Aluminum alloy butt joint welding method
By combining high-frequency pulsed MIG welding with small-angle bevels and small gaps, the problems of high stress, large deformation, and porosity defects in the welding of thick plates in aluminum alloy car bodies for rail transit have been solved. This has achieved welding effects with low stress, small filler volume, and large penetration depth, thereby improving production efficiency.
Patent Information
- Application Number
- CN202411312638.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-26
AI Technical Summary
Existing technologies for welding thick plates in aluminum alloy car bodies for rail transit suffer from problems such as high welding stress, significant deformation, large amounts of filler metal, low production efficiency, and numerous porosity defects, making it difficult to meet the requirements of high-precision shape control and low-damage performance control.
A method combining high-frequency pulse mode with small-angle bevel and small gap is adopted. High-frequency pulse MIG welding is used in conjunction with optimized welding parameters such as current, speed and shielding gas, and oxide film removal is performed to achieve low-stress, small filler volume and large penetration welding.
It effectively reduces welding stress and deformation, reduces porosity defects, improves production efficiency, and enhances welding quality and efficiency.
Smart Images

Figure CN119016842A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an aluminum alloy butt joint welding method and belongs to the technical field of welding technology. Background Art
[0002] The existing welding process for the butt joints of the aluminum alloy body bolsters and the medium and thick plates (above 8mm) of the chassis of rail transit uses the conventional pulse MIG welding process method, and the joint conditions are: the butt joint groove angle is 70°, the welding gap is 2-3mm, and the blunt edge size is 0-1mm. The production of medium and thick plate welding parts of the car body according to the existing process often encounters the following problems: 1. Large welding stress and deformation; 2. The amount of welding filler metal is large, and the welding production efficiency is low; 3. There are many welding pores and unfused defects; 4. The softening phenomenon of welded joints due to aging is relatively serious. In other words, it is difficult for traditional welding processes to meet the requirements of "double control", namely "high-precision shape control" and "low damage controllability".
[0003] Therefore, the development of deep-fusion welding technology with "low stress, small deformation and high reliability" for rail vehicle aluminum alloy bodies is of self-evident importance in meeting on-site welding manufacturing requirements and helping enterprises achieve the "dual carbon" goals. It can be seen that a welding method for aluminum alloy butt joints is urgently needed. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for welding aluminum alloy butt joints. The method adopts a high-frequency pulse mode combined with a small angle groove and a small gap, which can effectively achieve low stress, small filling amount and large penetration welding, reduce the sensitivity of porosity generation, and improve production efficiency.
[0005] In order to achieve the above purpose / solve the above technical problems, the present invention is implemented by adopting the following technical solutions: A method for welding an aluminum alloy butt joint, comprising: Acquire preset information and collected information of the to-be-welded portion, and call corresponding preset welding data based on the collected information and the preset information; Cleaning the oxide film on the welded area; Based on the preset welding data, high-frequency pulse MIG welding is used to weld the welded area to form a weld. In the preset welding data, the welding groove angle is not greater than 60° and the welding gap is 1-2 mm.
[0006] Furthermore, in the preset welding data, the average current of the base welding is 180-210A, the average current of the filling and capping welding is 170-220A, and the welding speed is 30-50cm / min.
[0007] Furthermore, the welding groove angle is 40° and the welding gap is 2 mm.
[0008] Further, based on the preset welding data, high-frequency pulse MIG welding is used to weld the to-be-welded portion to form a weld, including: With the welding machine and shielding gas switches turned on, select the high-frequency pulse mode; According to the preset welding data, welding is performed in a four-step mode.
[0009] Furthermore, the protective gas includes argon gas, and the purity of the argon gas is greater than 99.99%, and the gas flow rate is 20L / min.
[0010] Furthermore, the welding heat input of the high-frequency pulse MIG welding is lower than the welding heat input of the conventional welding process specification.
[0011] Further, the oxide film is cleaned on the welded part, including: After using organic solvents to remove oil and dust from the welded area, the oxide film is cleaned and removed mechanically.
[0012] Furthermore, high pulse frequency mode current value welding uses a left-right swing and the arc stays briefly on both sides of the weld to fill the molten pool and prevent undercutting.
