Bifunctional catalyst as well as preparation method and application thereof

By introducing Mg and Zn into ZrO2 aerogel oxide and mixing it with zeolite, the dual-function catalyst was prepared, which solved the problem of low alkane selectivity and yield in the preparation of liquefied petroleum gas by hydrogenation of CO2, and achieved efficient carbon utilization and low-cost industrial-grade catalytic effects.

CN119016099APending Publication Date: 2024-11-26SHANDONG ENERGY GROUP COAL GASIFICATION & NEW MATERIALS TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135095.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the alkane selectivity and yield of CO2 hydrogenation is low, precious metal catalysts are costly and low carbon utilization efficiency in industrial applications.

Method used

By introducing Mg and Zn into ZrO2 aerogel oxide, Mg-Zn co-doped ZrO2 aerogel oxide is formed and mixed with zeolite, a bifunctional catalyst is prepared for CO2 hydrogenation to prepare liquefied petroleum gas. The method includes gelling the Zr source, Zn source, and Mg source in a mixed solution of ethanol and water, passing it into supercritical CO2 and calcining it after drying, obtaining Mg-Zn co-doped ZrO2 aerogel oxide, and then Mixed with SAPO-34 or SSZ-13 zeolite to form a bifunctional catalyst.

Benefits of technology

The maximum spatiotemporal yield of liquefied petroleum gas is 88g·kgcat-1·h-1 and the maximum yield is 27.2%, the selectivity of LPG in hydrocarbons reaches 90%, and the stability of the catalyst is maintained during long-term operation. Provides an efficient industrial prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004999170220000071
    Figure BDA0004999170220000071
  • Figure BDA0004999170220000081
    Figure BDA0004999170220000081
  • Figure BDA0004999170220000082
    Figure BDA0004999170220000082
Patent Text Reader

Abstract

The invention provides a bifunctional catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: a) dissolving a Zr source, a Zn source and a Mg source in a mixed solution of ethanol and water, and sequentially adding formamide, 1, 2-epoxypropane and acetic acid for gelation to obtain wet gel; b) sealing the wet gel obtained in the step a) in an autoclave, and introducing supercritical CO2 for drying; and calcining the dried solid, so as to obtain the Mg-Zn co-doped ZrO2 aerogel oxide. And c) mixing the Mg-Zn co-doped ZrO2 aerogel oxide obtained in the step b) with zeolite to obtain the bifunctional catalyst. Compared with the prior art, the preparation method provided by the invention has the advantages that Mg and Zn are introduced into the ZrO2 aerogel oxide to obtain the Mg-Zn co-doped ZrO2 aerogel oxide, and then the Mg-Zn co-doped ZrO2 aerogel oxide is mixed with the zeolite to obtain the bifunctional catalyst, so that relatively good overall interaction is realized, and the bifunctional catalyst shows excellent catalytic performance in a reaction for preparing liquefied petroleum gas through CO2 hydrogenation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and more specifically to a bifunctional catalyst and a preparation method and application thereof. Background Art

[0002] The increasing concentration of carbon dioxide (CO2) in the atmosphere has led to a series of problems such as global warming, sea level rise, and ocean acidification. Therefore, there is an urgent need to develop powerful technical means to utilize, capture, or store CO2. Compared with storage, the direct conversion of CO2 into high-value-added chemicals has received widespread attention because it not only reduces CO2 emissions, but also utilizes CO2 as a carbon raw material. The effective conversion of CO2 contributes to the sustainable utilization of resources. There are two reaction pathways for CO2 hydrogenation: the modified Fischer-Tropsch synthesis (FTS) pathway and the methanol intermediate pathway. The modified FTS route is generally achieved using iron-based or cobalt-based catalysts, and the resulting products conform to the Anderson-Schulz-Flory (ASF) distribution. In contrast, the methanol intermediate pathway has attracted attention because it easily breaks the ASF rule. Due to the constraint of the zeolite catalyst, it shows high selectivity for the target product.

