Diamond wire for semiconductor wafer slicing and production method thereof
By removing the sharp edges and plating of diamond powder onto the diamond wire, the problem of hidden cracking of diamond wire in semiconductor wafer cutting is solved, achieving a higher quality cutting effect.
Patent Information
- Application Number
- CN202411329667.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-26
AI Technical Summary
When existing diamond wires cut semiconductor wafers, stress concentration is concentrated due to the sharp edges and angles of diamond powder, which easily lead to hidden crack defects, and cannot be effectively applied to the cutting of high-end semiconductor wafers.
By selecting two diamond powders of different specifications, using large-sized diamond powder as ball abrasive, the small-sized diamond powder is polished to remove sharp edges and corners, and then plating it on the steel wire after nickel plating on the surface to form diamond without sharp edges and corners. Wire.
It effectively avoids the impact of sharp edges and angles of diamond powder on the wafer, and improves the quality and reliability of semiconductor wafer cutting.
Smart Images

Figure CN119017571A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of diamond wire processing, and in particular relates to a diamond wire used for semiconductor wafer slicing and a production method thereof. Background Art
[0002] Nowadays, diamond wire has been widely used in photovoltaic silicon wafer cutting, but cannot be applied to the cutting of high-end semiconductor wafers (such as 12-inch silicon wafers and SiC wafers). The direct reason is that the diamond wire made by the existing process has sharp edges and corners due to the diamond powder solidified on the surface of the diamond wire. During the wafer cutting process, the sharp edges of the diamond powder form stress concentration on the hard and brittle wafer, which easily impacts the hard and brittle wafer and causes defects such as hidden cracks. Therefore, in order to solve this technical problem, we propose a diamond wire for semiconductor wafer slicing and a production method thereof. By first removing the sharp edges of the diamond powder and then plating it on the diamond wire, the sharp edges of the diamond powder during the cutting process can be avoided to avoid impacting the wafer with hidden cracks. Summary of the invention
[0003] The purpose of the present invention is to provide a diamond wire for semiconductor wafer slicing and a production method thereof, so as to solve the problems existing in the background technology.
[0004] In order to achieve the above technical objectives, the technical solution adopted by the present invention is as follows:
[0005] A method for producing a diamond wire for semiconductor wafer slicing comprises the following steps:
[0006] Step S100: Select two diamond micropowders of different specifications, use the large-sized diamond micropowder as a ball abrasive, grind the small-sized diamond micropowder, remove the sharp edges of the small-sized diamond micropowder, and turn it into a small-sized diamond micropowder without sharp edges, and re-sort the diamond micropowder according to specifications;
[0007] Step S200: nickel-plating the surface of the polished small-sized diamond powder;
[0008] Step S300: coating the processed diamond powder on a steel wire to obtain a diamond wire coated with diamond powder without sharp edges.
[0009] In step S100, “re-sorting the diamond powder according to specifications” is specifically as follows:
[0010] The diamond powder after ball milling is subjected to sedimentation sorting by a sedimentation sorting device. The small-sized diamond powder sorted out is used as the raw material for plating on the steel wire, and the large-sized diamond powder is continuously recycled and reused as ball milling material.
[0011] The step S200 includes the following steps:
[0012] Step S210: Diamond powder pretreatment:
[0013] Step S220: performing chemical nickel plating on the surface of diamond powder;
[0014] Step S230: electroplating a layer of nickel on the surface of the chemically plated nickel layer of diamond powder by roller plating.
[0015] The step S210 includes the following steps:
[0016] Step S211: removing oil and impurities on the surface of the diamond powder by using an alkaline degreasing agent or pickling;
[0017] Step S212: using a solution such as dilute nitric acid or dilute hydrochloric acid to roughen the surface of the diamond powder to increase its roughness so as to facilitate the adhesion of subsequent coatings;
[0018] Step S213: immersing the diamond powder in a solution containing a sensitizer such as stannous chloride, so that a layer of easily oxidizable metal ions is adsorbed on the surface of the diamond powder;
[0019] Step S214: activating the sensitized diamond powder with a solution containing an activator such as palladium chloride to further increase the catalytic activity of the surface.
[0020] The step S220 is specifically as follows:
[0021] The pretreated diamond powder is added into a plating solution containing nickel ions, a reducing agent (such as sodium hypophosphite), a chelating agent, a buffer and the like, so that the nickel ions in the plating solution are reduced and deposited on the surface of the diamond powder to form a nickel plating layer.
[0022] In the step S220, the plating solution temperature is 80°C-90°C, and the plating solution is mechanically stirred at a stirring rate of 100rpm-300rpm.
[0023] The rotation speed of the roller for roller plating in step S230 is 8 rpm-15 rpm.
