Method for producing purified precipitated calcium carbonate from lime sludge

Through heating aging, flotation and black-removing carbon treatment of lip slurry, purified precipitated calcium carbonate suitable for the paper industry is formed, which solves the problem that lip slurry cannot be reused in the paper industry and improves resource utilization and product performance.

CN119018924APending Publication Date: 2024-11-26SPECIALTY MINERALS MICHIGAN INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411136445.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-10-22
Filing Date
2020-10-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Limestone is difficult to directly use as fillers and pigments for paper and cardboard due to its low whiteness, low brightness, large particle size and high pH value, and contains residual caustic soda and high surface area siliceous minerals, and may contain black carbon impurities. , resulting in the inability to effectively reuse it in the paper industry, resulting in waste of resources.

Method used

By mixing the lip slurry with water and sodium carbonate, heating and aging, separating the solid parts, adjusting the pH, removing impurities and black carbon, grinding using flotation tanks, hydrocyclones, trapping tanks, ozone treatments and flotation methods To a suitable particle size, a purified precipitated calcium carbonate dispersed slurry is formed, suitable for use as fillers and pigments for paper and paperboard.

Benefits of technology

Purification of limestone has been achieved, the specific surface area and impurity content has been reduced, black charcoal has been removed, and the whiteness and brightness of the product has been improved. It is suitable as a filler and pigment in the paper industry, which has improved the utilization rate of lime and reduced minerals. The demand for fillers and pigments supports the goal of the circular economy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018924A_ABST
    Figure CN119018924A_ABST
Patent Text Reader

Abstract

A method of making purified precipitated calcium carbonate from lime mud can include mixing a lime mud cake with water and sodium carbonate to form a first slurry; heating the first slurry under conditions to age the slurry and form one or more of calcium hydroxide, sodium calcium carbonate, and monoclinic natrolite; separating a solid fraction from the aged slurry; washing the solids fraction under conditions sufficient to decompose one or more of the calcium water alkali, the sodium carbonate calcium stone and the monoclinic sodium calcium stone into a Ca CO3 solid fraction and a Na2CO3 solid fraction and remove the sodium salt, and washing the solid fraction under conditions sufficient to decompose one or more of the calcium water alkali, the sodium carbonate calcium stone and the monoclinic sodium calcium stone into the Ca CO3 solid fraction and the Na2CO3 solid fraction; and mixing the CaCO3 solid fraction with water and a dispersant to disperse the CaCO3 solid fraction in water and form a dispersed slurry having a Brookfield viscosity of less than about 1000 cps at 100 rpm, thereby producing a dispersed slurry containing the purified precipitated calcium carbonate.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Description of the case

[0002] This application is a divisional application of the invention patent application with an application date of October 16, 2020, national application number 202080073177.8, and invention name “Method for preparing purified precipitated calcium carbonate from lime mud”. Technical Field

[0003] The present disclosure relates generally to methods of processing lime mud cake produced as a waste product to produce precipitated calcium carbonate, and specifically to methods for processing lime mud cake produced as a waste product to produce precipitated calcium carbonate suitable for use as a filler and / or pigment in paper and paperboard. Background Art

[0004] The main component in paper and paperboard is cellulose pulp fibers produced from wood or other plant sources by various mechanical and / or chemical pulping processes. The main chemical pulping process used in the paper industry is the alkaline "kraft" process, which uses sodium hydroxide (caustic soda) and sodium sulfide in the cooking process step to extract and separate non-cellulosic materials from the cellulose pulp fibers. In particular, another common variation of pulping is without sodium sulfide, and this is called caustic pulping.

[0005] In order to maximize the operational and economic efficiency of the pulping process, as many chemicals as possible are recovered and reused. In this chemical recovery process, some pulping operations include a lime kiln. The lime kiln is used to produce lime (CaO) which is combined (slaked) with "green liquor" in a process called causticization. Green liquor originates from the pulping process between pulping and causticization. If a lime kiln does not exist, commercial lime (CaO) is purchased and used in a single-pass causticization loop.