[0003] Liquefied petroleum gas (LPG) is a general term for propane and butane, which is widely used as a clean fuel due to its environmentally friendly properties. LPG is a substitute for aerosol propellants, refrigerants, etc., and is comparable to gasoline or diesel in terms of engine performance and maintenance. In addition, LPG can be easily converted, stored and transported in liquid phase. Therefore, the hydrogenation of CO2 to produce LPG is a promising technology. In recent years, many researchers have devoted themselves to the development of efficient bifunctional oxide / zeolite catalysts. For example, CO / CO2 hydrogenation can be used to produce LPG on Cr2O3, ZnZrO x Methanol is produced on ZnCr2O4 oxides. Methanol is then converted to paraffins, olefins, aromatics or liquid fuels via zeolites (SAPO-11, SAPO-18, SSZ-13, SAPO-34 or ZSM-5). However, obtaining a single specific product remains challenging.

[0004] At present, the target products in CO2 hydrogenation research are mainly concentrated on small molecular weight hydrocarbons or oxygen-containing compounds such as methanol (such as CN201410604941.6), methyl ether (such as CN202210400970.5), methane (such as CN201811527768.9) and low carbon olefins (such as CN202310926848.6), while there are few studies on CO2 hydrogenation to produce long-chain hydrocarbons. Liu Zhongmin's team reported an InZrO x / h-ssz-13 composite catalyst, under the reaction conditions of 350℃, 4.0MPa, and H2 / CO2 ratio of 3 / 1, the CO2 conversion rate was 24% within 100h, and the propane selectivity was about 70%. However, the CO selectivity was 61%, the carbon utilization efficiency was low, and the LPG yield was about 8.5%. Li Hangjie and others designed the Pd / SiO2@S1@H-ZSM-5 double-shell capsule catalyst, which showed good selectivity in the CO2 hydrogenation to LPG reaction. The use of precious metal Pd reduces CO selectivity and improves CO2 conversion, but the use of Pd significantly increases the cost of catalyst preparation.

[0005] In summary, there are many studies on the direct conversion of CO2 into liquid chemicals through methods such as thermal catalysis, electrocatalysis and photocatalysis, but most of them have not been successfully implemented at the industrial level; similarly, compared with the latter two catalytic methods, the thermal catalytic method has a higher yield and broad prospects, and is the most promising candidate method. Summary of the invention

[0006] In view of this, the purpose of the present invention is to provide a bifunctional catalyst and its preparation method and application, which can solve the problems existing in the prior art such as low alkane selectivity and yield and low carbon utilization, and cost limitations of precious metal catalysts in industrial applications.

[0007] The present invention provides a method for preparing a bifunctional catalyst, comprising the following steps:

[0008] a) dissolving a Zr source, a Zn source and a Mg source in a mixed solution of ethanol and water, and sequentially adding formamide, 1,2-propylene oxide and acetic acid for gelation to obtain a wet gel;

[0009] b) sealing the wet gel obtained in step a) in an autoclave, introducing supercritical CO2 to dry it; and then calcining the dried solid to obtain Mg-Zn co-doped ZrO2 aerogel oxide;

[0010] c) mixing the Mg-Zn co-doped ZrO2 aerogel oxide obtained in step b) with zeolite to obtain a bifunctional catalyst.

[0011] Preferably, the molar ratio of the Zr source, formamide, 1,2-propylene oxide and acetic acid in step a) is 1: (0.5-1.5): (10-20): (1-2);

[0012] The molar ratio of the Zr source, the Zn source and the Mg source is 8:1:(1-3).

[0013] Preferably, in step a), the usage ratio of the Zr source to ethanol and water is 10.7 g: (50 mL to 150 mL): (50 mL to 150 mL).

[0014] Preferably, the process of sequentially adding formamide, 1,2-propylene oxide and acetic acid for gelation in step a) is specifically as follows:

[0015] First, stir at 20°C to 30°C for 0.5h to 1.5h, add formamide, 1,2-propylene oxide and acetic acid in sequence, stir again for 0.5h to 1.5h, and then heat the mixed solution to gel to obtain a wet gel.

