High-activity catalyst for three-way catalyst and preparation method of high-activity catalyst

By using the combination of cordierite ceramic honeycomb support and γ-Al2O3@Ce0.5Zr0.5O2/La2O3-CeO2 composite solid and precious metals Pt, Pd, and Rh, the problem of inactivation of the three-way catalyst at high temperature is solved, and high Improved activity and durability.

CN119016045APending Publication Date: 2024-11-26山东莲奥汽车科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410986693.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing three-way catalysts are prone to sintering metal particles, blockage of carrier channels or collapse of components under high temperature conditions, resulting in catalyst deactivation and reduction of conversion, affecting durability.

Method used

Cordierite ceramic honeycomb support and γ-Al2O3@Ce0.5Zr0.5O2/La2O3-CeO2 composite solid was used as catalyst support, and noble metals Pt, Pd, and Rh were supported by impregnation method, combined with high-temperature calcination and reduction treatment to form a highly active catalyst.

Benefits of technology

The activity and high temperature stability of the catalyst are improved, the highly dispersed state of precious metals is maintained, the durability of the catalyst is extended and the catalytic efficiency is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-activity catalyst for a three-way catalyst and a preparation method of the high-activity catalyst, and belongs to the technical field of environment-friendly catalysis. The high-activity catalyst for the three-way catalyst is prepared from a cordierite ceramic honeycomb carrier, a composite solid gamma-Al2O3 (at) Ce0. 5Zr0. 5O2 / La2O3-CeO2 and noble metals Pt, Pd and Rh. The cordierite ceramic honeycomb carrier is small in airflow resistance, high in mechanical strength, resistant to high temperature, high in catalytic conversion rate and low in price; gamma-Al2O3 in the composite solid has very strong adsorption capacity and a very large specific surface area, and Ce0. 5Zr0. 5O2, La2O3 and CeO2 in the composite solid have a synergistic effect, so that not only can the overall activity and high-temperature stability of the catalyst be improved, but also the highly dispersed state of noble metals Pt, Pd and Rh can be stabilized; therefore, the catalyst provided by the invention is not easy to inactivate due to sintering, and has excellent catalytic durability and high catalytic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of environmental protection catalysis, and in particular, relates to a high-activity catalyst for a three-way catalytic converter and a preparation method thereof. Background Art

[0002] The three-way catalytic converter is the most important external purification device installed in the automobile exhaust system. It can remove CO, HC and NO from the exhaust gas of the automobile. x Harmful gases such as CO, HC and NO are converted into harmless carbon dioxide, water and nitrogen through oxidation and reduction. When the high-temperature automobile exhaust passes through the purification device, the purifier in the three-way catalytic converter will enhance the removal of CO, HC and NO. x The activity of the three gases prompts them to undergo certain oxidation-reduction chemical reactions, among which CO is oxidized into colorless, non-toxic carbon dioxide gas at high temperatures; HC compounds are oxidized into water and carbon dioxide at high temperatures; NO x Reduced to nitrogen and oxygen. The three harmful gases become harmless gases, purifying the exhaust gas of the car.

[0003] The catalyst used in the three-way catalytic converter mainly includes a carrier and a precious metal loaded on the carrier. The operating temperature of the three-way catalytic converter is very high, up to 800°C, and even higher under equivalent ratio combustion conditions. Excessive temperature will cause thermal aging of the catalyst, such as sintering of metal particles, clogging of carrier channels, or collapse of carrier components, which will cause problems such as catalyst deactivation and decreased conversion rate, seriously affecting the durability of the catalyst. Therefore, it is urgent to design and prepare a high-activity catalyst for the three-way catalytic converter. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a high-activity catalyst for a three-way catalytic converter and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a high-activity catalyst for a three-way catalytic converter comprises the following steps:

[0007] The composite solid is mixed with the carrier, and then the precious metal is loaded by the impregnation method. After the loading is completed, it is dried, calcined and reduced to obtain a high-activity catalyst for a three-way catalytic converter.

