Method for improving bending resistance of ultra-high performance concrete outer wall decorative plate

By using high-strength fine aggregates, reducing viscosity, mechanical vibration and fine steel fibers in ultra-high performance concrete exterior wall decorative panels, the problem of insufficient bending performance is solved, and the ultimate bending strength is significant Improvement and performance optimization.

CN119017507APending Publication Date: 2024-11-26SHANGHAI RESEARCH INSTITUTE OF BUILDING SCIENCES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411414275.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Ultra-high performance concrete exterior wall decorative panels are not outstanding enough in terms of bending resistance and are difficult to match traditional glass fiber reinforced concrete, resulting in limitations in material selection in complex modeling buildings.

Method used

Use high-strength fine aggregate to replace quartz sand to reduce concrete viscosity, use small insertion vibrator to eliminate bubbles, use fine steel fiber to replace synthetic fibers, optimize fiber parameters and processes, and use jetting technology to prepare ultra-high performance concrete exterior wall decorative panels .

Benefits of technology

It significantly improves the bending resistance of ultra-high performance concrete exterior wall decorative panels, making their bending resistance limit strength reach more than 20MPa, which is better than traditional cement-based exterior wall panel materials, while maintaining strength, wear resistance and durability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for improving the bending resistance of an ultra-high-performance concrete outer wall decorative plate. The method adopts one or more of the following treatment means: 1, selecting high-strength fine aggregate to replace quartz sand during preparation of an ultra-high-performance concrete premix; 2, the viscosity reduction component is doped to reduce the viscosity of the ultra-high performance concrete mixture; 3, in the pouring process of the ultra-high performance concrete external wall panel, a small insertion type vibrating rod is adopted for conducting insertion tamping on the mixture, and a roller is used for removing bubbles in the mixture on the surface of the mixture in a rolling brush mode; 4, preparing an ultra-high performance concrete mixture by replacing synthetic crude fibers with fine fibers; 5, fiber parameters are optimized, and the orientation of the fibers in the ultra-high performance concrete mixture is improved; and 6, preparing the ultra-high performance concrete outer wall decorative plate by adopting a spraying process instead of a pouring process. By comprehensively adopting one or more of the methods, the bending resistance of the ultra-high-performance concrete can be greatly improved, and the light weight and thin wall of the ultra-high-performance concrete outer wall decorative plate are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ultra-high performance concrete, and in particular to a method for improving the bending resistance of an ultra-high performance concrete exterior wall decorative panel. Background Art

[0002] With the development of science and technology, new materials and new technologies are constantly emerging. As the most open and inclusive commercial building, the choice of building facade materials has gradually changed from single and simple to diversified, personalized, technological and modern. Cement-based materials represented by glass fiber reinforced concrete (GRC) and ultra-high performance concrete (UHPC) have unique advantages in the selection of building facade materials with complex shapes due to the convenience of pouring.

[0003] Glass fiber reinforced concrete is a fiber concrete composite material with alkali-resistant glass fiber as reinforcement material and cement mortar as matrix material. It has various textures and adjustable colors, and has been used in building exterior wall projects with high artistic requirements. However, GRC is essentially an ordinary fiber reinforced cement mortar board with poor durability and low technical threshold. There are mixed products on the market and serious quality and safety issues, which leads to designers being afraid of GRC when choosing exterior wall decorative panels. Shanghai clearly stipulates that high-rise buildings over 120 meters are not allowed to use GRC materials.

[0004] Ultra-high performance concrete (UHPC) is a new type of cement-based composite material with ultra-high strength (above 120MPa), ultra-high toughness and ultra-high durability, which enables it to reduce the size of the structural cross-section while meeting the requirements of structural bearing capacity, and to achieve lightweight and thin walls, allowing architectural designers to break through the constraints of materials and design light and beautiful structural shapes. However, although ultra-high performance concrete exterior wall panels have excellent comprehensive performance, they do not have an advantage over traditional GRC in terms of bending resistance, which is the most concerned aspect of designers. This is because ultra-high performance concrete exterior wall panels usually adopt a casting process, which has high requirements on the fluidity of the mixture performance, and the fiber volume content is limited, resulting in poor bending resistance. Therefore, how to significantly improve the bending resistance of ultra-high performance concrete exterior wall panels has always been a technical difficulty in the application of ultra-high performance concrete in the field of architectural decoration. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the problem that the bending resistance of existing ultra-high performance concrete is not outstanding enough when it is made into exterior wall decorative panels, and to provide a method that can greatly improve the bending resistance of ultra-high performance concrete exterior wall decorative panels, so that the ultra-high performance concrete exterior wall decorative panels can ensure the superior properties of strength, wear resistance, impact resistance, durability, etc., while the bending resistance is also better than traditional cement-based exterior wall panel materials such as GRC.

