Impermeable geosynthetic clay liner and preparation method thereof
By modifying the composite material of bentonite and acrylic water-absorbing resin, a three-dimensional network structure is formed, which solves the problem of poor anti-seepage performance of bentonite waterproof blankets in salt-containing sewage, and significantly improves the anti-seepage performance of the waterproof blankets and the hexavalent chromium ions. The adsorption capacity of the system broadens the scope of application.
Patent Information
- Application Number
- CN202411084280.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Bentonite waterproof blankets have poor anti-seepage performance in salt-containing sewage, resulting in a decrease in waterproofing effect.
Modified bentonite and acrylic water-absorbing resin are used to prepare composite highly absorbent materials, and a three-dimensional network structure is formed by cross-linking of positive and negative charge molecular chains, which improves the density and impermeability of the waterproof blanket, and enhances the salt resistance through the quaternary ammonium salt structure and Adsorption capacity to hexavalent chromium ions.
In a salt-containing sewage environment, the anti-seepage performance and stability of the waterproof blanket is significantly improved, the application scope is broadened, and the hexavalent chromium ions in the sewage has a significant adsorption capacity, which promotes environmental protection and ecological restoration.
Smart Images

Figure BDA0004984717470000061 
Figure BDA0004984717470000071 
Figure BDA0004984717470000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of waterproof blankets, and in particular relates to an anti-seepage bentonite waterproof blanket and a preparation method thereof. Background Art
[0002] Bentonite waterproof blanket (Geosynthetic Clay Lines, GCL) is a composite waterproof material with tiny gaps made by evenly laying bentonite particles between two geotextiles according to certain quality requirements through needle punching and other processes. The geotextile mainly plays a protective role. Bentonite waterproof blanket mainly uses the principle of bentonite swelling when it comes into contact with water. The sodium-based bentonite selected in the waterproof blanket can swell at least dozens of times when it comes into contact with water. The bentonite layer is locked between the two layers of geotextiles by needle-punched fibers, forming a uniform and dense colloid system with high viscosity and a small hydraulic permeability coefficient, which can effectively prevent water.
[0003] Bentonite waterproof blanket has both the excellent properties of geotechnical materials and excellent waterproof and anti-seepage performance. Compared with compacted clay liner, it has the advantages of small size, good flexibility, good sealing performance, high shear strength, simple construction, and adaptability to uneven settlement. It is mainly used in landfills, tailings ponds, hazardous waste dumps, artificial lakes, landscape water systems, underground infrastructure construction and other projects in environmental engineering to solve problems such as sealing, isolation, and anti-seepage. It has good effects and strong anti-destructive properties.
[0004] However, when bentonite waterproof blanket is placed in saline wastewater, due to ion exchange, the molecular structure of bentonite will be destroyed, or the particles cannot stick together, the viscosity is greatly reduced, and the anti-seepage performance of the bentonite waterproof blanket is reduced. Summary of the invention
[0005] The purpose of the present invention is to provide an anti-seepage bentonite waterproof blanket and a preparation method thereof, so as to solve the problem that the existing bentonite waterproof blanket has poor anti-seepage performance in saline sewage.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A permeability-resistant bentonite waterproof blanket comprises a woven fabric and a geotextile, wherein a composite high water-absorbent material is arranged between the woven fabric and the geotextile, and the composite high water-absorbent material comprises 100 parts of modified bentonite and 2-8 parts of acrylic water-absorbent resin in parts by weight.
[0008] The present invention uses modified bentonite and acrylic water-absorbent resin to prepare a composite high water-absorbent material. A large number of molecular chains carrying positive charges exist on the surface of the modified bentonite, and a large number of molecular chains carrying negative charges exist on the surface of the acrylic water-absorbent resin. When the modified bentonite and the acrylic water-absorbent resin absorb water and swell, the modified bentonite and the acrylic water-absorbent resin are cross-linked into a three-dimensional network structure in water due to the mutual attraction between the positive and negative charge molecular chains, thereby improving the density of the internal system of the waterproof blanket, reducing the seepage channels, and promoting a significant improvement in the anti-seepage performance compared with an ordinary bentonite waterproof blanket.