[0008] Furthermore, the carrier is a cordierite ceramic honeycomb carrier.

[0009] The cordierite ceramic honeycomb carrier has small airflow resistance, high mechanical strength, impact resistance, high temperature resistance, high catalytic conversion rate and low price.

[0010] Furthermore, the composite solid is prepared by the following steps:

[0011] (1) Powdered active γ-Al 2 O 3 、Ce(NO 3 ) 3 6H 2 O and Zr(NO 3 ) 4 ·5H 2 O was ultrasonically dispersed and dissolved in ethanol, and citric acid ethanol solution was added dropwise while stirring, and stirred at room temperature for 24 h to obtain an impregnation solution;

[0012] (2) Add La(NO) to the impregnation solution obtained in step (1) 3 ) 3 6H 2 O, stirred at room temperature for 12 h, and finally, Ce(NO 3 ) 3 6H 2 O, stirred at room temperature for 12 h, evaporated to dryness in a 60 ° C water bath, dried in an oven at 80 ° C for 12 h, then calcined at high temperature under nitrogen protection, and finally cooled naturally to room temperature to obtain γ-Al 2 O 3 @Ce 0.5 Zr 0.5 O 2 / La 2 O 3 -CeO 2 , that is, a composite solid.

[0013] Furthermore, the concentration of the citric acid ethanol solution in step (1) is 0.013 mol / L.

[0014] Furthermore, in step (1), γ-Al 2 O 3 、Ce(NO 3 ) 3 6H 2 O、Zr(NO 3 ) 4 ·5H 2 The dosage ratio of O and citric acid ethanol solution is 10g:0.07g:0.05g:50mL.

[0015] Furthermore, in step (2), La(NO 3 ) 3 6H 2 O and Ce(NO 3 ) 3 6H 2 The dosage ratio of O is 0.2g:2g.

[0016] Furthermore, in the step (2), the heating rate during calcination is 2-10°C / min, the calcination temperature is 400-1000°C, and the calcination time is 2-4h.

[0017] Furthermore, in the step (2), the heating rate during calcination is 2.5°C / min, the calcination temperature is 800°C, and the calcination time is 3h.

[0018] The specific surface area of ​​cordierite ceramic honeycomb carrier is greatly reduced after high temperature calcination, which is not conducive to loading active substances. 2 O 3 It has strong adsorption capacity and large specific surface area, and the combination of the two can provide a good catalytic reaction environment.

[0019] CeO 2 It has the function of storing and releasing oxygen, which can improve the efficiency of the catalyst, accelerate the water gas migration and steam reforming reaction in the catalytic reaction, and reduce the content of CO and HC through their oxidation under reducing conditions. 2 O 3 and Ce 0.5 Zr 0.5 O 2 It has good thermal stabilization effect on highly dispersed precious metals and carriers on the surface.

[0020] Furthermore, the precious metal is a compound of Pt, Pd and Rh in a mass ratio of 2:(3-5):1.

[0021] Pt has a stronger ability to resist poisoning than Pd and Rh. In the catalyst, Rh is a decisive component, especially under rich and stoichiometric air-fuel ratios. x and CO purification, Rh can promote NO x and CO purification performance; Pt and Pd can promote the oxidation of HC and CO, making them emit pollution-free H 2 O、CO 2 .

[0022] The invention also discloses a high-activity catalyst for a three-way catalytic converter, which is prepared according to the above-mentioned preparation method of the high-activity catalyst for a three-way catalytic converter.