[0016] Preferably, the pressure of supercritical CO2 introduced in step b) is 7MPa-8MPa; the drying temperature is 250°C-270°C, and the drying time is 0.5h-1.5h.

[0017] Preferably, the calcination temperature in step b) is 500° C. to 600° C., and the calcination time is 4 h to 6 h.

[0018] Preferably, the zeolite in step c) is selected from SAPO-34 and / or SSZ-13;

[0019] The mass ratio of the Mg-Zn co-doped ZrO2 aerogel oxide to the zeolite is 1:(1.5-2.5).

[0020] The present invention also provides a bifunctional catalyst, which is prepared by the preparation method described in the above technical solution.

[0021] The present invention also provides an application of a catalyst in the preparation of liquefied petroleum gas by hydrogenation of CO2, wherein the catalyst is the bifunctional catalyst described in the above technical solution.

[0022] Preferably, the reaction temperature for preparing liquefied petroleum gas is 300°C to 400°C, the reaction pressure is 4MPa to 6MPa, the volume fraction of CO2 is 20vol% to 30vol%, and the GHSV is 1000mlg -1 h -1 ~1500ml g -1 h -1 The reaction time is 2h~6h, and the amount of catalyst used is 0.1g~1g.

[0023] The present invention provides a bifunctional catalyst and a preparation method and application thereof; the preparation method comprises the following steps: a) dissolving a Zr source, a Zn source and a Mg source in a mixed solution of ethanol and water, and sequentially adding formamide, 1,2-propylene oxide and acetic acid for gelation to obtain a wet gel; b) sealing the wet gel obtained in step a) in an autoclave, and passing supercritical CO2 for drying; and then calcining the dried solid to obtain a Mg-Zn co-doped ZrO2 aerogel oxide; c) mixing the Mg-Zn co-doped ZrO2 aerogel oxide obtained in step b) with zeolite to obtain a bifunctional catalyst. Compared with the prior art, the preparation method provided by the present invention introduces Mg and Zn into the ZrO2 aerogel oxide to obtain a Mg-Zn co-doped ZrO2 aerogel oxide, and then mixes it with zeolite to obtain a bifunctional catalyst, thereby achieving overall better interaction: the bifunctional catalyst exhibits excellent catalytic performance in the CO2 hydrogenation to liquefied petroleum gas reaction. Experimental results show that the maximum space-time yield of LPG is 88g·kgcat when the bifunctional catalyst provided by the present invention is used. -1 ·h -1 , the highest yield was 27.2%, and the selectivity of LPG in hydrocarbons reached 90%; during long-term operation, no obvious deactivation was observed, and the doping process effectively increased the surface defects of the aerogel oxide, thereby promoting the conversion of CO2, providing an industrially promising route for the production of liquefied petroleum gas by highly selective CO2 hydrogenation. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 XPS spectra of different aerogel catalysts;

[0025] Figure 2 Effect of contact time on CO2 conversion, LPG selectivity, yield and space-time yield. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] The present invention provides a method for preparing a bifunctional catalyst, comprising the following steps:

[0028] a) dissolving a Zr source, a Zn source and a Mg source in a mixed solution of ethanol and water, and sequentially adding formamide, 1,2-propylene oxide and acetic acid for gelation to obtain a wet gel;

[0029] b) sealing the wet gel obtained in step a) in an autoclave, introducing supercritical CO2 to dry it; and then calcining the dried solid to obtain Mg-Zn co-doped ZrO2 aerogel oxide;

[0030] c) mixing the Mg-Zn co-doped ZrO2 aerogel oxide obtained in step b) with zeolite to obtain a bifunctional catalyst.

[0031] The present invention first dissolves a Zr source, a Zn source, and a Mg source in a mixed solution of ethanol and water, and then sequentially adds formamide, 1,2-propylene oxide, and acetic acid for gelation to obtain a wet gel. The present invention has no special restrictions on the sources of the Zr source, Zn source, Mg source, ethanol, formamide, 1,2-propylene oxide, and acetic acid, and commercially available products known to those skilled in the art can be used; the water is preferably deionized water.