[0006] The technical problem to be solved can be implemented through the following technical solutions.

[0007] A method for improving the bending resistance of ultra-high performance concrete exterior wall decorative panels, characterized by comprising one or more of the following treatment methods or means:

[0008] (1) When preparing ultra-high performance concrete premix, high-strength fine aggregate is used to replace quartz sand;

[0009] (2) Adding viscosity-reducing components to reduce the viscosity of ultra-high performance concrete mixtures;

[0010] (3) During the pouring process of the ultra-high performance concrete exterior wall panels, a small inserted vibrator is used to tamp the mixture and a roller is used to roll the surface of the mixture to remove bubbles inside the mixture;

[0011] (4) Using fine steel fibers instead of synthetic coarse fibers to prepare ultra-high performance concrete mixtures;

[0012] (5) Optimizing fiber parameters to improve fiber orientation in ultra-high performance concrete mixtures;

[0013] (6) Use spraying technology instead of casting technology to prepare ultra-high performance concrete exterior wall decorative panels.

[0014] Furthermore, in the treatment method (1), the high-strength fine aggregate is fine aggregate prepared from bauxite clinker or machine-made sand made from granite, andesite or basalt with a parent rock strength of more than 120 MPa.

[0015] Furthermore, in treatment method (2), the viscosity reducing component is one or a combination of white silica fume, fly ash microspheres and viscosity reducing polycarboxylic acid water reducing agent, wherein the amount of white silica fume is 15% to 20%, and the amount of fly ash microspheres is 10% to 20%.

[0016] Furthermore, the expansion of the ultra-high performance concrete after viscosity reduction is in the range of 750 to 850 mm, the expansion time is less than 3 s, and the inverted slump cone time is less than 25 s.

[0017] Furthermore, in treatment method (3), the diameter of the end of the vibrating rod is no more than 20 mm, and it is placed in the ultra-high performance concrete mixture parallel to the direction of the exterior wall panel to vibrate it, and the distance between adjacent vibration points is no more than 20 cm.

[0018] Furthermore, in treatment method (4), when the micro-fiber steel fiber is stainless steel fiber, the stainless steel fiber replaces the synthetic coarse fiber with the same volumetric dosage; when the fine steel fiber is copper-plated steel fiber, the copper-plated steel fiber is used in the ultra-high performance concrete mixture of the lower 2 / 3 of the plate thickness, and the synthetic fiber is still used in the ultra-high performance concrete mixture of the surface 1 / 3 of the plate thickness.

[0019] Furthermore, in treatment method (5), the fiber length is not less than 70% of the board thickness, and during pouring, multiple layers are poured from one end to the other end so that the fibers are parallel to the board surface.

[0020] Furthermore, in treatment method (6), 0.001% by weight of starch ether is first added to the ultra-high performance concrete premix and stirred into a thixotropic mixture, and a fiber shearing device is provided. During construction, the ultra-high performance concrete mixture and fibers are uniformly sprayed onto the surface of the formwork through the fiber nozzle and the ultra-high performance concrete mixture nozzle to form an ultra-high performance concrete exterior wall decorative panel.

[0021] This method was used to produce sample test blocks with a length of 250 mm, a width of 50 mm, and a thickness of 10 mm, and the ultimate bending strength reached over 20 MPa.

