Method for synthesizing ZSM-12 / ZSM-5 molecular sieve

By growing ZSM-5 molecular sieves on the outer layer of ZSM-12 molecular sieves to form a coating material, the aggregation problem of ZSM-12 molecular sieves in the hydrothermal synthesis process was solved, and the product selectivity and catalyst activity of the long-chain alkane isomerization reaction were improved.

CN119018908APending Publication Date: 2024-11-26CHINA UNIV OF PETROLEUM (BEIJING)

Patent Information

Application Number
CN202411120368.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

ZSM-12 molecular sieve exhibits severe aggregation during hydrothermal synthesis, leading to high mass transfer resistance and affecting the product selectivity of long-chain alkane isomerization reactions.

Method used

ZSM-5/ZSM-12 coated materials are produced using a protective agent. By growing ZSM-5 molecular sieves on the outer layer of ZSM-12 molecular sieves, a coated structure is formed, which reduces mass transfer resistance in the pores and increases isomer selectivity.

Benefits of technology

It effectively increases the yield of bibranched isomers in the isomerization reaction of long-chain alkane, reduces the content of light components, and improves the product selectivity of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018908A_ABST
    Figure CN119018908A_ABST
Patent Text Reader

Abstract

The invention discloses a method for synthesizing a ZSM-12 / ZSM-5 molecular sieve. A template agent Q is used as a main structure-directing agent, an organic salt K provides ions to maintain charge balance in the crystallization process, and the pH value is adjusted, so that the gel is in a ZSM-12 crystallization phase region. When a ZSM-12 crystal nucleus is generated in the crystallization process, crystallization is stopped, the material is taken out, a protective agent F is added in the presence of a mother solution, the protective agent F directionally coats the surface of the ZSM-12 molecular sieve, crystallization is continued after the pH value is changed at the same time, the unnucleated raw material can generate the ZSM-5 molecular sieve in the pH value interval, and ZSM-5 can grow around the ZSM-12 due to the action of the protective agent, so that the ZSM-5 molecular sieve is obtained. The ZSM-12 is wrapped inside, so that the mass transfer resistance in pore channels is effectively reduced, and the isomerization selectivity is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of molecular sieve catalytic material synthesis, and in particular relates to a method for synthesizing ZSM-12 / ZSM-5 molecular sieves. Background Art

[0002] ZSM-12 zeolite is a high-silicon zeolite with a one-dimensional twelve-membered ring pore structure. It was first synthesized by Rosinski and Rubin et al. in 1974. The pore size of ZSM-12 zeolite gives it excellent catalytic performance in isomerization, hydrocarbon cracking and conversion. However, due to the serious agglomeration of the molecular sieve during the hydrothermal synthesis process, it increases the mass transfer resistance during the reaction process, resulting in low product selectivity when performing long-chain alkane isomerization reactions.

[0003] ZSM-5 zeolite is a zeolite molecular sieve with a three-dimensional pore structure. The unit cell parameters are a=2.017nm, b=1.996nm, c=1.343nm. ZSM-5 molecular sieve is widely used in cracking reactions due to its acidity and pore structure.

[0004] In recent years, in order to solve the mass transfer problem of ZSM-12, many patents have proposed corresponding solutions.

[0005] Patent CN 113880110A provides a method for preparing nano-multi-level porous MOR / MTW molecular sieves. Its innovation lies in using a eutectic method to produce multi-level porous materials and applying the molecules to the isomerization of alkylbenzenes. However, this method does not produce coated materials. Compared with eutectic materials, the advantages of coated materials are that they can effectively reduce the agglomeration and sintering of nanoparticles, thereby alleviating the carbon deposition problem; and they can be precisely controlled during the synthesis process, providing more possibilities for optimizing catalytic performance.