[0009] Further, the modified bentonite is prepared by the following steps:
[0010] Add acrylamide to deionized water, stir and react for 20-30 minutes, then add sodium bentonite, stir for 10-20 minutes and then ultrasonically treat for 30-60 minutes, add N,N'-methylenebisacrylamide, quaternary ammonium polyethyleneimine and potassium persulfate, react at 70-80°C for 2-2.5 hours, cool naturally to room temperature, transfer to an oven and dry at 80-100°C to constant weight, and finally crush and pass through a 40-mesh sieve to obtain modified bentonite.
[0011] With acrylamide as polymerization monomer, N,N'-methylenebisacrylamide as cross-linking agent, quaternary ammonium salt polyethyleneimine as additive, potassium persulfate as initiator, highly absorbent polymer is introduced on the surface of sodium bentonite through polymerization reaction to obtain modified bentonite. Compared with sodium bentonite, the close combination between highly absorbent polymer and sodium bentonite blocks the cation exchange inside bentonite to a certain extent, thereby enhancing the salt resistance of bentonite material. A large number of hydrophilic amino groups and quaternary ammonium salt structures are introduced on the surface of modified bentonite, which can simultaneously combine the two expansion amounts of cationic hydration expansion and hydrophilic functional group water absorption expansion to further improve the expansion performance of modified bentonite. In addition, the introduction of quaternary ammonium salt structure can also improve the adsorption performance of sodium bentonite for hexavalent chromium ions in sewage, which is beneficial to expand the application of bentonite waterproof blanket in chromium (VI)-containing wastewater.
[0012] Furthermore, the dosage ratio of deionized water, acrylamide, sodium bentonite, N,N'-methylenebisacrylamide, quaternary ammonium salt polyethyleneimine and potassium persulfate is 200-300 mL: 15.06-16.86 g: 45 g: 0.05 g: 4.5-5.0 g: 0.3-0.4 g.
[0013] Further, the quaternized polyethyleneimine is prepared by the following steps:
[0014] The branched polyethyleneimine is added into a flask containing anhydrous ethanol, and allyl chloride is added, and the reaction is carried out at 80°C for 24 hours. After the reaction is completed, the anhydrous ethanol is removed by rotary evaporation at 60-80°C, and the rotary evaporation product is placed in a vacuum oven at 80°C for drying for 24 hours. The mass ratio of branched polyethyleneimine to allyl chloride is 8:1.4-2.1, and the Mw of hyperbranched polyethyleneimine is 800. The branched polyethyleneimine containing high-density amine groups is used as a raw material, and allyl chloride is used as a quaternizing agent. The quaternized polyethyleneimine is obtained through a quaternization reaction.
[0015] Further, the acrylic acid water-absorbing resin is prepared by the following steps:
[0016] Acrylic acid, sodium carboxymethyl cellulose and deionized water are mixed evenly, N,N'-methylenebisacrylamide and N-allyl-N'-(sodium aminobenzenesulfonate) thiourea are added, potassium persulfate solution is added dropwise at 60°C, after the addition is completed, the temperature is raised to 70°C for reaction for 2-3h, then the mixture is transferred to an oven and dried at 80-100°C to constant weight, and finally crushed through a 40-mesh sieve to obtain an acrylic acid water-absorbing resin.
[0017] Furthermore, the mass ratio of acrylic acid, sodium carboxymethyl cellulose, deionized water, N,N'-methylenebisacrylamide and N-allyl-N'-(sodium aminobenzenesulfonate) thiourea and potassium persulfate solution is 20g:2.6g:19-20mL:0.04g:2.5-4.5g:10mL, and the potassium persulfate solution is composed of potassium persulfate and deionized water in a dosage ratio of 0.4g:10mL.