[0013] Compared with the prior art, the present invention has the following beneficial effects: The aluminum alloy butt joint welding method provided by the present invention adopts a method combining a high-frequency pulse mode with a small-angle groove and a small gap, which can effectively achieve low-stress, small filling volume, and large penetration welding, reduce the sensitivity of pore generation, and improve production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 is a flow chart of the method of the present invention; Figure 2 -a is a schematic diagram of a 40° groove of a 12 mm thick aluminum alloy butt joint according to the present invention; Figure 2 -b is a schematic diagram of a 60° groove of a 12 mm thick aluminum alloy butt joint according to the present invention; (t - plate thickness / mm; c - blunt edge / mm; α - groove angle / °; b - welding gap / mm); Figure 3 This is the macroscopic morphology of the joint of Example 1; Figure 4 This is the macroscopic morphology of the joint in Example 2; Figure 5 This is the macroscopic morphology of the comparative joint; Figure 6 This is the macroscopic morphology of the comparative joint; Figure 7 This is a macroscopic image of the weld of the embodiment (with low porosity sensitivity); Figure 8 This is a macroscopic image of the weld for comparison (with greater porosity sensitivity). DETAILED DESCRIPTION
[0015] The present invention will be further described below in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.
[0016] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and the like are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", and the like may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0017] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances. Example
[0018] like Figure 1 As shown, this embodiment provides an aluminum alloy butt joint welding method, comprising: Acquire preset information and collected information of the to-be-welded portion, and call corresponding preset welding data based on the collected information and the preset information; Cleaning the oxide film on the welded area; Based on the preset welding data, high-frequency pulse MIG welding is used to weld the welded area to form a weld. In the preset welding data, the welding groove angle is not greater than 60° and the welding gap is 1-2 mm.
[0019] When this method selects the high-frequency pulse mode, compared with the conventional welding method, the droplet transfer frequency is higher (about 250Hz). Under the same heat input and the same joint conditions (plate thickness, groove angle, blunt edge size, welding gap), the weld root penetration can be increased by about 20%, and the welding residual stress can be reduced by 30-50%.
[0020] Compared with the traditional pulse MIG welding process, the high-frequency pulse MIG welding process has many advantages: 1) Fast welding speed, high frequency (high speed) pulse form of multiple drops in one pulse can achieve higher welding speed, which can increase the welding speed by 30%-40%; 2) The arc column is narrowed to form a compressed arc, which consumes less heat, has a greater welding penetration, better back-side formation of the weld, improves welding quality, and reduces welding heat input; 3) This process can achieve high-quality welding with low heat input, narrower heat-affected zone width, and can also achieve welding of small-angle grooves, which is beneficial to reduce welding deformation, reduce welding filling amount, and reduce welding heat input; 4) Small current is more stable, which is conducive to the back forming of the base welding; 5) The arc has stronger penetration power, and when the base welding has a small gap or no gap, single-sided welding and double-sided forming can be achieved; 6) Welding spatter is significantly reduced, making the welding process cleaner.
[0021] 7) It has a significant stirring effect on the welding molten pool, effectively reducing the surface tension of the liquid metal in the molten pool, making the crystal grains finer, the fusion better, the sensitivity of welding porosity lower, and the metallurgical and mechanical properties of the weld better.
[0022] Furthermore, in the preset welding data, the average current of the base welding is 180-210A, the average current of the filling and capping welding is 170-220A, and the welding speed is 30-50cm / min.
[0023] Furthermore, the welding groove angle is 40° and the welding gap is 2 mm.
[0024] Further, based on the preset welding data, high-frequency pulse MIG welding is used to weld the to-be-welded portion to form a weld, including: With the welding machine and shielding gas switches turned on, select the high-frequency pulse mode; According to the preset welding data, welding is carried out in a four-step mode; In the field of welding, the four-step model is a welding operation process that includes the following steps: 1. Preparation: This stage includes preparing welding materials, cleaning welding surfaces, selecting appropriate welding methods, etc. This is an important step to ensure the smooth progress of the welding process and reduce welding defects.
[0025] 2. Determine the welding position: At this stage, the welder needs to select the appropriate welding position according to the welding requirements, such as horizontal welding, longitudinal welding, flat welding, etc., and determine the welding posture.
[0026] 3. Welding equipment selection: This step involves choosing the right welding machine and welding current. According to the characteristics and requirements of the welding materials, choosing the right welding equipment is crucial to ensuring the welding effect and quality.