[0023] The beneficial effects of the present invention are as follows: the cordierite ceramic honeycomb carrier of the present invention has low airflow resistance, high mechanical strength, high temperature resistance, high catalytic conversion rate and low price; and the γ-Al in the composite solid 2 O 3 It has strong adsorption capacity and large specific surface area. Ce in composite solid 0.5 Zr 0.5 O 2 ,La 2 O3 and CeO 2 The synergistic effect of the three can not only improve the overall activity and high-temperature stability of the catalyst, but also stabilize the highly dispersed state of the precious metals Pt, Pd, and Rh; therefore, the catalyst of the present invention is not prone to sintering and deactivation, has excellent catalytic durability and high catalytic efficiency. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] The preparation of the composite solid is carried out in the following steps:

[0027] (1) 10 g of powdered active γ-Al 2 O 3 and 0.07 g of Ce(NO 3 ) 3 6H 2 O and 0.05 g Zr(NO 3 ) 4 ·5H 2 O was ultrasonically dispersed and dissolved in 200 mL of ethanol, and 50 mL of 0.013 mol / L citric acid ethanol solution was added dropwise at room temperature with stirring, and stirred at room temperature for 24 h to obtain an impregnation solution;

[0028] (2) Add 0.2 g of La(NO) to the impregnation solution obtained in step (1). 3 ) 3 6H 2 O, stirred at room temperature for 12 h, and finally, 2 g of Ce(NO 3 ) 3 6H 2 O, stirred at room temperature for 12 h, evaporated to dryness in a 60 ° C water bath, dried in an oven at 80 ° C for 12 h, and then calcined at high temperature under nitrogen protection, with a heating rate of 2.5 ° C / min, a calcination temperature of 800 ° C, a calcination time of 3 h, and then cooled to room temperature to obtain a composite solid.

[0029] Example 2

[0030] The preparation of the composite solid is carried out in the following steps:

[0031] (1) 10 g of powdered active γ-Al 2 O 3and 0.07 g of Ce(NO 3 ) 3 6H 2 O and 0.05 g Zr(NO 3 ) 4 ·5H 2 O was ultrasonically dispersed and dissolved in 200 mL of ethanol, and 50 mL of 0.013 mol / L citric acid ethanol solution was added dropwise at room temperature with stirring, and stirred at room temperature for 24 h to obtain an impregnation solution;

[0032] (2) Add 0.2 g of La(NO) to the impregnation solution obtained in step (1). 3 ) 3 6H 2 O, stirred at room temperature for 12 h, and finally, 2 g of Ce(NO 3 ) 3 6H 2 O, stirred at room temperature for 12 h, evaporated to dryness in a 60 ° C water bath, dried in an oven at 80 ° C for 12 h, and then calcined at high temperature under nitrogen protection, with a heating rate of 2 ° C / min, a calcination temperature of 400 ° C, and a calcination time of 2 h, and then cooled to room temperature to obtain a composite solid.

[0033] Example 3

[0034] The preparation of the composite solid is carried out in the following steps:

[0035] (1) 10 g of powdered active γ-Al 2 O 3 and 0.07 g of Ce(NO 3 ) 3 6H 2 O and 0.05 g Zr(NO 3 ) 4 ·5H 2 O was ultrasonically dispersed and dissolved in 200 mL of ethanol, and 50 mL of 0.013 mol / L citric acid ethanol solution was added dropwise at room temperature with stirring, and stirred at room temperature for 24 h to obtain an impregnation solution;

[0036] (2) Add 0.2 g of La(NO) to the impregnation solution obtained in step (1). 3 ) 3 6H 2 O, stirred at room temperature for 12 h, and finally, 2 g of Ce(NO 3 ) 3 6H 2 O, stirred at room temperature for 12 h, evaporated to dryness in a 60 ° C water bath, dried in an oven at 80 ° C for 12 h, and then calcined at high temperature under nitrogen protection, with a heating rate of 10 ° C / min, a calcination temperature of 1000 ° C, a calcination time of 4 h, and then cooled to room temperature to obtain a composite solid.