[0018] Furthermore, the woven fabric is polypropylene woven fabric or polyethylene woven fabric.
[0019] Furthermore, the geotextile is a non-woven geotextile, the fiber web of the non-woven geotextile is polyester or polypropylene fiber, and the unit area mass is 220g / m 2 .
[0020] The preparation method of the above-mentioned anti-seepage bentonite waterproof blanket comprises the following steps:
[0021] Add modified bentonite and acrylic acid absorbent resin into a stirring tank, stir and mix at 300-500rpm for 30-60min to obtain a composite super absorbent material; spread the composite super absorbent material evenly on a woven cloth, then lay a geotextile, and fix the composite super absorbent material between the woven cloth and the geotextile by needle punching to obtain an anti-seepage bentonite waterproof blanket.
[0022] Beneficial effects of the present invention:
[0023] 1. The present invention provides an anti-seepage bentonite waterproof blanket, which is prepared from a composite highly absorbent material using modified bentonite and acrylic acid absorbent resin, so that the waterproof blanket can maintain excellent anti-seepage performance even in the harsh environment of saline sewage, effectively ensuring the stability and reliability of the waterproof layer, thereby greatly broadening the application scope of the bentonite waterproof blanket under diverse and complex geological and hydrological conditions. At the same time, the waterproof blanket also has a significant adsorption capacity for harmful substances such as hexavalent chromium ions in sewage, further promoting the process of environmental protection and ecological restoration.
[0024] 2. The present invention modifies sodium-based bentonite, and compared with sodium-based bentonite, the expansion performance and salt resistance are greatly improved. In addition, it also has good adsorption performance for hexavalent chromium ions in sewage.
[0025] 3. The present invention uses carboxymethyl cellulose and N-allyl-N'-(sodium aminobenzenesulfonate) thiourea as auxiliary agents, acrylic acid as raw material, and adopts aqueous solution polymerization to obtain an acrylic acid water-absorbing resin, which not only has high water absorption and water retention performance, but also has enhanced salt resistance due to the sodium sulfonate group carried by N-allyl-N'-(sodium aminobenzenesulfonate) thiourea. In addition, N-allyl-N'-(sodium aminobenzenesulfonate) thiourea also carries a thiourea group, which has a good complexing effect on heavy metal ions and also has good adsorption performance for hexavalent chromium ions in sewage. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The sources of the following examples and comparative examples are as follows:
[0028] Branched polyethyleneimine (PEI, M W =800), 99%, Shanghai MacLean Biochemical Technology Co., Ltd.;
[0029] Sodium bentonite, montmorillonite content> 70%, cation exchange capacity of 83.69 cmol / kg, purchased from Liancheng County Henghe Bentonite Co., Ltd.
[0030] Sodium carboxymethyl cellulose, purchased from Guangzhou Yuanda New Materials Co., Ltd., purity ≥99%;
[0031] N-allyl-N'-(sodium aminobenzenesulfonate) thiourea and preparation methods belong to the prior art, for example, "A new method for the synthesis of N-allyl-N'-(sodium aminobenzenesulfonate) thiourea by phase transfer catalysis", Ma Donglan, Wang Yulan, Ding Guosheng, and Li Jianping.
[0032] Example 1
[0033] This embodiment provides a modified bentonite, which is prepared by the following steps:
[0034] Add 15.06 g of acrylamide to 200 mL of deionized water, stir and react for 20 minutes, then add 45 g of sodium bentonite, stir for 10 minutes and then ultrasonically treat for 30 minutes, add 0.05 g of N,N'-methylenebisacrylamide, 4.5 g of quaternary ammonium polyethyleneimine and 0.3 g of potassium persulfate, react at 70°C for 2 hours, cool naturally to room temperature, transfer to an oven and dry at 80°C to constant weight, and finally crush through a 40-mesh sieve to obtain modified bentonite.