[0006] The main chemical component of green liquor is sodium carbonate, and lime reacts with sodium carbonate to produce sodium hydroxide (caustic soda) and calcium carbonate (CaCO3) via the following reaction steps:

[0007] CaO+H2O→Ca(OH)2(1)

[0008] Ca(OH)2+Na2CO3→CaCO3+2NaOH(2)

[0009] The calcium carbonate produced in step 2 is referred to in the industry as "lime mud," while the sodium hydroxide (caustic soda) solution is referred to as "white liquor." The reaction conditions in step 2 cause the lime mud to precipitate as relatively large particles that can be quickly separated from the white liquor stream. After washing and filtering, the lime mud is either recycled back to the lime kiln (if present) or disposed of in a landfill. In practice, the system typically includes both recycled and some landfilled purified lime mud.

[0010] Paper and paperboard products often include calcium carbonate as fine particles produced from limestone powder or synthetic precipitates as fillers and / or coating pigments because of its inherent superior whiteness and brightness compared to other mineral pigments. Despite containing calcium carbonate, lime mud is generally not suitable for use as a filler and / or coating pigment in paper and paperboard. Lime mud has relatively low whiteness and brightness. In addition, lime mud generally has a large particle size and an elevated pH due to residual caustic soda. Lime mud produced by pulping non-wood species (such as reeds and straw) generally contains higher levels of high surface area siliceous minerals, which increases the specific surface area of ​​the lime mud particles and makes them unsuitable for use as fillers in conventional papermaking.

[0011] Another hazard of lime mud is that black carbon particles may be mixed with the lime mud particles. Black carbon can originate from combustion in the recovery boiler, which can be carried into green liquor and ultimately into the lime mud produced by causticization of green liquor. Black carbon, which can produce black specks, is highly undesirable in white pigments used for paper. For these reasons, when lime mud is not re-burned in the lime kiln to produce calcium oxide (CaO) for reuse in the causticization step, the lime mud is disposed of in landfills. Even when lime mud is recycled, it may be advantageous to purify more of the lime mud in order to (i) increase pulping capacity, (ii) or clean up the system of non-process elements and improve process efficiency. Summary of the invention

[0012] It would be advantageous if lime mud could be processed to make it suitable for use as a filler and / or coating pigment for paper and paperboard rather than being landfilled. It would also improve the overall utilization of the lime purchased by the paper mill and reduce its consumption of purchased mineral fillers and / or coating pigments. Additionally, refining this lime mud into viable new products supports the global efforts of companies supporting a circular economy, in which waste is minimized and resources are used more efficiently through the reuse, recycling or reuse of materials.

[0013] According to an embodiment of the present disclosure, a method for preparing purified precipitated calcium carbonate from lime mud may include mixing lime mud cake with water and sodium carbonate to form a first slurry; heating the first slurry under certain conditions to age the slurry and form one or more of lime water, sodalite and monoclinic sodalite; separating a solid portion from the aged slurry; washing the solid portion under conditions sufficient to decompose one or more of lime water, sodalite and monoclinic sodalite into a CaCO3 solid fraction and a Na2CO3 solid fraction and remove sodium salts; and mixing the CaCO3 solid fraction with water and a dispersant to disperse the CaCO3 solid fraction in water and form a dispersed slurry having a Brookfield viscosity of less than about 1000 cps at 100 rpm, thereby producing a dispersed slurry containing the purified precipitated calcium carbonate.

[0014] According to an embodiment of the present disclosure, a method for preparing purified precipitated calcium carbonate from lime mud may include mixing lime mud cake with water and a dispersant to form a first slurry having a Brookfield viscosity of less than about 1000 cps at 100 rpm; grinding the first slurry to a median particle size of about 0.4 microns to about 5 microns; phase separating the ground slurry under conditions sufficient to obtain a centrate filtrate slurry containing impurity particles and a paste containing purified calcium carbonate; and diluting the paste in water to a target solids content, thereby producing a dispersed slurry containing the purified precipitated calcium carbonate.