[0037] Example 4

[0038] The catalyst is prepared in the following specific steps:

[0039] The composite solid prepared in Example 1 is added to deionized water, stirred thoroughly until mixed evenly, then a cordierite ceramic honeycomb carrier is added, and ultrasonic immersion is performed at room temperature for 12 hours. After immersion, it is dried at 80°C for 12 hours. After repeating 3 times, the composite solid and the cordierite ceramic honeycomb carrier are mixed. The mass of the composite solid is 15% of the mass of the cordierite ceramic honeycomb carrier. Then, the precious metal Pd is first loaded by the impregnation method, and then the precious metal Rh is loaded. Finally, the precious metal Pt is loaded. The mass ratio of Pt, Pd, and Rh is 2:3:1. After loading, it is dried, calcined, and reduced to obtain a high-activity catalyst for a three-way catalytic converter.

[0040] Example 5

[0041] The catalyst is prepared in the following specific steps:

[0042] The composite solid prepared in Example 2 is added to deionized water, stirred thoroughly until mixed evenly, then a cordierite ceramic honeycomb carrier is added, and ultrasonic immersion is performed at room temperature for 12 hours. After immersion, it is dried at 80°C for 12 hours. After repeating 3 times, the composite solid and the cordierite ceramic honeycomb carrier are mixed. The mass of the composite solid is 15% of the mass of the cordierite ceramic honeycomb carrier. Then, the precious metal Pd is first loaded by the impregnation method, and then the precious metal Rh is loaded, and finally the precious metal Pt is loaded. The mass ratio of Pt, Pd and Rh is 2:5:1. After loading, it is dried, calcined and reduced to obtain a high-activity catalyst for a three-way catalytic converter.

[0043] Example 6

[0044] The catalyst is prepared in the following specific steps:

[0045] The composite solid prepared in Example 3 is added to deionized water, stirred thoroughly until mixed evenly, then a cordierite ceramic honeycomb carrier is added, and ultrasonic immersion is performed at room temperature for 12 hours. After immersion, it is dried at 80°C for 12 hours. After repeating 3 times, the composite solid and the cordierite ceramic honeycomb carrier are mixed. The mass of the composite solid is 15% of the mass of the cordierite ceramic honeycomb carrier. Then, the precious metal Pd is first loaded by the impregnation method, and then the precious metal Rh is loaded. Finally, the precious metal Pt is loaded. The mass ratio of Pt, Pd, and Rh is 2:4:1. After loading, it is dried, calcined, and reduced to obtain a high-activity catalyst for a three-way catalytic converter.

[0046] Comparative Example 1

[0047] The preparation of the composite solid is carried out in the following steps:

[0048] 10g of powdered active γ-Al2 O 3 and 0.2 g of La(NO 3 ) 3 6H 2 O was ultrasonically dispersed and dissolved in 200 mL of ethanol and stirred at room temperature for 12 h. Then 2 g of Ce(NO 3 ) 3 6H 2 O, stirred at room temperature for 12 h, evaporated in a water bath at 60 ° C, dried in an oven at 80 ° C for 12 h, and then annealed under nitrogen protection at a heating rate of 2.5 ° C / min, annealing temperature of 800 ° C, annealing time of 3 h, and then cooled to room temperature to obtain γ-Al 2 O 3 / La 2 O 3 -CeO 2 , that is, a composite solid.

[0049] Comparative Example 2

[0050] The preparation of the composite solid is carried out in the following steps:

[0051] 10g of powdered active γ-Al 2 O 3 and 2 g of Ce(NO 3 ) 3 6H 2 O was ultrasonically dispersed and dissolved in 200 mL of ethanol, stirred at room temperature for 24 h, evaporated to dryness in a 60 °C water bath, dried in an oven at 80 °C for 12 h, and then annealed under nitrogen protection at a heating rate of 2.5 °C / min, an annealing temperature of 800 °C, an annealing time of 3 h, and then cooled to room temperature to obtain γ-Al 2 O 3 / CeO 2 , that is, a composite solid.

[0052] Comparative Example 3

[0053] The catalyst is prepared in the following specific steps:

[0054] The remaining steps remained unchanged, except that the composite solid of Example 4 was replaced by the composite solid of Comparative Example 1 to prepare a catalyst.