[0006] Patent CN115709095A introduces a method for synthesizing a ZSM-12 / ZSM-5 eutectic molecular sieve. The innovation of this patent is to provide a method for preparing a highly active toluene disproportionation catalyst for producing benzene. The catalyst prepared by this method has the characteristics of high toluene conversion rate, high benzene selectivity and high stability. Compared with patent CN 113880110 A, firstly, the eutectic material synthesized by them is different. Secondly, its application is different from that of patent CN 113880110A.

[0007] Patent CN104591217A discloses a Beta / ZSM-12 composite molecular sieve and its synthesis method, which introduces glucose into the microporous channels of the ZSM-12 molecular sieve, converts it into carbon through roasting, occupies the channels of the ZSM-12 molecular sieve, prevents alkali from entering the ZSM-12 molecular sieve crystal, and prevents the ZSM-12 molecular sieve from being destroyed during the crystallization reaction, thereby maintaining the integrity of the crystal structure. It uses glucose to burn into carbon and then prepares Beta. Although this method can ensure the integrity of the ZSM-12 molecular sieve, carbon is not easy to remove in the channels, which easily causes a decrease in the activity of the molecular sieve.

[0008] Patent CN106587094A discloses the preparation of a blocky Beta / ZSM-12 intergrowth molecular sieve, which uses a solvent evaporation method. The material particles are blocky and have a multi-level pore structure. It is not a coating material. Compared with the coating material, it is impossible to see the different structural characteristics of the two molecular sieves from the scanning electron microscope, and the morphology cannot be accurately controlled.

[0009] Patent CN104549466A discloses an in-situ synthesized ZSM-5 / Beta symbiotic molecular sieve catalyst and a preparation method thereof. In this method, an aluminum source, a Beta molecular sieve, a silicon source and water are mixed in a certain proportion and sprayed to form spray-coated microspheres. The microspheres, an alkali source, an aluminum source, a template and water are mixed in a certain proportion and subjected to hydrothermal treatment to obtain a catalyst containing ZSM-5 and Beta symbiotic molecular sieves. Summary of the invention

[0010] In view of the problem that the mass transfer resistance of ZSM-12 molecular sieve is large and the product selectivity is low at the current stage, the present invention uses a protective agent to produce a ZSM-5 / ZSM-12 coated material, and adds an outer layer of ZSM-5 molecular sieve on the basis of ZSM-12 isomerization. The catalyst using the ZSM-5 / ZSM-12 molecular sieve as a carrier increases the product of double-branched isomers in the isomerization reaction of long-chain alkanes. Compared with the evaluation using ZSM-5 molecular sieve alone, the content of light components is reduced.

[0011] To achieve the above objectives, the present invention provides a method for preparing a ZSM-12 / ZSM-5 molecular sieve.

[0012] The preparation method of the ZSM-12 / ZSM-5 molecular sieve provided by the present invention comprises the following steps:

[0013] (1) First, dissolve the aluminum source Y in water and stir until a clear solution is obtained;

[0014] (2) dissolving the inorganic salt K in water, stirring until a clear solution is obtained, and then dropwise adding the solution to the clear solution obtained in step (1) to obtain a mixed solution;

[0015] (3) quickly adding the template Q to the mixed solution obtained in step (2);

[0016] (4) Adjust the pH value to 12.3-13.0;

[0017] (5) Slowly dropwise adding the silicon source X to the mixed solution obtained in step (4) under vigorous stirring, wherein the molar ratio of each material is X:Y (in terms of SiO2 / Al2O3) = 70-200, K:X = 0.01-0.2, and Q:X = 0.2-0.8;

[0018] (6) adding water and mixing evenly to obtain a gel, wherein the molar ratio of H2O to silicon source X in the final gel is controlled to be 8-35:1;

[0019] (7) the obtained gel is crystallized under closed conditions at 150-170° C. for 24-36 h;

[0020] (8) After the crystallized material is taken out, a protective agent F is added and stirred for 5-6 hours, wherein the amount of the protective agent F added is 0.5%-1.5% of the mass of the crystallized material (including the crystal nucleus and the mother liquor);

[0021] (9) adding a solution of an inorganic base M to the mixed turbid solution obtained in step (8) to adjust the pH value to 13.5-14.0;

[0022] (10) Crystallization at 170-180° C. under closed conditions for 10-20 h;

[0023] (11) The crystallized product is washed with water, dried at 100-120°C for 2-3 h, and calcined at 300-550°C for 10-20 h to obtain a ZSM-12 / ZSM-5 molecular sieve.