[0015] According to an embodiment of the present disclosure, a method for preparing purified precipitated calcium carbonate from lime mud may include mixing lime mud cake with water to form a first slurry; adjusting the pH of the first slurry to about 10 to about 11; centrifuging the first slurry for a residence time of about 1 minute to about 10 minutes under conditions sufficient to achieve a g-force of about 500 g to about 2000 g to obtain a centrate filtrate slurry containing impurity particles and a paste containing purified calcium carbonate; and mixing the paste with water and a dispersant to form a dispersed slurry having a Brookfield viscosity of less than about 1000 cps at 100 rpm and containing the purified precipitated calcium carbonate.

[0016] According to an embodiment of the present disclosure, a method for preparing purified precipitated calcium carbonate from lime mud comprises mixing lime mud cake with water to form a first slurry; adjusting the pH of the first slurry to about 8 to about 11; mixing the first slurry with a silicate flotation collector compound to form a second slurry; treating the second slurry through a flotation cell system under conditions sufficient to form a concentrated froth containing silicate particulate impurities and a final stage slurry containing CaCO3; washing and separating the final stage slurry into a liquid phase containing excess soluble salts and a paste containing purified CaCO3; and mixing the paste with water to form a dispersed slurry having a viscosity of less than about 100 cps at 100 rpm and containing the purified precipitated calcium carbonate.

[0017] According to an embodiment of the present disclosure, a method for removing black carbon from a starting slurry containing calcium carbonate and black carbon may include flowing the starting slurry into a first hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a first overflow and to leave the calcium carbonate at the bottom to form a first underflow; flowing the first underflow into a second hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a second overflow and to leave the calcium carbonate at the bottom to form a second underflow; flowing the first overflow into a third hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a third overflow and to leave the calcium carbonate at the bottom to form a third underflow; flowing the second underflow into a recovery chamber; flowing the second overflow into the first hydrocyclone; flowing the third underflow into the first hydrocyclone; flowing the third overflow into a fourth hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a fourth overflow and to leave the calcium carbonate at the bottom to form a fourth underflow; flowing the fourth overflow into a waste container; and flowing the fourth underflow into the third hydrocyclone.

[0018] According to an embodiment of the present disclosure, a method for removing black carbon from a starting slurry containing calcium carbonate and black carbon may include flowing the starting slurry into a hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form an overflow and cause the calcium carbonate to remain at the bottom to form an underflow; flowing the overflow into a waste; and flowing the underflow into a recovery chamber.

[0019] According to an embodiment of the present disclosure, a method for removing black carbon from a starting slurry containing calcium carbonate and black carbon may include flowing the starting slurry into a first hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a first overflow and to leave the calcium carbonate at the bottom to form a first underflow; flowing the first underflow into a second hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a second overflow and to leave the calcium carbonate at the bottom to form a second underflow; flowing the first overflow and the second overflow into waste; and flowing the second underflow into a recovery chamber.

[0020] According to an embodiment of the present disclosure, a method for removing black carbon from a starting slurry containing calcium carbonate and black carbon may include loading the starting slurry into a catch tank using a continuous inflow at or near the center of the catch tank; stirring the starting slurry in the catch tank using an agitator at a tip speed of about 0.1 m / sec to about 1.5 m / sec and under conditions sufficient to cause the black carbon particles to rise to the top of the catch tank and cause the calcium carbonate to settle to the bottom of the catch tank, with a residence time of about 4 min to about 10 min; and pumping the calcium carbonate from the bottom of the catch tank to a recovery container.

[0021] According to an embodiment of the present disclosure, a method for removing black carbon from a starting slurry containing calcium carbonate and black carbon may include flowing an ozone-containing gas through the starting slurry at a flow rate of about 0.1 liters / minute to about 2 liters / minute per liter of the starting slurry with an agitator at a tip speed of about 1 m / sec to about 5 m / sec, wherein the black carbon is oxidized by the ozone to form carbon dioxide gas and removed with the gas flow.