[0055] Comparative Example 4

[0056] The catalyst is prepared in the following specific steps:

[0057] The remaining steps remained unchanged, except that the composite solid of Example 4 was replaced by the composite solid of Comparative Example 2 to prepare the catalyst.

[0058] Comparative Example 5

[0059] The catalyst is prepared in the following specific steps:

[0060] The remaining steps remain unchanged, only the composite solid of Example 4 is removed to prepare the catalyst.

[0061] Performance Testing

[0062] The catalysts prepared in Examples 4-6 and Comparative Examples 3-5 were aged for 48 hours under the same conditions according to the GMAC875 bench cycle of General Motors, USA. The vehicle emission test was carried out according to the ECE+EUDC cycle to test the vehicle's emissions of hydrocarbons, carbon monoxide and nitrogen oxides. The test results are shown in the following table:

[0063] project Hydrocarbon (g / km) Carbon monoxide (g / km) Nitrogen oxides (g / km) Example 4 0.028 0.51 0.027 Example 5 0.031 0.54 0.030 Example 6 0.029 0.52 0.029 Comparative Example 3 0.036 0.69 0.041 Comparative Example 4 0.047 0.71 0.052 Comparative Example 5 0.291 0.85 0.068

[0064] It can be seen from the test results in the above table that the catalyst prepared in the embodiment of the present invention has a more excellent catalytic conversion rate.

[0065] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0066] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a high-activity catalyst for a three-way catalytic converter, characterized in that: The following steps are involved: The composite solid is mixed with the carrier, and then the precious metal is loaded by an impregnation method. After the loading is completed, it is dried, calcined, and reduced to obtain a high-activity catalyst for a three-way catalytic converter; Wherein, the composite solid is prepared by the following steps: (1) Dispersing γ-Al2O3, Ce(NO3)3·6H2O and Zr(NO3)4·5H2O in ethanol, stirring and adding citric acid ethanol solution, stirring at room temperature for 24 hours to obtain an impregnation solution; (2) Add La(NO3)3·6H2O to the impregnation solution obtained in step (1), stir at room temperature for 12 hours, then add Ce(NO3)3·6H2O, stir for another 12 hours, dry, calcine, and cool to obtain a composite solid.

2. The method for preparing a high-activity catalyst for a three-way catalytic converter according to claim 1, characterized in that: The carrier is a cordierite ceramic honeycomb carrier.

3. The method for preparing a high-activity catalyst for a three-way catalytic converter according to claim 1, characterized in that: The concentration of the citric acid ethanol solution in step (1) is 0.013 mol / L.

4. The method for preparing a high-activity catalyst for a three-way catalytic converter according to claim 1, characterized in that: In the step (1), the usage ratio of γ-Al2O3, Ce(NO3)3·6H2O, Zr(NO3)4·5H2O and citric acid ethanol solution is 10g:0.07g:0.05g:50mL.

5. The method for preparing a high-activity catalyst for a three-way catalytic converter according to claim 1, characterized in that: In the step (2), the usage ratio of La(NO3)3·6H2O and Ce(NO3)3·6H2O is 0.2g:2g.

6. The method for preparing a high-activity catalyst for a three-way catalytic converter according to claim 1, characterized in that: The heating rate during calcination in step (2) is 2-10°C / min, the calcination temperature is 400-1000°C, and the calcination time is 2-4h.

7. The method for preparing a high-activity catalyst for a three-way catalytic converter according to claim 6, characterized in that: The heating rate during calcination in step (2) is 2.5°C / min, the calcination temperature is 800°C, and the calcination time is 3h.

8. The method for preparing a high-activity catalyst for a three-way catalytic converter according to claim 1, characterized in that: The noble metals are Pt, Pd and Rh compounded in a mass ratio of 2:(3-5):

1.

9. A high-activity catalyst for a three-way catalytic converter, characterized in that: The catalyst is prepared according to the method for preparing a high-activity catalyst for a three-way catalytic converter according to any one of claims 1 to 8.