background of the present invention, the existing technology has the problem that the internal diffusion performance of the titanium-based denitration catalyst is poor, resulting in low catalyst utilization and low nitrogen oxide conversion rate.
[0042] In order to solve the above technical problems, in a typical embodiment of the present invention, a porous titanium-based denitration catalyst is provided, which includes 30-65 parts of a carrier and 0.5-5 parts of an active component loaded thereon; wherein the carrier includes titanium dioxide, silicon oxide and aluminum oxide, and the active component includes at least one of vanadium pentoxide, tungsten oxide, manganese oxide, cerium oxide, copper oxide and iron oxide; the pore size of the porous titanium-based denitration catalyst is 2-3 μm.
[0043] Titanium-based denitrification catalyst is a catalyst that uses titanium-based materials as carriers and loads active components on its surface to achieve denitrification reaction. The active components loaded on its surface can catalyze the selective catalytic reduction reaction of ammonia, converting nitrogen oxides into nitrogen and water vapor, thereby achieving denitrification; it is widely used in coal-fired power plants, industrial boilers, and automobile exhaust treatment, helping to reduce emissions of atmospheric pollutants and protect the environment and human health.
[0044] The present invention can reduce the influence of internal diffusion on the catalytic performance of the catalyst and improve its catalytic reduction performance of nitrogen oxides by designing the pore size of the titanium-based denitration catalyst; at the same time, the present invention can increase the strength of the catalyst and give full play to the performance of the catalyst by adding silicon oxide and aluminum oxide to the titanium-based carrier. The titanium-based denitration catalyst of the present invention has high efficiency in catalytic reduction of nitrogen oxides, can play a good catalytic role when used in a small amount, and has low cost.
[0045] In a preferred embodiment of the present invention, the average particle size of the porous titanium-based denitration catalyst is 2-4 mm.
[0046] Under the above conditions, the internal efficiency factor of the porous titanium-based denitrification catalyst is high, and NO x The conversion rate can reach 100%.
[0047] In a preferred embodiment of the present invention, in the carrier, the mass ratio of titanium dioxide, silicon oxide and aluminum oxide is (250-270): (6-12): (6-12).
[0048] Titanium dioxide will undergo a reversible sulfuric acid acidification reaction under the conditions of NH3-SCR reaction. The stability of sulfate on the surface of titanium dioxide is weaker than that of other oxides, so titanium-based catalysts have better resistance to sulfur poisoning. In addition, the active ingredients have good dispersion on titanium dioxide. For example, vanadium pentoxide can produce isolated vanadium-based centers and polymerized polyvanadates. Therefore, loading vanadium pentoxide on titanium dioxide can obtain a very active catalyst. At the same time, it has good chemical stability and activity. Adding an appropriate amount of silicon oxide can effectively improve the compressive strength and wear resistance of titanium dioxide, making it more durable in application. Alumina has good high temperature resistance and corrosion resistance, which can significantly improve the thermal stability and chemical stability of titanium dioxide, making it perform better in high temperature and corrosive environments. By making the above-mentioned optimization of the components of the carrier, it is more practical.
[0049] In another typical embodiment of the present invention, a method for preparing a porous titanium-based denitration catalyst according to the first aspect of the present invention is provided, comprising the following steps:
[0050] dissolving the active ingredient in water to obtain an active agent;
[0051] Mixing a pore structure modifier, a titanium source, a silicon source, an aluminum source, and a binder to obtain a first mixture;
[0052] adding an active agent to the first mixture to obtain a second mixture;
[0053] mixing the second mixture and a lubricant to obtain a third mixture;
[0054] The third mixture is dried and calcined to obtain a porous titanium-based denitration catalyst.
[0055] By adding a pore structure modifier, a large number of pores can be formed during the calcination process, thereby increasing the internal diffusion performance of the catalyst and improving the performance of the titanium-based denitrification catalyst in catalytic reduction of nitrogen oxides.
[0056] Typically but not limiting, oxalic acid or the like may be added during the preparation of the active agent to promote the dissolution of the active ingredient and form a uniform active agent.
[0057] Typically, but not limiting, the lubricant is first dispersed in water, which is then mixed with the second mixture to obtain a third mixture; additional water may be added and the mixing time increased to make the composition of the third mixture more uniform.
[0058] In a preferred embodiment of the present invention, the active ingredient is at least one of a vanadium source, a tungsten source, a manganese source, a cerium source, a copper source, and an iron source.