[0022] The method for improving the bending resistance of the ultra-high performance concrete exterior wall decorative panel of the present invention is further described below:

[0023] Essentially, the improvement of the bending performance of ultra-high performance concrete exterior wall decorative panels mainly solves the following two problems:

[0024] (1) Improvement of ultra-high performance concrete matrix strength

[0025] The improvement of the bending performance of ultra-high performance concrete exterior wall decorative panels is closely related to the strength of the matrix. As the strength of the matrix increases, the bending ratio ultimate strength of the ultra-high concrete increases, and the corresponding bending ultimate strength of the ultra-high performance concrete also increases. The ultra-high performance concrete premix used in existing ultra-high performance concrete exterior wall decorative panels is usually only 100MPa, and the compressive strength is lower than that of the ultra-high performance concrete used for structures, resulting in the final exterior wall decorative panels The bending strength is also low. Therefore, the premise for improving the bending performance of ultra-high performance concrete exterior wall decorative panels is to improve the compressive strength of the matrix, and the hardness of aggregates is an important method to improve the strength of ultra-high performance concrete. Fine aggregates made from bauxite clinker and machine-made sand made from igneous rocks such as granite, andesite or basalt with a parent rock strength of more than 120MPa are of great help in improving the strength of the ultra-high performance concrete matrix.

[0026] (2) Reducing the air bubble content in ultra-high performance concrete

[0027] During the mixing process of ultra-high performance concrete, bubbles will be generated due to the effect of water reducer. Since ultra-high performance concrete has a low water-binder ratio and a high viscosity, it is difficult to fully discharge the bubbles after pouring, resulting in a large number of bubbles in the hardened ultra-high performance concrete. The presence of bubbles will affect the compactness of ultra-high performance concrete and cause the reduction of the bending mechanical properties of the exterior wall decorative panels. Therefore, to improve the bending properties of ultra-high performance concrete exterior wall panels, it is necessary to reduce the internal bubble content. One way is to select viscosity-reducing components such as white silica fume and fly ash microbeads during formula design and raw material selection. These materials can effectively reduce the viscosity of the mixture within a reasonable dosage range and are conducive to the discharge of bubbles. In addition, viscosity-reducing polycarboxylic acid water reducers are also conducive to reducing the viscosity of the mixture. Practice shows that when the expansion of ultra-high performance concrete is in the range of 750-850mm, the expansion time is less than 3s, and the inverted slump cone time is less than 25s, the viscosity of ultra-high performance concrete is low.

[0028] However, even if the viscosity of ultra-high performance concrete is reduced, its viscosity is still much higher than that of ordinary concrete, and it is impossible to eliminate all bubbles by optimizing the material's own performance. Therefore, in order to maximize the density of ultra-high performance concrete, external mechanical vibration is required to expel the bubbles. The use of a small inserted vibrating rod can eliminate more than 95% of the bubbles inside the material through the mechanical action of the vibrating rod. In this case, the bending strength of the matrix can be increased by more than 50%.

[0029] (3) Optimizing the fiber of ultra-high performance concrete system

[0030] Due to the aesthetic requirements, ultra-high performance concrete exterior wall decorative panels usually use synthetic fibers such as polypropylene fiber, polyoxymethylene fiber, and polyvinyl alcohol fiber as reinforcement materials. Such fibers have no risk of corrosion and will not affect the quality of the decorative panel finish during use. However, since the bonding performance of synthetic fibers with ultra-high performance concrete is not as good as that of steel fibers, the impact on the bending strength is greater. Therefore, when the bending performance requirements of ultra-high performance concrete exterior wall decorative panels are high, copper-plated steel fibers should be used instead of synthetic fibers. If the risk of corrosion of steel fibers is high, the method of using steel fibers for the bottom 2 / 3 ultra-high performance concrete and synthetic fibers for the surface 1 / 3 ultra-high performance concrete can be used to ensure the quality of the surface layer and improve the bending performance at the same time.

[0031] The fiber orientation arrangement in UHPCC can also significantly improve the flexural strength of UHPCC, with the maximum improvement reaching more than 50%. When the fiber length exceeds 70% of the plate thickness, due to the low plate thickness, the vertical distribution of the fiber in the system is relatively difficult, and the fiber cannot be randomly distributed in the system, but tends to be distributed parallel to the plate surface. Layered pouring is adopted during pouring, and each pouring is from one end to the other, which is also conducive to the distribution of fibers along the plate surface, thereby improving the flexural performance of the UHPCC exterior wall decorative panels.