[0035] Quaternized polyethyleneimine is prepared by the following steps:
[0036] Add 8 g of branched polyethyleneimine into a flask containing 80 mL of anhydrous ethanol, add 1.4 g of allyl chloride, and react at 80°C for 24 hours. After the reaction is completed, remove the anhydrous ethanol by rotary evaporation at 60°C, and place the rotary evaporation product in a vacuum oven at 80°C and dry it for 24 hours.
[0037] Example 2
[0038] This embodiment provides a modified bentonite, which is prepared by the following steps:
[0039] 16.86 g of acrylamide was added to 300 mL of deionized water, and the mixture was stirred for 30 min. Then, 45 g of sodium bentonite was added, and the mixture was stirred for 20 min and ultrasonically treated for 60 min. Then, 0.05 g of N, N'-methylenebisacrylamide, 5.0 g of quaternary ammonium polyethyleneimine and 0.4 g of potassium persulfate were added, and the mixture was reacted at 80 ° C for 2.5 h. After naturally cooling to room temperature, the mixture was transferred to an oven and dried at 100 ° C to constant weight. Finally, the mixture was crushed and passed through a 40-mesh sieve to obtain modified bentonite.
[0040] Quaternized polyethyleneimine is prepared by the following steps:
[0041] Add 8 g of branched polyethyleneimine into a flask containing 100 mL of anhydrous ethanol, add 2.1 g of allyl chloride, and react at 80°C for 24 hours. After the reaction is completed, remove the anhydrous ethanol by rotary evaporation at 80°C, and place the rotary evaporation product in a vacuum oven at 80°C and dry it for 24 hours.
[0042] Comparative Example 1
[0043] This comparative example provides a modified bentonite. On the basis of Example 1, the quaternary ammonium salt polyethyleneimine in Example 1 is removed, and the remaining raw materials, parameters and preparation process are the same as those in Example 1.
[0044] Comparative Example 2
[0045] This comparative example is sodium bentonite.
[0046] The bentonite provided in Example 1-2 and Comparative Example 1-2 was tested, and the expansion property was carried out according to the "Sodium Bentonite Waterproof Blanket Industry Standard JG / T193-2006" as the standard, and the steps are as follows:
[0047] 1) The samples were sieved (200 mesh) and dried at 105°C for 48 hours to constant weight;
[0048] 2) Add 90 mL of deionized water to a 100 mL measuring cylinder and accurately weigh (2.00 ± 0.01) g of the sample. Add 0.1 g of the sample to the measuring cylinder within 30 seconds each time until the water surface is fully covered. Add the next amount of soil sample after the last addition has completely sunk to the bottom of the measuring cylinder.
[0049] 3) After the sample is completely added, use deionized water to rinse the soil sample attached to the inner wall of the measuring cylinder, and add deionized water to 100 mL;
[0050] 4) After the sample is left to stand for 24 hours, read the volume of the soil sample in the measuring cylinder. During the reading process, the low-density flocs attached to the upper layer should be ignored, and the expansion index m is calculated based on the top of the soil. F , the results are shown in Table 1;
[0051] The salt resistance is tested by the expansion performance system of the sample in different ion type solutions. The test method refers to the above expansion test, and the deionized water is replaced by 20mmol / L NaCl and 20mmol / L CaCl2 solutions respectively. The expansion index m F ;The results are shown in Table 1;
[0052] Table 1
[0053]
[0054]
[0055] It can be seen from the data recorded in Table 1 that the swelling properties of the modified bentonites in Examples 1-2 and Comparative Example 1 are greatly improved in water and salt solutions compared to the original sodium-based bentonite in Comparative Example 2, and Examples 1-2 are significantly better than Comparative Example 1.
[0056] Example 3
[0057] A permeability-resistant bentonite waterproof blanket comprises a woven fabric and a geotextile, wherein a composite high water-absorbent material is arranged between the woven fabric and the geotextile, and the composite high water-absorbent material comprises, by weight, 100 parts of the modified bentonite of Example 1 and 2 parts of an acrylic water-absorbent resin.