[0024] In step (1) of the above method, the aluminum source Y is selected from at least one of water-soluble aluminum salts, alkali metal aluminates, aluminum alkoxides and metallic aluminum; preferably, the aluminum source Y is sodium aluminate.

[0025] In step (2) of the above method, the inorganic salt K is selected from sodium chloride and sodium carbonate;

[0026] In step (3) of the above method, the template agent Q is selected from at least one of tetraethylammonium bromide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide and methyltriethylammonium chloride.

[0027] In step (5) of the above method, the silicon source X is selected from at least one of silicon dioxide, alkali metal silicate, and tetraalkyl orthosilicate;

[0028] Specifically, the silicon source X is silicon dioxide;

[0029] Preferably, the silicon dioxide is selected from at least one of silicon dioxide colloidal suspension, silicon dioxide precipitation, and fumed silicon dioxide.

[0030] The silica content in the silica colloidal suspension is 30wt%-40wt%,

[0031] More preferably, the silicon source X is silica sol (silica sol is a type of silica colloidal suspension);

[0032] Preferably, the molar ratio of each material is X:Y=75-150, K:X=0.05-0.18, and Q:X=0.3-0.7.

[0033] In step (8) of the above method, the protective agent F is selected from at least one of cocoyl glutamate TEA salt, dodecyl dimethyl betaine, α-hexadecyl trimethyl betaine, and disodium N-dodecyl iminodipropionate.

[0034] In step (9) of the above method, the inorganic base M is selected from one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide.

[0035] The above method step (1) may further include adding other trivalent element Y1 sources to the obtained clarified solution, wherein the other trivalent element Y1 is selected from at least one of Fe, Ga, and Be, and the molar ratio of the other trivalent element Y1 to the aluminum source Y may be 0.1-1.0:1.

[0036] The ZSM-12 / ZSM-5 molecular sieve prepared by the above method also belongs to the protection scope of the present invention.

[0037] The present invention also provides a catalyst for isomerization reaction of long-chain alkanes, wherein the catalyst uses the above ZSM-12 / ZSM-5 molecular sieve as a carrier.

[0038] In the present invention, template agent Q is the main structure directing agent, organic salt K provides ions to maintain charge balance during crystallization, and pH value is adjusted so that gel is in the crystallization phase region of ZSM-12. After ZSM-12 nuclei are generated during crystallization, crystallization is stopped, material is taken out, and protective agent F is added under the condition of mother liquor. Protective agent F is an amphoteric surfactant, which can form micelles in aqueous solution. Since there are more cations in aqueous solution and some vacancies on the surface of the nuclei are occupied by cations, there are still certain oxygen vacancies. Surfactants form micelle protective layers between water and nuclei through the joint action of positive and negative ions. Protective agent F is directional coated on the surface of ZSM-12 molecular sieve, and crystallization continues after changing pH value at the same time. Unnucleated raw materials will generate ZSM-5 molecular sieves in the pH value interval, and due to the effect of protective agent, ZSM-5 will grow around ZSM-12, wrapping ZSM-12 inside.

[0039] The scheme of the present invention adopts a synthetic method of a composite molecular sieve with a protective agent, composites ZSM-5 and ZSM-12 molecular sieves, and grows the ZSM-5 molecular sieve coated with the ZSM-12 molecular sieve, effectively reducing the mass transfer resistance in the pores and increasing the isomerization selectivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is the XRD pattern of the ZSM-5 / ZSM-12 molecular sieve prepared in Example 1 of the present invention.