[0032] (4) Optimizing the manufacturing process of ultra-high performance concrete exterior wall panels

[0033] Ultra-high performance concrete exterior wall panels are usually constructed by pouring technology, which must reduce the ultra-high performance concrete premix mixture into a uniform mixture. In this case, the fiber content in ultra-high performance concrete is relatively limited, usually 2% to 3% by volume. When using the spraying process, the fiber can be separated from the ultra-high performance concrete mixture. By adding starch ether, the ultra-high performance concrete mixture can be made thixotropic, which is conducive to spraying construction. The fiber can be fully mixed with the ultra-high performance concrete during the spraying process, so that the fiber volume rate in the ultra-high performance concrete exterior wall decorative panel eventually reaches about 5% to 7%, and the fiber is also oriented, which is conducive to improving the bending resistance of the ultra-high performance concrete exterior wall decorative panel.

[0034] The ultimate bending strength of GRC decorative panels can reach more than 18MPa, while the ultimate bending strength of ultra-high performance concrete exterior wall decorative panels is usually around 12MPa. A single technical means is usually unable to achieve a 50% increase in bending strength. Therefore, the improvement of the bending performance of ultra-high performance concrete exterior wall panels requires the comprehensive use of one or more technical means proposed in the present invention, which can ultimately achieve an ultimate bending strength of ultra-high performance concrete exterior wall panels of more than 20MPa. DETAILED DESCRIPTION

[0035] The specific implementation of the present invention is further described in detail below in conjunction with specific examples.

[0036] Embodiment 1:

[0037] The ultra-high performance concrete used in the production of exterior wall decorative panels of an ultra-high performance concrete exterior wall decorative panel manufacturer in A has a 28d compressive strength of 101.5MPa, a measured prismatic specimen bending strength of 10MPa, and a panel bending ultimate strength of 13MPa. The mix parameters of ultra-high performance concrete are: water-cement ratio 0.18, sand-cement ratio 1.0, silica fume content in cementitious materials 12%, polypropylene crude fiber volume content 2%, of which quartz sand of 40-80 mesh and 80-120 mesh is used, and the ratio of the two is 1:1.

[0038] Due to the low bending strength of ultra-high performance concrete exterior wall decorative panels, a certain proportion of the panels actually produced have longitudinal through cracks during transportation. In order to improve the bending performance of the decorative panels, the following measures were taken: basalt artificial sand with a parent rock compressive strength of 130MPa was used to replace quartz sand. The maximum particle size of basalt artificial sand is 1.2mm. Using this technical method, the compressive strength of the ultra-high performance concrete matrix was increased from 101.5MPa to 123MPa, and the bending strength of the prism test block was increased to 12.7MPa.

[0039] During the pouring process, an inserted vibrator was placed in the ultra-high performance concrete mixture parallel to the direction of the exterior wall panel to vibrate it. The distance between adjacent vibration points was no more than 20 cm, and the diameter of the end of the vibrator was no more than 20 mm. A roller was used to roll the surface of the mixture to remove bubbles inside the mixture, and samples were taken to form bending performance test pieces. After the samples were hardened after vibration, no bubbles were visible to the naked eye. The compressive strength was further increased to 135 MPa, and the bending strength of the prismatic test piece was increased to 14.5 MPa.

[0040] In order to further improve the bending strength of ultra-high performance concrete exterior wall decorative panels, copper-plated fine steel fibers were used to replace polypropylene synthetic crude fibers to prepare ultra-high performance concrete. Since copper-plated fine steel fibers are used in the surface layer, there is a risk of corrosion. In actual production, copper-plated fine steel fibers are used to replace synthetic fibers in the lower 2 / 3 of the ultra-high performance concrete, and synthetic fibers are still used in the surface 1 / 3 of the ultra-high performance concrete. The compressive strength of the ultra-high performance concrete measured by sampling is further increased to 155MPa, and the bending strength of the prism test block is increased to 18.9MPa.