[0058] Acrylic water-absorbing resin is prepared by the following steps:
[0059] 20g acrylic acid, 2.6g sodium carboxymethyl cellulose and 19mL deionized water were stirred and mixed for 30min, 0.04g N,N'-methylenebisacrylamide and 2.5g N-allyl-N'-(sodium aminobenzenesulfonate) thiourea were added, 10mL potassium persulfate solution was added dropwise at 60°C, after the addition was completed, the temperature was raised to 70°C for reaction for 2h, then transferred to an oven and dried at 80°C to constant weight, and finally crushed through a 40-mesh sieve to obtain an acrylic acid water-absorbing resin. The potassium persulfate solution was composed of potassium persulfate and deionized water in a dosage ratio of 0.4g:10mL.
[0060] The woven fabric is polypropylene woven fabric.
[0061] The geotextile is a non-woven geotextile. The fiber mesh of the non-woven geotextile is polyester, and the unit area mass is 220g / m 2 .
[0062] The preparation method of the above-mentioned anti-seepage bentonite waterproof blanket comprises the following steps:
[0063] Add modified bentonite and acrylic acid absorbent resin into a stirring tank, stir and mix at 300 rpm for 30 minutes to obtain a composite super absorbent material; spread the composite super absorbent material evenly on the woven cloth, then lay the geotextile, and use the needle punching method to fix the composite super absorbent material between the woven cloth and the geotextile, so as to obtain a 3mm thick and 4000g / m2 unit area mass. 2 Anti-seepage bentonite waterproof blanket.
[0064] Example 4
[0065] A permeability-resistant bentonite waterproof blanket comprises a woven fabric and a geotextile, wherein a composite super absorbent material is arranged between the woven fabric and the geotextile, and the composite super absorbent material comprises, by weight, 100 parts of the modified bentonite of Example 2 and 5 parts of an acrylic water-absorbing resin.
[0066] Acrylic water-absorbing resin is prepared by the following steps:
[0067] 20g acrylic acid, 2.6g sodium carboxymethyl cellulose and 19mL deionized water were stirred and mixed for 40min, 0.04g N,N'-methylenebisacrylamide and 3.2g N-allyl-N'-(sodium aminobenzenesulfonate) thiourea were added, 10mL potassium persulfate solution was added dropwise at 60°C, after the addition was completed, the temperature was raised to 70°C for reaction for 2.5h, then transferred to an oven and dried at 90°C to constant weight, and finally crushed through a 40-mesh sieve to obtain an acrylic acid water-absorbing resin. The potassium persulfate solution was composed of potassium persulfate and deionized water in a dosage ratio of 0.4g:10mL.
[0068] The woven fabric is polyethylene woven fabric.
[0069] The geotextile is a non-woven geotextile. The fiber mesh of the non-woven geotextile is polypropylene fiber, and the unit area mass is 220g / m 2 .
[0070] The preparation method of the above-mentioned anti-seepage bentonite waterproof blanket comprises the following steps:
[0071] The modified bentonite and acrylic acid absorbent resin were added into a stirring tank and stirred at 500 rpm for 60 min to obtain a composite super absorbent material; the composite super absorbent material was evenly spread on the woven cloth, and then the geotextile was laid, and the composite super absorbent material was fixed between the woven cloth and the geotextile by needle punching to obtain a 3 mm thick and 4000 g / m2 unit area mass. 2 Anti-seepage bentonite waterproof blanket.
[0072] Example 5
[0073] A permeability-resistant bentonite waterproof blanket comprises a woven fabric and a geotextile, wherein a composite super absorbent material is arranged between the woven fabric and the geotextile, and the composite super absorbent material comprises 100 parts of the modified bentonite of Example 2 and 8 parts of acrylic water-absorbing resin in parts by weight.