[0059] The above ingredients are all commonly used active ingredients in titanium-based deNOx catalysts, which can effectively promote the selective catalytic reduction reaction of ammonia.
[0060] In a preferred embodiment of the present invention, the pore structure modifier is at least one of plastic, rosin and sawdust.
[0061] As there are many plastic products now, a large amount of waste plastic will be generated. The low price and secondary utilization of plastic conform to the concept of conservation and environmental protection. Rosin and sawdust as pore structure modifiers are natural and environmentally friendly, do not pollute the environment, do not produce harmful gases, and have good pore-forming properties.
[0062] In a preferred embodiment of the present invention, the pore structure modifier is wood chips, and the particle size of the wood chips is 40-100 mesh; and / or the ratio of the mass of the wood chips to the total mass of the titanium source, the silicon source, and the aluminum source is 1: (1.5-3.1).
[0063] It is easier to create large pores by using sawdust as a pore structure modifier. The particle size is controlled to 40-100 mesh because the raw material is easier to obtain. The above-mentioned limitation on its dosage can further improve the internal diffusion performance of the porous titanium-based denitrification catalyst. At the same time, the catalyst also has certain strength and stability.
[0064] Typically, but not limiting, the wood chips are at least one of pine wood chips, poplar wood chips, fir wood chips, and birch wood chips.
[0065] Typically, but not limiting, the binder is at least one of hydroxypropyl cellulose, hydroxypropyl methylcellulose, hydroxymethyl cellulose, and polyethylene oxide; and / or the lubricant is at least one of glycerol, palm oil, and paraffin oil.
[0066] Typically, but not limiting, the titanium source is at least one of tetrabutyl titanate, titanyl sulfate, and titanium oxide; and / or the aluminum source is at least one of aluminum chloride and aluminum oxide; and / or the silicon source is at least one of silicon chloride and silicon oxide; and / or the vanadium source is at least one of ammonium metavanadate and vanadium pentoxide; and / or the tungsten source is at least one of ammonium metatungstate and tungsten oxide; and / or the manganese source is at least one of manganese nitrate, manganese sulfate, potassium permanganate, and manganese oxide; and / or the cerium source is at least one of cerium nitrate and cerium oxide; and / or the copper source is at least one of copper nitrate, copper sulfate, and copper oxide; and / or the iron source is at least one of ferric nitrate, ferrous sulfate, and ferric oxide.
[0067] In a preferred embodiment of the present invention, based on the total mass fraction of the raw materials for preparing the porous titanium-based denitration catalyst being 100%, the mass fraction of the binder is 1%-12%, and the mass fraction of the lubricant is 0.5%-12%.
[0068] Adding an appropriate amount of binder can improve the stability and durability of the catalyst, and can also help form uniform catalyst particles, promote the diffusion and contact of the reactants, and thus improve the efficiency and activity of the catalyst. Adding an appropriate amount of lubricant can reduce friction resistance, make the processing smoother, and prepare a catalyst with uniform composition.
[0069] In a preferred embodiment of the present invention, the drying conditions are: 30-100° C., 1-36 h; the calcination conditions are: 200-1000° C., 1-15 h, 0.5-10° C. / min.
[0070] The porous titanium-based denitration catalyst prepared under the above conditions has good performance in catalyzing the selective reduction of nitrogen oxides by ammonia.
[0071] In another typical embodiment of the present invention, there is provided a porous titanium-based denitration catalyst according to the above embodiment or a porous titanium-based denitration catalyst prepared by the preparation method according to the above embodiment for use in catalytic reduction of nitrogen oxides.
[0072] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0073] Performance Testing
[0074] 1) Surface morphology: The surface morphology of the titanium-based denitration catalysts in the examples and comparative examples was observed using an optical microscope;
[0075] 2) Average pore size: The average pore size is directly measured using a mercury intrusion instrument;
[0076] 3) Internal efficiency factor: calculated by the following formula:
[0077] k=Aexp(-E / RT)
[0078] Where k is the reaction rate constant, A is the frequency factor, and E is the activation energy;
[0079] ∈ p =1-ρ f / ρ t
[0080] Among them, ∈ p is the porosity, ρ f is the pseudo density, ρ t is the true density.
[0081] D k =9700r(T / M) 1 / 2
[0082] Among them, D k is the Knudsen diffusion coefficient, and r is the average pore size.