[0022] According to an embodiment of the present disclosure, a method for removing black carbon from a starting slurry containing calcium carbonate and black carbon may include mixing the starting slurry with a frother and a flotation collector compound to form a second slurry; treating the second slurry for about 1 min to about 10 min through a flotation device at an airflow of about 1 slpm to about 3 slpm per liter of the second slurry and with an agitator at a tip speed of about 150 m / min to about 500 m / min, the foam overflowing from the flotation device and the final slurry remaining in the flotation device, the foam containing the black carbon and the final slurry containing calcium carbonate; and collecting the final slurry and dispersing the final slurry in water to form a dispersed slurry containing the calcium carbonate.

[0023] In any of the foregoing embodiments of the method of removing black carbon, the starting slurry can be a slurry of purified precipitated carbonate product.For example, the starting slurry can be a slurry of purified precipitated carbonate product produced by any of the methods disclosed herein. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1A is a schematic diagram of a capture tank according to an embodiment of the present disclosure;

[0025] Figure 1B is a schematic diagram of a capture tank according to an embodiment of the present disclosure;

[0026] Figure 2 is a simplified flow diagram showing four hydrocyclones for removing black carbon from waste products.

[0027] Figure 3 Field emission scanning electron microscope images of a lime mud sample are shown at two magnifications. The higher magnification shows how impurities (flakes and very fine particles) are embedded in the calcium carbonate agglomerates. DETAILED DESCRIPTION

[0028] The method of treating lime mud according to embodiments of the present disclosure may include a series of chemical and mechanical treatments. The method according to the present disclosure processes the lime mud waste product into particles of suitable size and purity for use as fillers and / or pigments in paper and paperboard products, and removes undesirable inorganic substances such as mineral silicates and black carbonaceous materials. Precipitated calcium carbonate suitable for use as fillers or pigments may have a median particle size distribution of about 0.5 μm to about 5 μm, about 3 μm to about 1 μm, about 1 μm to about 2 μm, about 2 μm to about 3 μm, about 3 μm to about 5 μm, about 1 μm to about 2 μm, about 3 μm to about 5 μm, about 1 μm to about 2 μm, about 3 μm to about 5 μm, about 1 μm to about 2 μm, about 3 μm to about 2 μm, about 3 μm to about 5 μm, about 1 μm to about 2 ...2 / g to about 20m 2 / g specific surface area, an ISO brightness greater than about 80, and no visible black carbon. Unless otherwise specified, in this article, the median particle size distribution of the precipitated calcium carbonate is measured using a laser scattering instrument (such as Horiba LA-950). Sample preparation for particle size measurement involves mixing with a dispersant polymer (such as poly (acrylic acid)) and then ultrasonic treatment.

[0029] The method for preparing precipitated calcium carbonate from lime mud according to the present disclosure may include removing one or both of impurities with high specific surface area and removing visible black carbon. The method for preparing precipitated calcium carbonate by removing or reducing impurities with high specific surface area and removing visible black carbon may include a two-step process. In an embodiment, the method of the present disclosure may remove high specific surface area materials to produce purified precipitated calcium carbonate. In an embodiment, the method may include further processing the purified precipitated calcium carbonate obtained to remove visible black carbon to further refine the purified precipitated calcium carbonate. In an embodiment, the method of the present disclosure may remove black carbon to produce purified precipitated calcium carbonate.

[0030] High specific surface area impurities may include one or more of silicates, calcium silicate hydrates, hydrotalcite-like compounds, calcium aluminates, calcium phosphates, and amorphous silicates. High specific surface area generally refers to a specific surface area greater than 20 m 2 / g of impurity particles. For example, a high specific surface area material may have a surface area greater than 20m 2 / g to 100m 2 For example, a typical surface area of ​​such high surface area materials is about 40 m 2 / g to about 60m 2 / g.

[0031] Carbon black is a black carbonaceous material that may be present in lime mud. Depending on the source of the lime mud, it may be necessary to treat the lime mud to remove high specific surface area impurities and carbon black. Alternatively, it may be necessary to remove only the carbon black. When used in combination with a method for removing high specific surface area materials, removal of the carbon black may be performed after removal of the high specific surface area materials. Typically, removal of the carbon black is performed to a point where no visible carbon black remains.