[0041] Figure 2 This is a SEM image of ZSM-5 / ZSM-12 prepared in Example 1 of the present invention. The magnification of a is ×10000, and the magnification of b is ×50000.

[0042] Figure 3 This is the SEM image of ZSM-5 prepared in Comparative Example 1 of the present invention.

[0043] Figure 4 This is the SEM image of the product prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0044] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.

[0045] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.

[0046] The sources of raw materials or equipment in the following examples, including raw material names, specifications, manufacturers, etc.

[0047]

[0048] Evaluation and analysis methods:

[0049] XRD tests were performed on a Bruker diffraction instrument using a Cu target K α Light source (λ=0.15432nm), graphite monochromator, tube voltage 40kV, tube current 40mA. Scanning speed in the range of 5-55° is 10° / min. X-ray diffraction card (JCPDS) is used for qualitative analysis.

[0050] Scanning electron microscopy analysis:

[0051] The particle size and surface morphology of the samples were measured using a JEOL JSN-6460LV scanning electron microscope with an acceleration voltage of 30 kV and a magnification of 500 to 20,000 times. A FEI Quanta 200F field scanning electron microscope was used with an acceleration voltage of 30 kV and a magnification of 100 to 50,000 times.

[0052] Example 1

[0053] (1) First, dissolve 0.25 g of sodium aluminate in water and stir until a clear solution is obtained;

[0054] (2) dissolving 0.06 g of sodium chloride in water, stirring until a clear solution is obtained, and then dropwise adding the solution to the clear solution in step (1) to obtain a mixed solution;

[0055] (3) adding 19.09 g of tetraethylammonium hydroxide (concentration 35%) to the mixed solution in step (2);

[0056] (4) using 1 mol / L sulfuric acid solution to adjust the pH value of the mixed solution to 12.3;

[0057] (5) 16.2 g of 40% silica sol was slowly added dropwise to the mixed solution of step (4) under vigorous stirring; the molar ratio of each material was SiO2 / Al2O3=71, K:X=0.01, Q:X=0.42;

[0058] (6) adding water and mixing evenly to obtain a gel, wherein the molar ratio of H2O to silicon source X in the final gel is 35:1;

[0059] (7) The obtained gel was crystallized under sealed conditions at 150°C for 36 h;

[0060] (8) After the crystallized material is taken out, 1.38 g of TEA cocoyl glutamate is added and stirred for 5 hours. The amount of TEA cocoyl glutamate added is 0.5% of the mass of the crystallized material;

[0061] (9) adding 1 mol / L sodium hydroxide solution to the mixed turbid solution in step (8) to adjust the pH value to 14.0;

[0062] (10) Crystallization at 170°C in a sealed environment for 20 h;

[0063] (11) The crystallized product was washed with distilled water, dried at 120 °C for 2 h, and calcined at 300 °C for 20 h to obtain ZSM-12 / ZSM-5 molecular sieve.

[0064] Figure 1 This is the XRD pattern of the prepared ZSM-5 / ZSM-12 molecular sieve.

[0065] Figure 2 This is the SEM image of the prepared ZSM-5 / ZSM-12.

[0066] Depend on Figure 1 and Figure 2 It can be seen that after the synthesis of ZSM-12, the ZSM-5 molecular sieve grows on the outside and covers the ZSM-12 molecular sieve inside to form a coating material.