[0074] Acrylic water-absorbing resin is prepared by the following steps:
[0075] 20g acrylic acid, 2.6g sodium carboxymethyl cellulose and 20mL deionized water were stirred and mixed for 60min, 0.04g N,N'-methylenebisacrylamide and 4.5g N-allyl-N'-(sodium aminobenzenesulfonate) thiourea were added, 10mL potassium persulfate solution was added dropwise at 60°C, after the addition was completed, the temperature was raised to 70°C for reaction for 3h, then transferred to an oven and dried at 100°C to constant weight, and finally crushed through a 40-mesh sieve to obtain an acrylic acid water-absorbing resin. The potassium persulfate solution was composed of potassium persulfate and deionized water in a dosage ratio of 0.4g:10mL.
[0076] The woven fabric is polypropylene woven fabric.
[0077] The geotextile is a non-woven geotextile. The fiber mesh of the non-woven geotextile is polyester, and the unit area mass is 220g / m 2 .
[0078] The preparation method of the above-mentioned anti-seepage bentonite waterproof blanket comprises the following steps:
[0079] The modified bentonite and acrylic acid absorbent resin were added into a stirring tank and stirred at 500 rpm for 30 min to obtain a composite super absorbent material; the composite super absorbent material was evenly spread on the woven cloth, and then the geotextile was laid, and the composite super absorbent material was fixed between the woven cloth and the geotextile by needle punching to obtain a 3 mm thick and 4000 g / m2 unit area mass. 2 Anti-seepage bentonite waterproof blanket.
[0080] Comparative Example 3
[0081] A permeability-resistant bentonite waterproof blanket is prepared in Example 3, wherein the modified bentonite in Example 3 is replaced by the product prepared in Comparative Example 1, and the remaining raw materials and preparation process are the same as those in Example 3.
[0082] Comparative Example 4
[0083] A permeability-resistant bentonite waterproof blanket is prepared based on Example 3, wherein the modified bentonite in Example 3 is replaced by the material in Comparative Example 2, and the remaining raw materials, parameters and preparation process are the same as those in Example 3.
[0084] Comparative Example 5
[0085] A permeability-resistant bentonite waterproof blanket is prepared by removing N-allyl-N'-(sodium aminobenzenesulfonate) thiourea in the preparation process of acrylic acid water-absorbing resin on the basis of Example 3, and the remaining raw materials, parameters and preparation process are the same as those in Example 3.
[0086] Comparative Example 6
[0087] A permeability-resistant bentonite waterproof blanket is prepared by removing the propionic acid absorbing resin from Example 3, and the remaining raw materials, parameters and preparation process are the same as those of Example 3.
[0088] The bentonite waterproof blankets obtained in Examples 3 to 5 and Comparative Examples 3 to 6 were subjected to a performance test, specifically, the permeability coefficient was tested according to the method in the "Sodium Bentonite Waterproof Blanket Industry Standard JG / T193-2006", and then immersed in a 10wt% sodium chloride aqueous solution and a 5mg / L potassium dichromate aqueous solution for 30d, respectively, and the permeability coefficient was tested again. After the immersion was completed, the concentration of Cr(VI) in the remaining solution of the potassium dichromate aqueous solution was tested using an ultraviolet spectrophotometer, and the removal rate of Cr(VI) was calculated. The test results are shown in Table 2:
[0089] Table 2
[0090]
[0091] It can be seen from the data recorded in Table 2 that the permeability coefficient of the bentonite waterproof blanket prepared in Examples 3-5 is 2.6-3.4×10 -12 m / s, and the permeability coefficient after immersion in 10wt% sodium chloride aqueous solution for 30 days was 2.7-3.5×10 -12 m / s, and the permeability coefficient after immersion in 5 mg / L potassium dichromate aqueous solution for 30 days was 2.9-3.9×10 -12 m / s, and the Cr(VI) removal rate is above 99.6%. Compared with comparative examples 3-5, it not only has a smaller permeability coefficient, but also has better salt resistance and Cr(VI) removal rate.