[0032] In the present invention, the Zr source is preferably ZrO(NO3)2·2H2O; the Zn source is preferably Zn(NO3)2; and the Mg source is preferably Mg(NO3)2·9H2O.

[0033] In the present invention, the molar ratio of the Zr source, formamide, 1,2-propylene oxide and acetic acid is preferably 1:(0.5-1.5):(10-20):(1-2); the molar ratio of the Zr source, Zn source and Mg source is preferably 8:1:(1-3).

[0034] In the present invention, the usage ratio of the Zr source to ethanol and water is preferably 10.7 g: (50 mL to 150 mL): (50 mL to 150 mL), and more preferably 10.7 g: 100 mL: 100 mL.

[0035] In the present invention, the process of sequentially adding formamide, 1,2-propylene oxide and acetic acid for gelation is preferably as follows:

[0036] First, stir at 20°C to 30°C for 0.5h to 1.5h, add formamide, 1,2-propylene oxide and acetic acid in sequence, stir again for 0.5h to 1.5h, and then heat the mixed solution to gel to obtain a wet gel.

[0037] After obtaining the wet gel, the present invention seals the obtained wet gel in an autoclave, introduces supercritical CO2 for drying, and then calcines the dried solid to obtain Mg-Zn co-doped ZrO2 aerogel oxide. The present invention doping Mg and Zn in ZrO2 is conducive to generating more surface defects, improving the adsorption capacity of the oxide aerogel for CO2, and the pore size of the oxide aerogel increases with the increase of the Mg doping amount.

[0038] In the present invention, the pressure of the supercritical CO2 is preferably 7MPa to 8MPa; the temperature of the drying is preferably 250°C to 270°C, and the drying time is preferably 0.5h to 1.5h.

[0039] In the present invention, the calcination temperature is preferably 500° C. to 600° C., and the calcination time is preferably 4 h to 6 h.

[0040] After obtaining the Mg-Zn co-doped ZrO2 aerogel oxide, the present invention mixes the obtained Mg-Zn co-doped ZrO2 aerogel oxide with zeolite to obtain a bifunctional catalyst.

[0041] In the present invention, the zeolite is preferably selected from SAPO-34 and / or SSZ-13, more preferably SAPO-34 or SSZ-13; SAPO-34 and SSZ-13 molecular sieves exhibit the highest LPG selectivity, SSZ-13 has the highest propane selectivity, and SAPO-34 is more conducive to the production of butane. The present invention has no particular restrictions on the source of the zeolite, and commercially available products or self-made products known to those skilled in the art can be used.

[0042] In the present invention, the mass ratio of the Mg-Zn co-doped ZrO2 aerogel oxide to the zeolite is 1:(1.5-2.5). In the present invention, the matching of the contact interface between the oxide and the zeolite is the key to directional acquisition of liquefied petroleum gas.

[0043] The preparation method provided by the present invention introduces Mg and Zn into ZrO2 aerogel oxide to obtain Mg-Zn co-doped ZrO2 aerogel oxide, and then mixes it with zeolite to obtain a bifunctional catalyst to achieve overall good interaction: the bifunctional catalyst exhibits excellent catalytic performance in the reaction of CO2 hydrogenation to produce liquefied petroleum gas.

[0044] The present invention also provides a bifunctional catalyst, which is prepared by the preparation method described in the above technical solution. The bifunctional catalyst provided by the present invention is composed of Mg-Zn co-doped ZrO2 aerogel oxide and SAPO-34 / SSZ-13 zeolite, and is used for the CO2 hydrogenation to LPG reaction. The introduction of Mg-Zn into the ZrO2 aerogel oxide not only improves the CO2 conversion rate, but also adjusts the ratio of propane and butane in LPG. The experimental results show that the maximum space-time yield and yield of liquefied petroleum gas are 88g·kgcat -1 ·h -1 and 27.2%, and the selectivity of liquefied petroleum gas in hydrocarbons reaches 90%; in addition, no obvious deactivation phenomenon is observed during the 100-hour production process; therefore, the present invention provides a stable and efficient catalyst for the hydrogenation of carbon dioxide to produce liquefied petroleum gas.