[0032] Embodiments of the present disclosure include removal of high surface area impurities by one or more flotation cell methods, thermal aging methods, and phase separation methods. Embodiments of the present disclosure may individually or additionally include removal of visible black carbon by one or more of a hydrocyclone method, a catch tank method, an ozone method, and a flotation method. Any suitable combination of any one or more high surface area impurity removal methods and any one or more visible black carbon removal methods may be used.

[0033] In any of the methods of the present disclosure, lime mud cake may be produced as a waste product in many processes, such as a by-product of kraft pulp mills, sugar beet production, and acetylene production. Lime mud may be a reaction product of lime reacting with green liquor from recovery boiler smelting. The smelt may be from burning kraft process black liquor or soda process (NSSC) black liquor or from chemical mechanical pulping liquor (CMP, CTMP, APMP).

[0034] In any of the methods disclosed herein, the lime mud cake may be washed by mixing the lime mud cake with water to form a first slurry and washing the first slurry to remove caustic soda present in the lime mud cake.

[0035] In any of the methods of the present disclosure where pH adjustment is performed, the pH may be lowered by passing carbon dioxide gas and / or a gas containing carbon dioxide through the slurry. For example, flue gas may be used. Other suitable gases include pure carbon dioxide gas such as from a liquefied source, diluted combustion flue gas, carbon dioxide byproducts from ethanol or petrochemical sources. Flue gas may come from a boiler or kiln having a carbon dioxide content of about 8% to about 30%.

[0036] In any method of the present disclosure for grinding, grinding can be accomplished by any known suitable method for fine grinding. For example, the slurry can be ground by various known grinding techniques such as ball mills, sand mills and media grinders. For example, glass, sand and / or ceramic media can be used to grind the slurry using a vertical or horizontal stirring media grinder. The medium can have a median diameter of about 0.5 mm to about 3 mm. The slurry is ground into a particle size suitable for the intended end use. For example, when treating lime mud to form precipitated calcium carbonate, the method of the present disclosure can include grinding to a median particle size of about 0.5 micron to about 5 microns, about 1 micron to about 2 microns, about 0.5 micron to about 1 micron, about 3 microns to about 5 microns or about 2 microns to about 3 microns. Suitable sizes include a median particle size of about 0.5 micron, 1 micron, 1.5 microns, 2 microns, 2.5 microns, 3 microns, 3.5 microns, 4 microns, 4.5 microns and 5 microns.

[0037] Flotation Cell Method

[0038] In an embodiment, a method for preparing precipitated calcium carbonate from lime mud may include using a flotation cell to remove high surface area impurities from the lime mud. Flotation cell technology is typically used to remove larger particle size impurities having an average particle size of about 50 microns to 500 microns. It has been advantageously found that the method according to the present disclosure can allow the use of flotation cell technology to remove smaller particle size impurities, such as particle sizes of 4 microns to 20 microns. Reference Figure 3, high surface area materials are often combined with calcium carbonate crystals to form agglomerates. It has been surprisingly found that despite this agglomeration, separation of such impurities can be achieved by the flotation cell method of the present disclosure. The skilled person would not expect to use conventional flotation cell technology or even centrifugation to separate such agglomerates without removing or adversely affecting the ability of calcium carbonate.

[0039] The method may include mixing the lime mud cake with water to form a first slurry and adjusting the pH to about 8 to about 11, or about 9 to about 10.5, or about 8 to about 10, or about 8 to about 11. Other suitable pH values ​​include about 8, 8.5, 9, 9.5, 10, 10.5, and 11. The first slurry may then be mixed with a silicate flotation collector compound to form a second slurry and the second slurry may be diluted with water to a solid content of about 5 wt % to about 15 wt % based on the total weight of the second slurry. Alternatively, a solid content of about 5 wt % to about 15 wt % based on the total weight of the slurry may be achieved by diluting the lime mud cake when it is mixed with water to form the first slurry.

[0040] The second slurry may then be processed through a flotation cell system under conditions sufficient to form a concentrated froth containing silicate particulate impurities and a final slurry containing CaCO3.