[0067] Example 2

[0068] (1) First, dissolve 0.51 g of sodium aluminate in 0.38 g of water and stir until a clear solution is obtained;

[0069] (2) dissolving 2.71 g of sodium chloride in 4.08 g of water, stirring until a clear solution is obtained, and then dropwise adding the solution to the clear solution in step (1) to obtain a mixed solution;

[0070] (3) adding 9.83 g of an aqueous solution prepared with tetraethylammonium bromide to the mixed solution in step (2);

[0071] (4) adjusting the pH value of the mixed solution to 13.0 using 1 mol / L sulfuric acid solution;

[0072] (5) 46.35 g of 30% silica sol was slowly added dropwise to the mixed solution of step (4) under vigorous stirring; the molar ratio of each material was X:Y=100, K:X=0.2, Q:X=0.2;

[0073] (6) After uniform mixing, a gel is obtained, wherein the molar ratio of H2O to silicon source X in the final gel is 8.2:1;

[0074] (7) The obtained gel was crystallized under sealed conditions at 170°C for 24 h;

[0075] (8) After the crystallized material is taken out, 3.05 g of dodecyl dimethyl betaine is added and stirred for 6 hours. The amount of dodecyl dimethyl betaine added is 1.5% of the mass of the crystallized material;

[0076] (9) adding 1 mol / L sodium hydroxide solution to the mixed turbid liquid in step (8) to adjust the pH value to 13.5;

[0077] (10) Crystallization at 180°C in a sealed environment for 10 h;

[0078] (11) The crystallized product was washed with distilled water, dried at 120 °C for 2 h, and calcined at 550 °C for 20 h to obtain ZSM-12 / ZSM-5 molecular sieve.

[0079] Example 3

[0080] (1) First, dissolve 0.12 g of sodium aluminate in 2 g of water and stir until a clear solution is obtained;

[0081] (2) dissolving 1.36 g of sodium chloride in 3 g of water, stirring until a clear solution is obtained, and then dropwise adding the clear solution in step (1) to obtain a mixed solution;

[0082] (3) adding 19.10 g of an aqueous solution prepared with methyltriethylammonium chloride to the mixed solution in step (2);

[0083] (4) using 1 mol / L sulfuric acid solution to adjust the pH value of the mixed solution to 12.6;

[0084] (5) 23.17 g of 40% silica sol was slowly added dropwise to the mixed solution of step (4) under vigorous stirring; the molar ratio of each material was X:Y=200, K:X=0.15, Q:X=0.8;

[0085] (6) adding 31.082 g of water and mixing evenly to obtain a gel, wherein the molar ratio of H2O to silicon source X in the final gel is 25:1;

[0086] (7) The obtained gel was crystallized under sealed conditions at 165°C for 34 h;

[0087] (8) After the crystallized material is taken out, 0.508 g of disodium N-dodecyl imino dipropionate is added and stirred for 6 hours. The amount of disodium N-dodecyl imino dipropionate added is 0.5% of the mass of the crystallized material;

[0088] (9) Add 1 mol / L potassium hydroxide solution to the mixed turbid solution in step (8) and adjust the pH value to 13.7.

[0089] (10) Crystallization at 180°C in a sealed environment for 15 h;

[0090] (11) The crystallized product was washed with distilled water, dried at 120 °C for 2 h, and calcined at 500 °C for 20 h to obtain ZSM-12 / ZSM-5 molecular sieve.

[0091] Example 4

[0092] (1) First, dissolve 0.25 g of sodium aluminate and 0.41 g of gallium nitrate in 5 g of water and stir until a clear solution is obtained;

[0093] (2) dissolving 1.76 g of sodium chloride in 2 g of water, stirring until a clear solution is obtained, and then adding dropwise the clear solution in step (1) to obtain a mixed solution;

[0094] (3) adding 14.33 g of an aqueous solution prepared with methyltriethylammonium chloride to the mixed solution in step (2);

[0095] (4) adjusting the pH value of the mixed solution to 12.4 using 1 mol / L sulfuric acid solution;

[0096] (5) 34.76 g of 40% silica sol was slowly added dropwise to the mixed solution of step (4) under vigorous stirring; the molar ratio of each material was X:Y=150, K:X=0.13, Q:X=0.4, Y1:Y=0.1;