[0041] The above-mentioned ultra-high performance concrete mixture was cast into a sample test block with a length of 250mm, a width of 50mm and a thickness of 10mm. The ultimate flexural strength reached 22MPa, which was 10MPa higher than the initial panel’s ultimate flexural strength of 12MPa, and the flexural strength was increased by 83%, thus greatly avoiding the risk of cracking of ultra-high performance concrete exterior wall decorative panels due to insufficient flexural performance.

[0042] Embodiment 2:

[0043] The ultra-high performance concrete used in the production of exterior wall decorative panels of an ultra-high performance concrete exterior wall decorative panel manufacturer in S has a 28d compressive strength of 110.5MPa, a measured prismatic specimen bending strength of 11.8MPa, and a panel bending ultimate strength of 13MPa. The mix parameters of ultra-high performance concrete are: water-cement ratio 0.19, sand-cement ratio 0.8, silica fume content in cementitious materials 10%, polyvinyl alcohol crude fiber volume content 2.5%, and the sand is quartz sand.

[0044] During the production process of ultra-high performance concrete exterior wall decorative panels, it was found that the strength development of ultra-high performance concrete is slow in winter, and the factory production mold turnover requirements are high, which makes it easy for the decorative panels to crack due to insufficient bending resistance.

[0045] In order to improve the flexural properties of the decorative panels, the quartz sand in the ultra-high performance concrete was replaced by fine aggregate prepared from bauxite clinker, and the silica fume was replaced by white silica fume, a by-product of zirconium smelting. The dosage was increased from 12% to 20%, which can be adjusted to 15% to 20% in the actual production process. In addition, a viscosity-reducing polycarboxylic acid water-reducing agent was used to increase the expansion of the ultra-high performance concrete mixture from 700mm to 800mm, the expansion time was less than 3s, and the inverted slump cone time was less than 25s. The viscosity of the ultra-high performance concrete was greatly reduced, which was conducive to the discharge of bubbles. After sampling and molding, the number of bubbles in the ultra-high performance concrete was reduced by 80%, the compressive strength was increased to more than 120MPa, and the flexural strength of the prismatic specimen was increased to 14.5MPa.

[0046] In order to further improve the bending strength of the ultra-high performance concrete exterior wall decorative panels, the fiber parameters were optimized, and stainless steel fibers were selected to replace polyvinyl alcohol coarse fibers in equal volume. Since the ultra-high performance concrete board thickness is 25mm, the stainless steel fiber length is 20mm, that is, the fiber length is not less than 70% of the board thickness. During pouring, multiple layers are poured from one end to the other end to make the fibers parallel to the board surface direction, thereby improving the orientation of the fibers in the ultra-high performance concrete mixture. Through the above measures, the compressive strength is further increased to 140MPa, and due to the fiber orientation distribution, the bending strength is increased to 21MPa.

[0047] The above-mentioned ultra-high performance concrete mixture was cast into a sample test block with a length of 250mm, a width of 50mm and a thickness of 10mm. The ultimate bending strength reached 23.2MPa, which was 10MPa higher than the initial panel ultimate bending strength of 13MPa, and the bending strength increased by 78%. As the final bending strength was greatly improved, the bending strength in the early production process of the factory was also improved synchronously, which accelerated the factory's production efficiency.

[0048] Embodiment 3:

[0049] The 28d compressive strength of the ultra-high performance concrete used by a manufacturer of ultra-high performance concrete exterior wall decorative panels in Z is 103.5MPa, the measured bending strength of the prism test block is 11.1MPa, and the ultimate bending strength of the panel is 10.5MPa. Due to design requirements, the thickness of the decorative panel needs to be reduced from 30mm to 20mm, and the panel size is changed to a special-shaped structure to achieve light weight and thin walls, which requires a significant improvement in the bending performance of ultra-high performance concrete.

[0050] In order to improve the bending strength of ultra-high performance concrete mixture, the production process is adjusted from casting process to spraying process. First, fly ash micro-beads are used in ultra-high performance concrete mixture to replace 15% cement to reduce the viscosity of ultra-high performance concrete to improve the sprayability of the mixture. Then, starch ether accounting for 0.001% of the mass ratio of cementitious materials is added to stir into a thixotropic mixture and equipped with a fiber shearing device. During construction, the ultra-high performance concrete mixture and fibers are evenly sprayed onto the surface of the formwork through the fiber nozzle and the ultra-high performance concrete mixture nozzle to form an ultra-high performance concrete exterior wall decorative board.