[0027] 4. Welding operation: This is the actual stage of welding, including preparation before welding, the welding process itself, and post-welding treatment. The welder needs to operate according to the welding method and requirements, and perform necessary cleaning and inspection after welding.
[0028] The four-step mode helps welders to perform welding work systematically, ensuring welding quality and efficiency.
[0029] Furthermore, the protective gas includes argon gas, and the purity of the argon gas is greater than 99.99%, and the gas flow rate is 20L / min.
[0030] Furthermore, the welding heat input of the high-frequency pulse MIG welding is lower than the welding heat input of the conventional welding process specification.
[0031] Further, the oxide film is cleaned on the welded part, including: After using organic solvents to remove oil and dust from the welded area, the oxide film is cleaned and removed mechanically.
[0032] Furthermore, high-frequency pulse mode current value welding uses a technique of swinging left and right and the arc staying briefly on both sides of the weld to fill the molten pool and prevent undercutting.
[0033] The welding process parameters of the embodiment and comparative example of this case and the residual stress values at the weld toe of the butt joint weld are shown in Table 1 and Table 2: Table 1 Welding process parameters of Example (2) and Comparative Example (2)
[0034] Note: E—welding line energy of each welding layer (weld pass); E 总 —The sum of welding line energy for each welding layer (weld pass) Table 2 Residual stress values at the weld toe of the butt joint weld of the implementation and comparison examples
[0035] like Figure 2 -a and Figure 2 -b, where Figure 2 -a is a schematic diagram of the 40° groove of the aluminum alloy 12mm medium-thick plate butt joint. Figure 2 -b is a schematic diagram of a 60° groove for a 12mm thick aluminum alloy butt joint (t - plate thickness / mm; c - blunt edge / mm; α - groove angle / °; b - welding gap / mm); Combination Figure 3~Figure 8 As shown, it can be seen that compared with conventional pulse MIG, the high-frequency pulse MIG welding groove angle of the present invention is changed from 60° to 40°, the welding gap is changed from 2~3mm to 1~2mm, and a method combining a small angle groove and a small gap is adopted to effectively reduce the amount of welding wire filling; the number of welding layers is reduced from 5 layers to 3 layers, which significantly reduces the number of welding layers, greatly reduces the occurrence of welding defects, reduces welding heat input by 20%~30%, and reduces welding residual stress by 30%~40%, effectively realizing low stress, small filling amount, and large penetration welding, and can reduce the sensitivity of porosity generation, while improving production efficiency.
[0036] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for welding aluminum alloy butt joints, characterized in that: include: Acquire preset information and collected information of the to-be-welded portion, and call corresponding preset welding data based on the collected information and the preset information; Cleaning the oxide film on the welded area; Based on the preset welding data, high-frequency pulse MIG welding is used to weld the welded area to form a weld. In the preset welding data, the welding groove angle is not greater than 60° and the welding gap is 1-2 mm.
2. The aluminum alloy butt joint welding method according to claim 1, characterized in that: In the preset welding data, the average current of the base welding is 180-210A, the average current of the filling and capping welding is 170-220A, and the welding speed is 30-50cm / min.
3. The aluminum alloy butt joint welding method according to claim 1, characterized in that: The welding groove angle is 40° and the welding gap is 2 mm.
4. The aluminum alloy butt joint welding method according to claim 1, characterized in that: Based on the preset welding data, high-frequency pulse MIG welding is used to weld the to-be-welded portion to form a weld, including: With the welding machine and shielding gas switches turned on, select the high-frequency pulse mode; According to the preset welding data, welding is performed in a four-step mode.
5. The aluminum alloy butt joint welding method according to claim 4, characterized in that: The protective gas includes argon gas, and the purity of the argon gas is greater than 99.99%, and the gas flow rate is 20L / min.
6. The aluminum alloy butt joint welding method according to claim 1, characterized in that: The welding groove angle is 40° and the welding gap is 1 mm.
7. The aluminum alloy butt joint welding method according to claim 1, characterized in that: The oxide film is cleaned on the welding site, including: After using organic solvents to remove oil and dust from the welded area, the oxide film is cleaned and removed mechanically.
8. The aluminum alloy butt joint welding method according to claim 1, characterized in that: High-frequency pulse mode current value welding uses left and right swings and the arc stays for a while on both sides of the weld to fill the molten pool and prevent undercutting.