[0097] (6) adding 7.52 g of water and mixing evenly to obtain a gel, wherein the molar ratio of H2O to silicon source X in the final gel is 12:1;

[0098] (7) The obtained gel was crystallized under sealed conditions at 155°C for 36 h;

[0099] (8) After the crystallized product is taken out, 2.71 g of TEA cocoyl glutamate is added and stirred for 6 hours. The amount added is 1.5% of the total mass of the taken out product plus the mother liquor;

[0100] (9) adding 1 mol / L sodium hydroxide solution to the mixed turbid liquid in step (8) to adjust the pH value to 13.5;

[0101] (10) Crystallization at 175°C under closed conditions for 15 h;

[0102] (11) The crystallized product was washed with distilled water, dried at 120 °C for 2 h, and calcined at 500 °C for 20 h to obtain ZSM-12 / ZSM-5 molecular sieve.

[0103] Example 5

[0104] (1) First, dissolve 0.11 g of sodium aluminate and 0.26 g of ferric nitrate nonahydrate in 3 g of water and stir until a clear solution is obtained;

[0105] (2) dissolving 0.91 g of sodium chloride in 1.5 g of water, stirring until a clear solution is obtained, and then dropwise adding the clear solution in step (1) to obtain a mixed solution;

[0106] (3) adding 7.16 g of an aqueous solution prepared with methyltriethylammonium chloride to the mixed solution in step (2);

[0107] (4) using 1 mol / L sulfuric acid solution to adjust the pH value of the mixed solution to 12.8;

[0108] (5) 11.59 g of 40% silica sol was slowly added dropwise to the mixed solution of step (4) under vigorous stirring; the molar ratio of each material was X:Y=120, K:X=0.2, Q:X=0.6, Y1:Y=0.5;

[0109] (6) adding 41.537 g of water and mixing evenly to obtain a gel, wherein the molar ratio of H2O to silicon source X in the final gel is 35:1;

[0110] (7) The obtained gel was crystallized under sealed conditions at 155°C for 36 h;

[0111] (8) After the crystallized material is taken out, 1.43 g of TEA cocoyl glutamate is added and stirred for 6 hours. The amount of TEA cocoyl glutamate added is 0.7% of the mass of the crystallized material;

[0112] (9) adding 1 mol / L sodium hydroxide solution to the mixed turbid solution in step (8) to adjust the pH value to 13.8;

[0113] (10) Crystallization at 180°C in a sealed environment for 10 h;

[0114] (11) The crystallized product was washed with distilled water, dried at 120 °C for 2 h, and calcined at 550 °C for 20 h to obtain ZSM-12 / ZSM-5 molecular sieve.

[0115] Comparative Example 1

[0116] (1) First, dissolve 0.25 g of sodium aluminate in water and stir until a clear solution is obtained;

[0117] (2) dissolving 0.06 g of sodium chloride in water, stirring until a clear solution is obtained, and then dropwise adding the solution to the clear solution in step (1) to obtain a mixed solution;

[0118] (3) adding 19.09 g of tetraethylammonium hydroxide to the mixed solution in step (2);

[0119] (4) 16.2 g of 40% silica sol was slowly added dropwise to the mixed solution of step (4) under vigorous stirring; the molar ratio of each material was X:Y=71, K:X=0.01, Q:X=0.42;

[0120] (5) adding water and mixing evenly to obtain a gel, wherein the molar ratio of H2O to silicon source X in the final gel is 35:1;

[0121] (6) The obtained gel was crystallized under sealed conditions at 150°C for 36 h;

[0122] (7) After the crystallized product is taken out, 1.38 g of TEA cocoyl glutamate is added and stirred for 5 hours. The amount added is 0.5% of the total mass of the taken out product plus the mother liquor.