[0045] The present invention also provides an application of a catalyst in the preparation of liquefied petroleum gas by hydrogenation of CO2, wherein the catalyst is a bifunctional catalyst as described in the above technical solution. The present invention provides a new thermal catalytic method for preparing LPG by hydrogenation of CO2, which is a new strategy for directly converting carbon dioxide molecules into liquefied petroleum gas (LPG). The selectivity of LPG in hydrocarbons reaches 90%, while the carbon dioxide yield of liquefied petroleum gas is 27.2%, and 88g·kg -1 ·h -1 Space-time yield of CO2 to liquefied petroleum gas.

[0046] In the present invention, the reaction temperature for preparing liquefied petroleum gas is preferably 300°C to 400°C, the reaction pressure is preferably 4MPa to 6MPa, the volume fraction of CO2 is preferably 20vol% to 30vol%, and the GHSV is preferably 1000ml g -1 h -1 ~1500mlg -1 h -1 The reaction time is preferably 2h to 6h, and the amount of catalyst used is preferably 0.1g to 1g.

[0047] The thermal catalytic method for producing LPG by hydrogenating CO2 mentioned above in the present invention directly converts carbon dioxide into high value-added chemicals compared with storage, thereby reducing carbon dioxide emissions; precious metal catalysts show good selectivity in the reaction of hydrogenating CO2 to produce LPG, but the use of precious metals significantly increases the preparation cost, while the present invention uses inexpensive metal catalysts; currently, research on direct conversion of CO2 by thermal catalysis, electrocatalysis and photocatalysis is in the ascendant. Compared with the latter two catalytic methods, the thermal catalytic method adopted in the present invention has a higher yield and broad prospects, and is the most promising candidate method.

[0048] The present invention provides a bifunctional catalyst and a preparation method and application thereof; the preparation method comprises the following steps: a) dissolving a Zr source, a Zn source and a Mg source in a mixed solution of ethanol and water, and sequentially adding formamide, 1,2-propylene oxide and acetic acid for gelation to obtain a wet gel; b) sealing the wet gel obtained in step a) in an autoclave, and passing supercritical CO2 for drying; and then calcining the dried solid to obtain a Mg-Zn co-doped ZrO2 aerogel oxide; c) mixing the Mg-Zn co-doped ZrO2 aerogel oxide obtained in step b) with zeolite to obtain a bifunctional catalyst. Compared with the prior art, the preparation method provided by the present invention introduces Mg and Zn into the ZrO2 aerogel oxide to obtain a Mg-Zn co-doped ZrO2 aerogel oxide, and then mixes it with zeolite to obtain a bifunctional catalyst, thereby achieving overall better interaction: the bifunctional catalyst exhibits excellent catalytic performance in the CO2 hydrogenation to liquefied petroleum gas reaction. Experimental results show that the maximum space-time yield of LPG is 88g·kgcat when the bifunctional catalyst provided by the present invention is used. -1 ·h -1 , the highest yield was 27.2%, and the selectivity of LPG in hydrocarbons reached 90%; during long-term operation, no obvious deactivation was observed, and the doping process effectively increased the surface defects of the aerogel oxide, thereby promoting the conversion of CO2, providing an industrially promising route for the production of liquefied petroleum gas by highly selective CO2 hydrogenation.

[0049] In order to further illustrate the present invention, the following examples are provided for detailed description.

[0050] Preparation Example

[0051] 10.7 g ZrO(NO3)2·2H2O was dissolved in a mixed solution of 100 mL ethanol solution and 100 mL water. After stirring at room temperature for 1 h, 1.8 g formamide, 30.2 g 1,2-propylene oxide and 2.7 g acetic acid were added in sequence. After stirring again for about 1 hour, the mixed solution was heated to gelation. The wet gel was sealed in an autoclave, and supercritical CO2 flowed into the autoclave through a high-pressure pump to keep the pressure in the autoclave at about 7.5 MPa. The autoclave was then heated to 260°C for 1 h for CO2 supercritical drying. The dried solid was calcined at 550°C for 5 h, and the resulting catalyst was ZrO2 aerogel, denoted as sc-ZrO2.