[0083] D e =∈ p D k / τ
[0084] Among them, D e is the effective diffusion coefficient, ∈ p is the porosity, τ is the tortuosity factor, which takes a value of 4.
[0085]
[0086] in, is the Ziehler modulus, R is the particle radius (the radius of the circumscribed circle of the cloverleaf mold), k is the reaction rate constant, and D e is the effective diffusion coefficient.
[0087]
[0088] Among them, η 内 is the internal efficiency factor, is the Ziller modulus.
[0089] 4) Denitration performance: The denitration catalysts prepared in the examples and comparative examples were placed in a quartz tube and the denitration performance was tested by programmed temperature rise in a fixed bed reactor. The simulated gas composition was: NO (1000ppm), NH3 (1000ppm) and O2 (3%), with N2 as the carrier gas; the total flow rate of the raw gas was controlled to be 800mL / min; the catalyst dosage was 4.8mL; NO x The conversion rate was calculated using the following formula: x Conversion rate (%) = (NO x入 -NO x出 ) / NOx入 .
[0090] 5) Mechanical strength: The crushing strength of 8 samples of uniform size was tested using a particle strength tester, and the average value was taken as the final result.
[0091] Example 1
[0092] An embodiment of the porous titanium-based denitration catalyst of the present invention, the preparation method of this embodiment comprises the following steps:
[0093] Weigh 12.2 g of ammonium metavanadate and 28.8 g of oxalic acid respectively and dissolve them in 20 mL of water. Stir at 80°C for 10 min until the solution turns dark blue to obtain an active reagent.
[0094] Weigh 260.85g titanium dioxide, 12g silicon dioxide, 6g aluminum oxide, 150g pine sawdust (particle size 40-100 mesh), and 24g hydroxypropyl cellulose respectively, pour into an extruder and knead for 30 minutes;
[0095] Pour the active agent into the above extruder and knead for 10 minutes;
[0096] Dissolve 9 g of glycerol in 10 mL of water, add dropwise into the extruder, and knead for 10 min;
[0097] Then add 30 mL of water dropwise and knead for 30 min;
[0098] Install a cloverleaf die with a diameter of 5 mm to extrude the material;
[0099] The extruded samples were placed in an oven at 60 °C and dried for 12 h;
[0100] The dried sample was placed in a muffle furnace and calcined in air at 550° C. for 4 h (with a programmed heating rate of 2° C. / min) to obtain a porous titanium-based denitration catalyst.
[0101] Embodiment 2-4
[0102] Example 2-4 is a porous titanium-based denitration catalyst, and the difference between Example 2-6 and Example 1 is only that the size of the mold used in the preparation process is different;
[0103] The diameter of the clover leaf mold used in Example 2 was 2 mm;
[0104] The diameter of the clover leaf mold used in Example 3 was 3 mm;
[0105] The diameter of the clover leaf mold used in Example 4 was 4 mm.
[0106] Embodiment 5-7
[0107] Embodiment 5-7 is a porous titanium-based denitration catalyst. The difference between Embodiment 5-7 and Embodiment 1 is only that the amount of pine wood chips added is different;
[0108] The mass of pine wood chips in Example 5 is 90 g;
[0109] The mass of pine wood chips in Example 6 is 120 g;
[0110] The mass of pine wood chips in Example 7 is 180 g.
[0111] Examples 8-12
[0112] Examples 8-12 are porous titanium-based denitration catalysts. The only difference between Examples 8-12 and Example 1 is that the mesh size range of the added pine wood chips is smaller;
[0113] In Example 8, the mesh size of the pine wood chips is 20-30 mesh;
[0114] In Example 9, the mesh size of the pine wood chips is 30-40 mesh;
[0115] In Example 10, the mesh size of the pine wood chips is 40-50 mesh;
[0116] In Example 11, the mesh size of the pine wood chips is 50-60 mesh;
[0117] The mesh size of the pine wood chips in Example 12 is 60-70 mesh.
[0118] Examples 13-14
[0119] Embodiments 13-14 are porous titanium-based denitration catalysts. The only difference between Embodiments 13-14 and Embodiment 1 is that the amounts of ammonium metavanadate, oxalic acid, and water used in the preparation process are different;
[0120] In Example 13, the amount of ammonium metavanadate used is 6.1 g, the amount of oxalic acid used is 14.4 g, and the amount of water used is 10 mL;
[0121] In Example 14, the amount of ammonium metavanadate used is 18.3 g, the amount of oxalic acid used is 43.2 g, and the amount of water used is 30 mL.