[0123] (8) adding 1 mol / L sodium hydroxide solution to the mixed turbid solution in step (7) to adjust the pH value to 14.0;

[0124] (9) Crystallization at 170°C in a sealed condition for 20 h;

[0125] (10) The crystallized product was washed with distilled water, dried at 120°C for 2 h, and calcined at 300°C for 20 h; the synthesized product was ZSM-5 molecular sieve. Figure 3 shown.

[0126] Comparative Example 2

[0127] (1) First, dissolve 0.51 g of sodium aluminate in 0.5 g of water and stir until a clear solution is obtained;

[0128] (2) dissolving 2.71 g of sodium chloride in 4.08 g of water, stirring until a clear solution is obtained, and then dropwise adding the clear solution in step (1) to obtain a mixed solution;

[0129] (3) adding 9.82 g of an aqueous solution prepared with tetraethylammonium bromide to the mixed solution in step (2);

[0130] (4) adjusting the pH value of the mixed solution to 13.0 using 1 mol / L sulfuric acid solution;

[0131] (5) 46.35 g of 30% silica sol was slowly added dropwise to the mixed solution of step (4) under vigorous stirring, and the molar ratio of each material was X:Y=100, K:X=0.2, Q:X=0.2;

[0132] (6) After uniform mixing, a gel is obtained, wherein the molar ratio of H2O to silicon source X in the final gel is 8.2:1;

[0133] (7) The obtained gel was crystallized under sealed conditions at 170°C for 24 h;

[0134] (8) taking out the crystallized material, adding 1 mol / L sodium hydroxide solution to the crystallized material, and adjusting the pH value to 13.5;

[0135] (9) Crystallization at 180°C in a sealed environment for 10 h;

[0136] (10) The crystallized product was washed with distilled water, dried at 120°C for 2 h, and calcined at 550°C for 20 h; the synthesized products were ZSM-5 and ZSM-12 molecular sieves, which did not show coating morphology. Figure 4 .

[0137] Table 1 Formulations and test conditions in Examples and Comparative Examples

[0138]

[0139] Example 6. Catalyst Activity Evaluation

[0140] The molecular sieve synthesized by the embodiment and comparative example is used to prepare a catalyst by a loading and extrusion method. The preparation process of the catalyst is as follows: 70% molecular sieve and 30% SB powder, 1% of the total mass of the molecular sieve is added with 1.5mol / L nitric acid for kneading and extrusion to obtain a catalyst carrier (tetraamine platinum is loaded by impregnation method, and the model compound is normal dodecane. The activity evaluation process conditions are: evaluation temperature 315°C, pressure 8Mpa, hydrogen-to-material ratio 290, and the conversion performance of the catalyst is evaluated under the same reaction conditions. The results show that the coated ZSM-5 / ZSM-12 molecular sieve is more conducive to the diffusion of raw materials, making the dibranched isomer conversion rate higher (referring to a higher DM-C12 yield). Compared with the catalyst prepared by the molecular sieve synthesized in Comparative Example 2, the yield of DM-C12 is higher and the product selectivity is also higher.

[0141] Table 2. Catalyst activity evaluation

[0142]

[0143]

[0144] Note: Pt0.5 / ZSM-12 was prepared by the following method: pure phase ZSM-12 molecular sieve was used to prepare the catalyst by loading and extrusion. The preparation process of the catalyst is as follows: 70% molecular sieve and 30% SB powder were added with 1.5mol / L nitric acid, which was 1% of the total mass of the molecular sieve, and kneaded and extruded to obtain a catalyst carrier, which was loaded with tetraamine platinum by impregnation method, and then calcined at 200℃ in a muffle furnace for 6 hours.

[0145] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, and without the need to carry out unnecessary experimental conditions, the present invention can be implemented in a wide range under equivalent parameters, concentrations and conditions. Although the present invention provides specific embodiments, it should be understood that the present invention can be further improved. In a word, according to the principles of the present invention, the application is intended to include any changes, uses or improvements to the present invention, including departure from the disclosed scope in the application, and changes made with conventional techniques known in the art.