[0052] By the above method, ZrO2 catalysts with different Zn / Mg doping amounts can be synthesized by adding Zn(NO3)2 or Mg(NO3)2·9H2O into the system. The molar ratio of Zr to Zn / Mg is 8:1, and the obtained catalyst is recorded as sc-Zn-ZrO2 or sc-Mg-ZrO2. The Zn-Mg co-doped ZrO2 catalyst is recorded as sc-MZZO. The sc-MZZO-X aerogel catalyst refers to a catalyst with a Zr:Zn:Mg molar ratio of 8:1:X. The catalyst obtained by directly drying and calcining the MZZO sol without supercritical CO2 drying is named sg-MZZO.

[0053] SSZ-13 and SAPO-34 zeolites were purchased from ACS Materials. According to XRF, SSZ-13 is composed of Al2O3-SiO2 with a mass ratio of 6.69-93.31, and SAPO-34 is composed of P2O5-Al2O3-SiO2 with a mass ratio of 58.35-24.61-17.04. Beta, MOR, ZSM-5 and Y zeolites were purchased from Tosoh. XRF analysis showed that Beta, MOR, ZSM-5 and Y molecular sieves are composed of Al2O3-SiO2 with mass ratios of 2.01-97.99, 4.59-95.41, 3.55-96.45 and 6.05-93.95, respectively. Before testing, the zeolite was calcined at 550°C for 2 hours. The composite catalyst was prepared by mixing the aerogel oxide with the zeolite powder to obtain a bifunctional catalyst.

[0054] The bifunctional catalyst provided by the present invention is composed of a co-doped aerogel catalyst and zeolite, wherein the molar ratio (optimal ratio) of each element component of the aerogel catalyst is shown in Table 1 below.

[0055] Table 1

[0056]

[0057] The parameters of the metal oxide catalyst were obtained by physical adsorption analysis of N2, as shown in Table 2 below.

[0058] Table 2

[0059]

[0060]

[0061] The oxygen vacancy concentration was calculated by the area ratio of the oxygen vacancy signal peak to the oxygen lattice signal peak, as Figure 1 shown by Figure 1It can be seen that three different O1s signal peaks were observed. The peak at 529.44 eV is considered to be the lattice oxygen atom, and the peaks at 531.01 and 532.6 eV are attributed to the oxygen vacancies near the oxygen atoms and the adsorption of water molecules, respectively. The presence of abundant oxygen vacancies on the outer surface of the aerogel catalyst is conducive to the activation of CO bonds, which makes sc-MZZO-2 a potential CO2 activation catalyst. In addition, the oxygen vacancy concentration was calculated by the area ratio of the oxygen vacancy signal peak to the oxygen lattice signal peak. After H2 reduction, the O Vac. / O Lat The value is 0.46. Vac. / O Lat The value is 0.89. Compared with the sg-MZZO-2 catalyst, the sc-MZZO-2 catalyst has a larger specific surface area and a higher O Vac. / O Lat value.

[0062] It can be seen that after H2 reduction, the O Vac. / O Lat The value is 0.46, and that of the sc-MZZO-2 catalyst is 0.89. The abundant oxygen vacancies on the outer surface are conducive to the activation of CO bonds, which makes the sc-MZZO-2 oxide a potential CO2 activation catalyst. Compared with the sg-MZZO-2 catalyst, the sc-MZZO-2 catalyst has a larger surface area and higher O Vac. / O Lat value.

[0063] Application Examples

[0064] Reaction conditions: 360°C, 5.0 MPa (22.99 vol% CO2, 3.0 vol% CO, 3.0 vol% Ar and H2 balance), GHSV = 1200 mlg -1 h -1 , reaction time (TOS) = 4h. Catalyst weight 0.5g, oxide / zeolite mass ratio 1:2. C2-C4 0 Indicates the selectivity of products other than propane and butane to C2 to C4.