[0122] Examples 15-16
[0123] Examples 15-16 are porous titanium-based denitration catalysts. The only difference between Examples 15-16 and Example 1 is that the qualities of hydroxypropyl cellulose and glycerol are different;
[0124] In Example 15, the mass of hydroxypropyl cellulose is 19.2 g, and the mass of glycerol is 7.2 g;
[0125] In Example 16, the mass of hydroxypropyl cellulose is 28.8 g, and the mass of glycerol is 10.8 g;
[0126] Examples 17-20
[0127] Examples 17-20 are examples of the porous titanium-based denitration catalyst of the present invention. The only difference between Examples 17-20 and Example 1 is that the masses of the three components of the carrier are different;
[0128] In Example 17, the mass of titanium dioxide is 278.85 g, the mass of silicon dioxide is 0 g, and the mass of aluminum oxide is 0 g;
[0129] In Example 18, the mass of titanium dioxide is 260.85 g, the mass of silicon dioxide is 6 g, and the mass of aluminum oxide is 12 g;
[0130] In Example 19, the mass of titanium dioxide is 266.85 g, the mass of silicon dioxide is 6 g, and the mass of aluminum oxide is 6 g;
[0131] In Example 20, the mass of titanium dioxide is 254.85 g, the mass of silicon dioxide is 12 g, and the mass of aluminum oxide is 12 g.
[0132] Comparative Example 1
[0133] Comparative Example 1 is a titanium-based denitration catalyst, which differs from Example 1 only in that no pine wood chips are added and the added amount of hydroxypropyl cellulose is 9 g.
[0134] Figure 1-2 They are cross-sectional views of the titanium-based denitration catalysts in Example 1 and Comparative Example 1, respectively. It can be seen from the figures that the titanium-based denitration catalyst in Example 1 has a pore structure with large pores visible to the naked eye. Figure 3-4 They are the pore size distribution diagrams of the titanium-based denitration catalysts in Example 1 and Comparative Example 1, respectively. It can be seen from the diagram that after pore expansion, the average pore size of the catalyst increases from about 20 nm to about 2 μm, and the number of macroporous structures increases significantly.
[0135] Table 1 shows the calculation results of the internal efficiency factors of the titanium-based denitration catalysts in Example 1 and Comparative Example 1 at different temperatures.
[0136] Table 1
[0137] project 200℃ 250℃ 300℃ 350℃ 400℃ Example 1 0.974 0.917 0.811 0.672 0.536 Comparative Example 1 0.307 0.176 0.109 0.072 0.051
[0138] It can be seen from Table 1 that the internal efficiency factors of the titanium-based denitration catalyst in Example 1 at 200-400°C are all higher than 0.5, and are significantly higher than those in Comparative Example 1. The results show that the present invention improves the internal diffusion performance of the titanium-based denitration catalyst by improving the structure of the titanium-based denitration catalyst and introducing macropores, which helps to improve the utilization rate of the catalyst and improve its catalytic reduction performance of nitrogen oxides.
[0139] Table 2 shows the calculation results of the internal efficiency factor of the titanium-based denitration catalyst at 300°C in the examples and comparative examples and the NO x The conversion rate test results, the test conditions are: 8000h -1 Space velocity, 300°C.
[0140] Table 2
[0141] project Internal efficiency factor NOx conversion rate (%) Example 1 0.811 99.3 Example 2 0.961 100 Example 3 0.918 100 Example 4 0.866 100 Comparative Example 1 0.109 91.4
[0142] From the above test results, it can be seen that the internal efficiency factor of the titanium-based denitration catalyst in the embodiment is significantly higher than that in the comparative example, and when the average particle size is 5 mm, its internal efficiency factor can reach 0.811, which has good internal diffusion performance. Among them, when the average particle size of the porous titanium-based denitration catalyst is 2 mm, its internal efficiency factor can reach 0.95, and the internal diffusion performance is excellent.
[0143] Comparing the test results of Example 1 and Comparative Example 1 in Table 2, it can be found that NO x The removal rate was increased by almost 10%.
[0144] Table 3 shows the strength test results of titanium-based denitration catalysts and NO in the examples and comparative examples. x The conversion rate test results, the test conditions are: 30000h -1 Space velocity, 200°C.