[0024] The step S300 specifically includes the following steps:
[0025] Step S310: treating the surface of the steel wire by using an alkaline degreasing agent or pickling to remove oil stains and impurities on the surface of the steel wire;
[0026] Step S320: preparing the electroplating solution, the raw materials are:
[0027] Nickel sulfamate 600g / L, boric acid 35g / L, nickel chloride 10g / L, add a small amount of auxiliary agent, the auxiliary agent can be a wetting agent sodium dodecyl sulfate and a softener saccharin, and adjust the pH value to 4 to 4.5;
[0028] Step S330: Evenly disperse the sorted diamond powder in the electroplating solution, with the diamond powder as the anode and the steel wire as the cathode, adjust the current density to 0.5A / dm2-2.0A / dm2, and the electroplating temperature to 60°C. Through electrolysis, a metal film is formed on the surface of the diamond powder. This metal film acts as a binder to fix the diamond powder on the steel wire, thereby obtaining a diamond wire plated with diamond powder without sharp edges.
[0029] The invention removes the sharp edges and corners of the diamond micropowder first and then plates the diamond wire, thereby preventing the sharp edges and corners of the diamond micropowder from impacting and causing hidden cracks on the wafer during the cutting process. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The present invention is further illustrated by means of the non-limiting examples given in the accompanying drawings.
[0031] Figure 1 It is a schematic diagram of the main process of the present invention; DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the present invention, the technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0033] A method for producing a diamond wire for semiconductor wafer slicing comprises the following steps:
[0034] Step S100: Select two diamond micropowders of different specifications, use the large-sized diamond micropowder as a ball abrasive, grind the small-sized diamond micropowder, remove the sharp edges of the small-sized diamond micropowder, and turn it into a small-sized diamond micropowder without sharp edges, and re-sort the small-sized diamond micropowder, specifically:
[0035] The diamond powder after ball milling is subjected to sedimentation sorting by a sedimentation sorting device. The small-sized diamond powder sorted out is used as the raw material for plating on the steel wire, and the large-sized diamond powder is continuously recycled and reused as ball milling material.
[0036] Step S200: nickel-plating the surface of the polished small-size diamond powder, specifically:
[0037] Step S210: Pretreatment of diamond powder, specifically:
[0038] Step S211: removing oil and impurities on the surface of the diamond powder by using an alkaline degreasing agent or pickling;
[0039] Step S212: using a solution such as dilute nitric acid or dilute hydrochloric acid to roughen the surface of the diamond powder to increase its roughness so as to facilitate the adhesion of subsequent coatings;
[0040] Step S213: immersing the diamond powder in a solution containing a sensitizer such as stannous chloride, so that a layer of easily oxidizable metal ions is adsorbed on the surface of the diamond powder;
[0041] Step S214: activating the sensitized diamond powder with a solution containing an activator such as palladium chloride to further increase the catalytic activity of the surface;
[0042] Step S220: performing chemical nickel plating on the surface of diamond powder, specifically:
[0043] The pretreated diamond powder is added to a plating solution containing nickel ions, a reducing agent (such as sodium hypophosphite), a chelating agent, a buffer and the like, so that the nickel ions in the plating solution are reduced and deposited on the surface of the diamond powder to form a nickel coating. In this step, the plating solution temperature is 80°C-90°C, and the plating solution is mechanically stirred at a stirring rate of 100rpm-300rpm.
[0044] Step S230: electroplating a layer of nickel on the surface of the chemically plated nickel layer of diamond powder by roller plating. In this step, the roller speed of the roller plating is 8 rpm-15 rpm.
[0045] Step S300: Plating the processed diamond powder on the steel wire to obtain a diamond wire coated with diamond powder without sharp edges and corners, specifically:
[0046] Step S310: treating the surface of the steel wire by using an alkaline degreasing agent or pickling to remove oil stains and impurities on the surface of the steel wire;
[0047] Step S320: preparing the electroplating solution, the raw materials are:
[0048] Nickel sulfamate 600g / L, boric acid 35g / L, nickel chloride 10g / L, add a small amount of auxiliary agent, the auxiliary agent can be a wetting agent sodium dodecyl sulfate and a softener saccharin, and adjust the pH value to 4 to 4.5;
[0049] Step S330: Evenly disperse the sorted diamond powder in the electroplating solution, with the diamond powder as the anode and the steel wire as the cathode, adjust the current density to 0.5A / dm2-2.0A / dm2, and the electroplating temperature to 60°C. Through electrolysis, a metal film is formed on the surface of the diamond powder. This metal film acts as a binder to fix the diamond powder on the steel wire, thereby obtaining a diamond wire plated with diamond powder without sharp edges.
[0050] Example:
[0051] ① Mix diamond powder with a D50 of 8.5 microns and diamond micropowder with a D50 of about 50 microns. The diamond micropowder with a D50 of 50 microns is used as the ball milling material for ball milling. During ball milling, the two specifications of diamond micropowders roll and rub against each other to remove sharp edges. After removing the edges and corners, the particle size of the diamond micropowder will become slightly smaller.
[0052] It should be noted that in the powder metallurgy or micro powder industry, D50 is usually used to describe the particle size specification of micro powder, because a pile of powder micro powder, usually no matter how it is selected, its particle size will not be completely consistent, and often presents a normal distribution. D50 is also called the median diameter or median particle size, which reflects the central trend of the particle size distribution of micro powder. In this example, D50 of 8.5 microns means that in this sample, 50% of the micro powder particles are less than 8.5 microns, and 50% of the micro powder particles are larger than 8.5 microns. D50 of 50 microns means that in this sample, 50% of the micro powder particles are less than 50 microns, and 50% of the micro powder particles are larger than 50 microns.