[0065] See Tables 3-4 below for product distribution.

[0066] Table 3

[0067]

[0068] The results in Table 3 show that SAPO-34 and SSZ-13 molecular sieves with a single 8 MR micropores exhibit the highest LPG selectivity. SSZ-13 has the highest propane selectivity, reaching 75.4%, while SAPO-34 is more conducive to the formation of butane. In turn, the hydrogenation ability of the aerogel catalyst is another key to obtaining high LPG selectivity.

[0069] Table 4

[0070]

[0071] The results in Table 4 show that when sc-ZrO2 / SAPO-34 was tested at 360°C and 5.0MPa, the LPG selectivity was 66.1%, the CO2 conversion rate was only 6.5%, and the CO selectivity was 52.2% (see Table 5). Doping Mg or (and) Zn in ZrO2 is conducive to generating more surface defects, improving the adsorption capacity of oxide aerogel for CO2, and the pore size of oxide aerogel increases with the increase of Mg doping amount.

[0072] The performance of the bifunctional catalyst is shown in Table 5 below.

[0073] Table 5

[0074] catalyst <![CDATA[CO2 conversion rate]]> CO selectivity LPG yield <![CDATA[sc-ZrO2 / SAPO-34]]> 6.5 52.2 2.1 <![CDATA[sc-Zn-ZrO2 / SAPO-34]]> 16.3 56.6 4.8 <![CDATA[sc-Mg-ZrO2 / SAPO-34]]> 13.6 67.8 3.2 sc-MZZO-1 / SAPO-34 20.9 52.7 8.0 sc-MZZO-2 / SAPO-34 23.9 49.1 10.5 sc-MZZO-3 / SAPO-34 22.1 46.7 8.4

[0075] Experiments have found that adjusting the amount of Mg-Zn on the ZrO2 catalyst can change the ratio with butane. Under the same conditions, after the introduction of Zn, the CO2 conversion rate of sc-Zn-ZrO2 reached 16.3%. The selectivity and yield of LPG reached 67.7% and 4.8%, respectively. After introducing Zn and Mg on ZrO2, the sc-MZZO-1 / SAPO-34 catalyst achieved a CO2 conversion rate of 20.9% and a propane selectivity of 73.1%. Further increasing the Mg content, the selectivity of the sc-MZZO-2 / SAPO-34 catalyst for propane decreased, and the selectivity for butane reached 17.8%, at which time the LPG yield was 10.5%. However, with the increase of Mg content, the selectivity and yield of liquefied petroleum gas decreased, and the amount of CH4 generated increased.

[0076] In addition, the present invention systematically studies the effect of contact time on CO2 conversion, LPG selectivity, yield and space-time yield, see Figure 2 As shown; Figure 2 The effect of contact time on CO2 conversion, LPG selectivity, yield and space-time yield was systematically studied. The gas hourly space velocity (GHSV) was 300 mL / g cat / h, CO2 conversion rate is 35.2%, CO selectivity is 14.2%, LPG selectivity is 90%, and LPG yield is 27.2%. With the increase of GHSV, the contact time between the feed gas and the catalyst is shortened, the CO2 conversion rate is reduced, and the CO selectivity is improved. At high GHSV (12000mL / g cat / h) condition, LPG selectivity reached 76%, and LPG space-time yield reached 88g·kg cat -1 ·h -1 . Further increase GHSV to 24000mL / g cat / h, some intermediates are separated from the catalyst bed because they do not have time to be completely converted. They are separated directly from the bed before they can be converted on the zeolite, resulting in a large amount of methanol and dimethyl ether in the final product. CH4 selectivity increased from 0.9% to 6%. The increase in greenhouse gas emissions also directly reduced C 5+ The selectivity of low-carbon products is improved.