Claims

1. A method for preparing a ZSM-12 / ZSM-5 molecular sieve, comprising the following steps: (1) First, dissolve the aluminum source Y in water and stir until a clear solution is obtained; (2) dissolving the inorganic salt K in water, stirring until a clear solution is obtained, and then dropwise adding the solution to the clear solution obtained in step (1) to obtain a mixed solution; (3) quickly adding the template Q to the mixed solution obtained in step (2); (4) Adjust the pH value to 12.3-13.0; (5) Slowly adding the silicon source X dropwise to the mixed solution obtained in step (4) under vigorous stirring, wherein the molar ratio of each material is X:Y=70-200, K:X=0.01-0.2, Q:X=0.2-0.8; (6) adding water and mixing evenly to obtain a gel, wherein the molar ratio of H2O to silicon source X in the final gel is controlled to be 8-35:1; (7) the obtained gel is crystallized under closed conditions at 150-170° C. for 24-36 h; (8) After the crystallized material is taken out, a protective agent F is added and stirred for 5-6 hours, wherein the amount of the protective agent F added is 0.5%-1.5% of the mass of the crystallized material; (9) adding a solution of an inorganic base M to the mixed turbid solution obtained in step (8) to adjust the pH value to 13.5-14.0; (10) crystallization at 170-180°C in a sealed condition for 10-20h; (11) The crystallized product is washed with water, dried at 100-120°C for 2-3 h, and calcined at 300-550°C for 10-20 h to obtain a ZSM-12 / ZSM-5 molecular sieve.

2. The preparation method according to claim 1, characterized in that: In step (1), the aluminum source Y is selected from at least one of water-soluble aluminum salts, alkali metal aluminates, aluminum alkoxides and metallic aluminum.

3. The preparation method according to claim 1, characterized in that: In step (2), the inorganic salt K is selected from sodium chloride and sodium carbonate; In step (3), the template agent Q is selected from at least one of tetraethylammonium bromide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, and methyltriethylammonium chloride.

4. The preparation method according to claim 1, characterized in that: In step (5), the silicon source X is selected from at least one of silicon dioxide, alkali metal silicate, and tetraalkyl orthosilicate.

5. The preparation method according to claim 1, characterized in that: In step (5), the molar ratio of each material is X:Y=75-150, K:X=0.05-0.18, and Q:X=0.3-0.

7.

6. The preparation method according to claim 1, characterized in that: In step (8), the protective agent F is selected from at least one of cocoyl glutamate TEA salt, dodecyl dimethyl betaine, α-hexadecyl trimethyl betaine, and disodium N-dodecyl iminodipropionate.

7. The preparation method according to claim 1, characterized in that: In step (9), the inorganic base M is selected from one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide.

8. The preparation method according to claim 1, characterized in that: Step (1) further comprises adding other trivalent element Y1 sources to the obtained clarified solution, wherein the other trivalent element Y1 is selected from at least one of Fe, Ga, and Be, and the molar ratio of the other trivalent element Y1 to the aluminum source Y is 0.1-1.0:

1.

9. ZSM-12 / ZSM-5 molecular sieve prepared by the method according to any one of claims 1 to 8.

10. A catalyst for isomerization reaction of long-chain alkanes, wherein the catalyst uses the ZSM-12 / ZSM-5 molecular sieve according to claim 9 as a carrier.

Citation Information

Patent Citations

  • Highly-stable small-grain NaY molecular sieve

    CN103449470A

  • ZSM-5 / ZSM-12 composite molecular sieve and synthetic method thereof

    CN104591216A

  • ZSM-12 molecular sieve and preparation method thereof

    CN115959678A

Cited By

  • EMT / TS-1 mixed crystal molecular sieve, preparation method thereof and application of EMT / TS-1 mixed crystal molecular sieve in polyethylene waste hydrocracking

    CN120838472A