[0053] ② The diamond powder after ball milling is re-sorted by sedimentation sorting method. The sorted diamond powder with D50 of 8.0 microns is used to plate on the steel wire, and the remaining diamond powder with D50 of 50 microns is further recycled and used as ball milling material.
[0054] ③ The surface of the diamond powder is subjected to pretreatment, chemical nickel plating and electrolytic nickel plating in sequence, and finally plated on a steel wire with a busbar diameter of 0.12 mm to obtain a 0.12 mm diamond wire plated with diamond micropowder without sharp edges. Since the diamond micropowder no longer has sharp edges, when used for high-end semiconductor wafer cutting, it can effectively avoid impact cracking caused by the sharp edges of the diamond micropowder during the wafer cutting process.
[0055] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by those with ordinary knowledge in the technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.
Claims
1. A method for producing a diamond wire for semiconductor wafer slicing, characterized in that: The following steps are included: Step S100: Select two diamond micropowders of different specifications, use the large-sized diamond micropowder as a ball abrasive, grind the small-sized diamond micropowder, remove the sharp edges of the small-sized diamond micropowder, and turn it into a small-sized diamond micropowder without sharp edges, and re-sort the diamond micropowder according to specifications; Step S200: nickel-plating the surface of the polished small-sized diamond powder; Step S300: coating the processed diamond powder on a steel wire to obtain a diamond wire coated with diamond powder without sharp edges.
2. The method for producing a diamond wire for semiconductor wafer slicing according to claim 1, characterized in that: In step S100, "re-sorting the diamond powder according to specifications" is specifically as follows: The diamond powder after ball milling is subjected to sedimentation sorting by a sedimentation sorting device. The small-sized diamond powder sorted out is used as the raw material for plating on the steel wire, and the large-sized diamond powder is continuously recycled and reused as ball milling material.
3. The method for producing a diamond wire for semiconductor wafer slicing according to claim 2, characterized in that: The step S200 includes the following steps: Step S210: Diamond powder pretreatment: Step S220: performing chemical nickel plating on the surface of diamond powder; Step S230: electroplating a layer of nickel on the surface of the chemically plated nickel layer of diamond powder by roller plating.
4. The method for producing a diamond wire for semiconductor wafer slicing according to claim 3, characterized in that: The step S210 includes the following steps: Step S211: removing oil and impurities on the surface of the diamond powder by using an alkaline degreasing agent or pickling; Step S212: using a solution such as dilute nitric acid or dilute hydrochloric acid to roughen the surface of the diamond powder to increase its roughness so as to facilitate the adhesion of subsequent coatings; Step S213: immersing the diamond powder in a solution containing a sensitizer such as stannous chloride, so that a layer of easily oxidizable metal ions is adsorbed on the surface of the diamond powder; Step S214: activating the sensitized diamond powder with a solution containing an activator such as palladium chloride to further increase the catalytic activity of the surface.
5. The method for producing a diamond wire for semiconductor wafer slicing according to claim 4, characterized in that: The step S220 is specifically as follows: The pretreated diamond powder is added into a plating solution containing nickel ions, a reducing agent (such as sodium hypophosphite), a chelating agent, a buffer and the like, so that the nickel ions in the plating solution are reduced and deposited on the surface of the diamond powder to form a nickel plating layer.
6. The method for producing a diamond wire for semiconductor wafer slicing according to claim 5, characterized in that: In step S220, the plating solution temperature is 80°C-90°C, and the plating solution is mechanically stirred at a stirring rate of 100rpm-300rpm.
7. The method for producing a diamond wire for semiconductor wafer slicing according to claim 6, characterized in that: The rotation speed of the roller for roller plating in step S230 is 8 rpm-15 rpm.
8. The method for producing a diamond wire for semiconductor wafer slicing according to claim 7, characterized in that: The step S300 specifically includes the following steps: Step S310: treating the surface of the steel wire by using an alkaline degreasing agent or pickling to remove oil stains and impurities on the surface of the steel wire; Step S320: preparing the electroplating solution, the raw materials are: Nickel sulfamate 600g / L, boric acid 35g / L, nickel chloride 10g / L, add a small amount of auxiliary agent, the auxiliary agent can be a wetting agent sodium dodecyl sulfate and a softener saccharin, and adjust the pH value to 4 to 4.5; Step S330: Plating diamond powder on the surface of the steel wire, specifically, evenly dispersing the sorted diamond powder in the electroplating solution, using the diamond powder as the anode and the steel wire as the cathode, and adjusting the current density to 0.5A / dm 2 -2.0A / dm 2 The electroplating temperature is 60°C. Through electrolysis, a metal film is formed on the surface of the diamond powder. This metal film acts as a binder to fix the diamond powder on the steel wire, thereby obtaining a diamond wire plated with diamond powder without sharp edges.
9. The diamond wire produced by the diamond wire production method for semiconductor wafer slicing according to any one of claims 1 to 8.