[0092] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0093] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An anti-seepage bentonite waterproof blanket, comprising a woven cloth and a geotextile, wherein a composite high water-absorbent material is arranged between the woven cloth and the geotextile, characterized in that: The composite super absorbent material comprises, by weight, 100 parts of modified bentonite and 2-8 parts of acrylic absorbent resin; Modified bentonite is made by the following steps: Add acrylamide to deionized water, stir and then add sodium bentonite, stir for 10-20 minutes and then ultrasonically treat for 30-60 minutes, add N,N'-methylenebisacrylamide, quaternary ammonium polyethyleneimine and potassium persulfate, react at 70-80°C for 2-2.5 hours, dry, and grind through a 40-mesh sieve to obtain modified bentonite.
2. The anti-seepage bentonite waterproof blanket according to claim 1, characterized in that: The dosage ratio of deionized water, acrylamide, sodium bentonite, N,N'-methylenebisacrylamide, quaternary ammonium salt polyethyleneimine and potassium persulfate is 200-300 mL: 15.06-16.86 g: 45 g: 0.05 g: 4.5-5.0 g: 0.3-0.4 g.
3. The anti-seepage bentonite waterproof blanket according to claim 1, characterized in that: Quaternized polyethyleneimine is prepared by the following steps: The branched polyethyleneimine and anhydrous ethanol are mixed, allyl chloride is added, and the reaction is carried out at 80°C for 24 hours, followed by rotary evaporation to remove the anhydrous ethanol, and the rotary evaporation product is dried; the mass ratio of the branched polyethyleneimine to the allyl chloride is 8:1.4-2.1, and the Mw of the hyperbranched polyethyleneimine is 800.
4. The anti-seepage bentonite waterproof blanket according to claim 1, characterized in that: Acrylic water-absorbing resin is prepared by the following steps: Mix acrylic acid, sodium carboxymethyl cellulose and deionized water evenly, add N,N'-methylenebisacrylamide and N-allyl-N'-(sodium aminobenzenesulfonate) thiourea, add potassium persulfate solution dropwise at 60°C, react at 70°C for 2-3h after the addition is complete, dry at 80-100°C to constant weight, crush and pass through a 40-mesh sieve to obtain an acrylic acid water-absorbing resin.
5. The anti-seepage bentonite waterproof blanket according to claim 4, characterized in that: The mass ratio of acrylic acid, sodium carboxymethyl cellulose, deionized water, N,N'-methylenebisacrylamide and N-allyl-N'-(sodium aminobenzenesulfonate) thiourea and potassium persulfate solution is 20g:2.6g:19-20mL:0.04g:2.5-4.5g:10mL, and the potassium persulfate solution is composed of potassium persulfate and deionized water in a dosage ratio of 0.4g:10mL.
6. The anti-seepage bentonite waterproof blanket according to claim 1, characterized in that: The woven fabric is polypropylene woven fabric or polyethylene woven fabric.
7. The anti-seepage bentonite waterproof blanket according to claim 1, characterized in that: Geotextile is a non-woven geotextile. The fiber mesh of non-woven geotextile is polyester or polypropylene fiber, and the unit area mass is 220g / m 2 .
8. A method for preparing the anti-seepage bentonite waterproof blanket according to any one of claims 1 to 7, characterized in that: The following steps are involved: Modified bentonite and acrylic absorbent resin are mixed to obtain a composite super absorbent material; the composite super absorbent material is evenly spread on a woven cloth, and then a geotextile is laid, and the composite super absorbent material is fixed between the woven cloth and the geotextile by a needle punching method to obtain an anti-seepage bentonite waterproof blanket.
Citation Information
Patent Citations
Super absorbent water-retaining agent and preparation method thereof
CN102167769A
Preparation method for bentonite anti-seepage material
CN102584056A
Light powder geosynthetic clay liner
CN103171182A
Sodium base bentonite waterproof blanket and preparation method thereof
CN105398149A
Preparation method for fire preventing and extinguishing colloid material for coal mines
CN106902487A
Cited By
Water-blocking tape material for optical cable with rapid water swelling performance and preparation method of water-blocking tape material
CN120307722A