[0145] Table 3
[0146] project Strength (N / cm) <![CDATA[NO x Conversion rate (%)]]> Example 1 45.20 86.4 Example 5 73.00 84.1 Example 6 61.66 81.5 Example 7 30.29 88.0 Comparative Example 1 200.00 74.6
[0147] It can be seen from Table 3 that the strength of the titanium-based denitrification catalyst decreases after pore formation, but at high space velocity (30000h -1 ), the catalytic performance of porous titanium-based denitrification catalyst at low temperature (200°C) is significantly better. The more sawdust is added, the more the strength decreases, but the cost also decreases. Therefore, the best comprehensive performance can be obtained by controlling the ratio of the mass of sawdust to the total mass of titanium source, aluminum source, and silicon source during the preparation process to 1: (1.5-3.1).
[0148] Table 4 shows the titanium-based denitration catalyst NO in the examples. x The conversion rate test results, the test conditions are: 16000h -1 Space velocity, 300°C.
[0149] Table 4
[0150] project <![CDATA[NO x Conversion rate (%)]]> Example 1 96.7 Example 8 95.4 Example 9 95.3 Example 10 94.7 Embodiment 11 95.0 Example 12 96.8
[0151] From Table 4, we can see that the particle size of sawdust has an important influence on NO x The removal rate has little effect. Considering the difficulty of obtaining raw materials, 40-100 mesh sawdust is selected for pore making.
[0152] Table 5 shows the titanium-based denitration catalyst NO in the examples. x The conversion rate test results, the test conditions are: 8000h -1 Space velocity, 300°C.
[0153] Table 5
[0154] project <![CDATA[NO x Conversion rate (%)]]> Example 1 99.3 Embodiment 13 90 Embodiment 14 100
[0155] It can be seen from Table 5 that the more ammonium metavanadate is used, the better the catalytic performance of the porous titanium-based denitrification catalyst is. When the amount of ammonium metavanadate is 12.2 g, under certain test conditions, NO x The conversion rate can reach 99%. Considering the cost issue, the amount of ammonium metavanadate is no longer increased on this basis.
[0156] Table 6 shows the titanium-based denitration catalyst NO in the examples. x The conversion rate test results, the test conditions are: 8000h -1 Space velocity, 300°C.
[0157] Table 6
[0158]
[0159]
[0160] As shown in Table 6, the amount of hydroxypropyl cellulose as a binder and glycerol as a lubricant has an effect on the NO x The removal rate was not significantly affected. In order to ensure smooth extrusion of the catalyst during the molding process, it was more appropriate to add 24g of hydroxypropyl cellulose and 9g of glycerol. The dosage can be appropriately adjusted according to the specific molding phenomenon.
[0161] Table 7 shows the strength test results of titanium-based denitration catalysts and NO in the examples and comparative examples. x The conversion rate test results, the test conditions are: 30000h -1 Space velocity, 200°C.
[0162] Table 7
[0163] project Strength (N / cm) <![CDATA[NO x Conversion rate (%)]]> Example 1 45.20 99.3 Embodiment 17 20.70 100 Embodiment 18 47.64 98.5 Embodiment 19 40.52 100 Embodiment 20 50.40 97.5
[0164] It can be seen from Table 7 that adding appropriate amounts of aluminum oxide and silicon oxide has a significant effect on NO x The removal rate has little effect. Compared with the porous titanium-based denitrification catalyst without the addition of alumina and silica, the strength of the catalyst is significantly improved after the addition of alumina and silica. In addition, the experiment found that when the mass ratio of titanium dioxide, silica and aluminum oxide in the carrier is (250-270): (6-12): (6-12), its strength is higher and it has good catalytic performance.
[0165] Figure 5 For Example 1 and Comparative Example 1 at 10000h -1 The SCR activity curve comparison at air velocity is as follows: -1 The catalytic efficiency is kept as high as 80%-100% at a high space velocity and in a wide temperature window of 200-400°C.
[0166] Figure 6 For different airspeeds (5000-50000h -1 ) is a comparison diagram of the SCR activity curves of Example 1 and Comparative Example 1. It can be seen from the figure that under all space velocity conditions, the catalytic performance of the titanium-based denitration catalyst in Example 1 is significantly better than that of Comparative Example 1, which further proves that the present invention effectively improves the performance of the titanium-based denitration catalyst in catalyzing the selective reduction of nitrogen oxides with ammonia by improving the pore structure of the titanium-based denitration catalyst.