[0077] It can be seen that when the gas hourly space velocity (GHSV) is 300mL / gcat / h, the CO2 conversion rate is 35.2%, the CO selectivity is 14.2%, the LPG selectivity is 90%, and the LPG yield is 27.2%. The CO2 conversion rate decreases, and the contact time between the feed gas and the catalyst is shortened as the GHSV increases, and the selectivity increases. Under high GHSV (12000mL / gcat / h), the LPG selectivity reaches 76%, and the LPG space-time yield reaches 88g·kgcat -1 ·h -1 . Further increasing the GHSV to 24000mL / gcat / h, some intermediates separated from the catalyst bed because they did not have time to be fully converted. They were separated directly from the bed before they could be converted on the zeolite, resulting in a large amount of methanol and dimethyl ether in the final product. The CH4 selectivity increased from 0.9% to 6%. The increase in greenhouse gas emissions also directly reduced the selectivity of C5+ and increased the selectivity of low-carbon products.

[0078] In summary, the catalytic behavior of the bifunctional catalyst provided by the present invention shows that zeolite is the main factor in the selective formation of liquefied petroleum gas, but the aerogel catalyst cannot be ignored. Compared with two separate reactions, tandem catalysis has thermodynamic advantages. Due to the chemical inertness of CO2, it is difficult to directly hydrogenate CO2 to methanol. However, when the two reactions are coupled, the generation of liquefied petroleum gas is more favorable from a thermodynamic point of view.

[0079] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a bifunctional catalyst, comprising the following steps: a) dissolving a Zr source, a Zn source and a Mg source in a mixed solution of ethanol and water, and sequentially adding formamide, 1,2-propylene oxide and acetic acid for gelation to obtain a wet gel; b) sealing the wet gel obtained in step a) in an autoclave, introducing supercritical CO2 to dry it; and then calcining the dried solid to obtain Mg-Zn co-doped ZrO2 aerogel oxide; c) mixing the Mg-Zn co-doped ZrO2 aerogel oxide obtained in step b) with zeolite to obtain a bifunctional catalyst.

2. The preparation method according to claim 1, characterized in that: The molar ratio of the Zr source, formamide, 1,2-propylene oxide and acetic acid in step a) is 1: (0.5-1.5): (10-20): (1-2); The molar ratio of the Zr source, Zn source and Mg source is 8:1:(1-3).

3. The preparation method according to claim 1, characterized in that: The usage ratio of the Zr source to ethanol and water in step a) is 10.7 g: (50 mL to 150 mL): (50 mL to 150 mL).

4. The preparation method according to claim 1, characterized in that: The process of sequentially adding formamide, 1,2-propylene oxide and acetic acid for gelation in step a) is specifically as follows: First, stir at 20°C to 30°C for 0.5h to 1.5h, add formamide, 1,2-propylene oxide and acetic acid in sequence, stir again for 0.5h to 1.5h, and then heat the mixed solution to gel to obtain a wet gel.

5. The preparation method according to claim 1, characterized in that: The pressure of supercritical CO2 introduced in step b) is 7MPa-8MPa; the drying temperature is 250°C-270°C, and the drying time is 0.5h-1.5h.

6. The preparation method according to claim 1, characterized in that: The calcination temperature in step b) is 500° C. to 600° C., and the calcination time is 4 h to 6 h.

7. The preparation method according to claim 1, characterized in that: In step c), the zeolite is selected from SAPO-34 and / or SSZ-13; The mass ratio of the Mg-Zn co-doped ZrO2 aerogel oxide to the zeolite is 1:(1.5-2.5).

8. A bifunctional catalyst, characterized in that The preparation method is described in any one of claims 1 to 7.

9. Use of a catalyst in the preparation of liquefied petroleum gas by hydrogenation of CO2, characterized in that: The catalyst is the bifunctional catalyst as claimed in claim 8.

10. Use of the catalyst according to claim 9 in preparing liquefied petroleum gas by hydrogenation of CO2, characterized in that: The reaction temperature for preparing liquefied petroleum gas is 300°C to 400°C, the reaction pressure is 4MPa to 6MPa, the volume fraction of CO2 is 20vol% to 30vol%, and the GHSV is 1000mlg -1 h -1 ~1500ml g -1 h -1 The reaction time is 2h~6h, and the amount of catalyst used is 0.1g~1g.