[0051] After adopting the above method, the volume content of synthetic fibers in ultra-high performance concrete was increased from 2% to 3% to about 6%, the prism bending strength reached 17MPa, and the panel ultimate bending strength was increased to 22.5MPa, which was an increase of 114% compared with the initial panel bending ultimate strength of 10.5MPa, realizing the lightweight and thin-walled high-performance concrete exterior wall decorative panels without using steel fibers.

Claims

1. A method for improving the bending resistance of ultra-high performance concrete exterior wall decorative panels, characterized in that: This includes one or more of the following treatment methods: (1) When preparing ultra-high performance concrete premix, high-strength fine aggregate is used to replace quartz sand; (2) Adding viscosity-reducing components to reduce the viscosity of ultra-high performance concrete mixtures; (3) During the pouring process of the ultra-high performance concrete exterior wall panels, a small inserted vibrator is used to tamp the mixture and a roller is used to roll the surface of the mixture to remove bubbles inside the mixture; (4) Using fine steel fibers instead of synthetic coarse fibers to prepare ultra-high performance concrete mixtures; (5) Optimizing fiber parameters to improve fiber orientation in ultra-high performance concrete mixtures; (6) Use spraying technology instead of casting technology to prepare ultra-high performance concrete exterior wall decorative panels.

2. The method for improving the bending resistance of ultra-high performance concrete exterior wall decorative panels according to claim 1, characterized in that: In the treatment method (1), the high-strength fine aggregate is fine aggregate prepared from bauxite clinker or machine-made sand made from granite, andesite or basalt with a parent rock strength of more than 120 MPa.

3. The method for improving the bending resistance of ultra-high performance concrete exterior wall decorative panels according to claim 1, characterized in that: In treatment method (2), the viscosity reducing component is one or a combination of white silica fume, fly ash microspheres and viscosity reducing polycarboxylic acid water reducing agent, wherein the content of white silica fume is 15% to 20%, and the content of fly ash microspheres is 10% to 20%.

4. The method for improving the bending resistance of ultra-high performance concrete exterior wall decorative panels according to claim 3, characterized in that: After viscosity reduction, the expansion of ultra-high performance concrete is in the range of 750 to 850 mm, the expansion time is less than 3 s, and the inverted slump cone time is less than 25 s.

5. The method for improving the bending resistance of ultra-high performance concrete exterior wall decorative panels according to claim 1, characterized in that: In treatment method (3), the end diameter of the vibrating rod is no more than 20 mm, and it is placed in the ultra-high performance concrete mixture parallel to the direction of the exterior wall panel to vibrate it, and the distance between adjacent vibration points is no more than 20 cm.

6. The method for improving the bending resistance of ultra-high performance concrete exterior wall decorative panels according to claim 1, characterized in that: In treatment method (4), when the micro-fiber steel fiber is stainless steel fiber, the stainless steel fiber replaces the synthetic coarse fiber with the same volumetric dosage; when the fine steel fiber is copper-plated steel fiber, the ultra-high performance concrete mixture of the lower 2 / 3 of the plate thickness uses copper-plated steel fiber, and the ultra-high performance concrete mixture of the surface 1 / 3 of the plate thickness still uses synthetic fiber.

7. The method for improving the bending resistance of ultra-high performance concrete exterior wall decorative panels according to claim 1, characterized in that: In treatment method (5), the fiber length is not less than 70% of the board thickness, and during pouring, multiple layers are poured from one end to the other end so that the fibers are parallel to the board surface.

8. The method for improving the bending resistance of ultra-high performance concrete exterior wall decorative panels according to claim 1, characterized in that: In treatment method (6), 0.001% by weight of starch ether is first added to the ultra-high performance concrete premix and stirred into a thixotropic mixture, and a fiber shearing device is provided. During construction, the ultra-high performance concrete mixture and fibers are uniformly sprayed onto the surface of the formwork through the fiber nozzle and the ultra-high performance concrete mixture nozzle to form an ultra-high performance concrete exterior wall decorative panel.