[0167] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A porous titanium-based denitrification catalyst, It is characterized in that It comprises 30-65 parts of a carrier and 0.5-5 parts of an active component loaded thereon; the carrier comprises titanium dioxide, silicon oxide and aluminum oxide, the active component comprises at least one of vanadium pentoxide, tungsten oxide, manganese oxide, cerium oxide, copper oxide and iron oxide; the pore size of the porous titanium-based denitration catalyst is 2-3 μm.
2. The porous titanium-based denitration catalyst according to claim 1, It is characterized in that In the carrier, the mass ratio of the titanium dioxide, the silicon oxide and the aluminum oxide is (250-270):(6-12):(6-12).
3. A method for preparing a porous titanium-based denitration catalyst according to claim 1 or 2, It is characterized in that The steps include: dissolving the active ingredient in water to obtain an active agent; Mixing a pore structure modifier, a titanium source, a silicon source, an aluminum source, and a binder to obtain a first mixture; adding the active agent to the first mixture to obtain a second mixture; mixing the second mixture with a lubricant to obtain a third mixture; The third mixture is dried and calcined to obtain the porous titanium-based denitration catalyst.
4. The method for preparing the porous titanium-based denitration catalyst according to claim 3, It is characterized in that The active ingredient is at least one of a vanadium source, a tungsten source, a manganese source, a cerium source, a copper source, and an iron source; and / or The pore structure modifier is at least one of plastic, rosin, and sawdust; and / or The binder is at least one of hydroxypropyl cellulose, hydroxypropyl methyl cellulose, hydroxymethyl cellulose and polyethylene oxide; and / or The lubricant is at least one of glycerol, palm oil and paraffin oil.
5. The method for preparing the porous titanium-based denitration catalyst according to claim 4, It is characterized in that The titanium source is at least one of tetrabutyl titanate, titanyl sulfate and titanium oxide; and / or The aluminum source is at least one of aluminum chloride and aluminum oxide; and / or The silicon source is at least one of silicon chloride and silicon oxide; and / or The vanadium source is at least one of ammonium metavanadate and vanadium pentoxide; and / or The tungsten source is at least one of ammonium metatungstate and tungsten oxide; and / or The manganese source is at least one of manganese nitrate, manganese sulfate, potassium permanganate and manganese oxide; and / or The cerium source is at least one of cerium nitrate and cerium oxide; and / or The copper source is at least one of copper nitrate, copper sulfate and copper oxide; and / or The iron source is at least one of ferric nitrate, ferrous sulfate and ferric oxide; and / or The pore structure modifier is wood chips.
6. The method for preparing the porous titanium-based denitration catalyst according to claim 5, It is characterized in that The particle size of the wood chips is 40-100 meshes.
7. The method for preparing the porous titanium-based denitration catalyst according to claim 5, It is characterized in that The ratio of the mass of the sawdust to the total mass of the titanium source, the aluminum source and the silicon source is 1:(1.5-3.1); and / or the sawdust is at least one of pine sawdust, poplar sawdust, fir sawdust and birch sawdust.
8. The method for preparing a porous titanium-based denitration catalyst according to any one of claims 3 to 7, It is characterized in that Taking the total mass fraction of the raw materials for preparing the porous titanium-based denitration catalyst as 100%, the mass fraction of the binder is 1%-12%, and the mass fraction of the lubricant is 0.5%-12%.
9. The method for preparing the porous titanium-based denitration catalyst according to claim 8, It is characterized in that The drying conditions are: 30-100° C., 1-36 h; the calcination conditions are: 200-1000° C., 1-15 h.
10. Use of the porous titanium-based denitration catalyst according to claim 1 or 2 or the porous titanium-based denitration catalyst prepared by the preparation method according to any one of claims 3 to 9 in catalytic reduction of nitrogen oxides.
Citation Information
Patent Citations
High-water absorption flue gas denitration honeycomb ceramic support and preparation method thereof
CN102600910A
Polynary metallic oxide denitration catalyst
CN103877990A
Cerium oxide-based loaded smoke denitrification catalyst and preparation method thereof
CN104014324A
Strip-shaped clover denitration catalyst and preparation method thereof
CN115845834A
Regenerated denitration catalyst and method for manufacturing the same, and denitration apparatus
US20220126280A1
Cited By
Low-temperature sulfur-resistant denitration catalyst for refining flue gas and preparation method thereof
CN122806525A