[0041] The final pulp can be washed and separated into a liquid phase containing excess soluble salts and a paste containing purified CaCO 3. The paste can be mixed with water and a dispersant to form a dispersed slurry having a viscosity of less than about 1000 cps at 100 rpm.

[0042] The purified precipitated calcium carbonate product produces a dispersed slurry. If required for a particular application, the dispersed slurry can be ground to a median particle size of about 0.5 microns to 5 microns and / or the pH can be adjusted to about 9 to about 10.5 if the pH after grinding is outside this range.

[0043] In embodiments, the first slurry with silicate flotation collector compound can be mixed to a solid content of about 5 wt % to about 40 wt % based on the total weight of the slurry. Other suitable ranges include about 5 wt % to about 20 wt %, about 5 wt % to about 10 wt %, about 20 wt % to about 25 wt %, about 30 wt % to about 40 wt %. Other suitable values ​​include about 5 wt %, 6 wt %, 7 wt %, 8 wt %, 9 wt %, 10 wt %, 12 wt %, 14 wt %, 16 wt %, 18 wt %, 20 wt %, 22 wt %, 24 wt %, 26 wt %, 28 wt %, 30 wt %, 32 wt %, 34 wt %, 36 wt %, 37 wt %, 38 wt % and 40 wt % based on the total weight of the first slurry.

[0044] The silicate flotation collector compound may be an amine-based compound. For example, the silicate flotation collector may be one or more of a primary amine, a dialkylamine, a tertiary amine, and a quaternary amine. Specific examples of compounds include, but are not limited to, tallow, coconut amine, hydroxyethyl alkyl imidazoline, lauryl amine, long chain alkyl pyridinium, and n-alkyl trimethyl ammonium. Silicate flotation collector compounds are commercially available and may include 3135 (Clariant), K2C (Clariant), 1019(Akzo Nobel Surface Chemistry,LLC)、MD 20763(Akzo Nobel)、 1208 (ArrMaz) and DA-17 (Evonik Industries), (AkzoNobel) and (Akzo Nobel) one or more.

[0045] The silicate flotation collector compound may be provided in the first slurry in an amount of about 0.1 wt % to about 0.3 wt % based on the dry mass of the lime mud cake.

[0046] Heat aging method

[0047] According to embodiments, a method for preparing precipitated calcium carbonate from lime mud may include thermally aging the lime mud in sodium carbonate to reduce high surface area impurities. In embodiments, the method may include mixing lime mud cake with water and sodium carbonate to form a first slurry, and heating the first slurry under conditions to age the slurry and form calcium carbonate (Na2Ca(CO3)2 2H2O, sodalite (Na2Ca2(CO3)3 and monoclinic sodalite (Na2Ca(CO3)2.5H2O). The method may also include separating a solid portion from the aged slurry and washing the solid portion under conditions to decompose one or more of sodalite, sodalite and monoclinic sodalite into a CaCO3 solid fraction and a Na2CO3 solution fraction and remove sodium salts. The CaCO3 solid fraction may then be mixed with water and a dispersant to disperse the CaCO3 solid fraction in water and form a dispersed slurry having a Brookfield viscosity of less than about 100 cps at 100 rpm. Unless otherwise specified, the viscosity values ​​reported herein are Brookfield viscosity values. The CaCO3 solid fraction is a purified precipitated calcium carbonate having a suitable specific surface area, for example, for papermaking applications.

[0048] If required for the desired application, the dispersed slurry can then be ground to a median particle size of about 0.5 microns to about 5 microns, and / or the pH can be adjusted to a pH of about 8 to about 11. For example, the pH can be about 9 to about 10, or about 9 to about 10.5, or about 8 to about 10, or about 8 to about 11. Other suitable pH values ​​include about 8, 8.5, 9, 9.5, 10, 10.5, and 11.

[0049] In embodiments, the method may include washing the first slurry prior to heat aging. The first slurry may be washed, for example, using a filter press, a clarifier, and / or a rotary vacuum filter. In embodiments, washing may be accomplished using water. For example, an amount of water equal to about 1 to about 5 times the dry mass of solids of the first slurry may be used.

[0050] In embodiments, heat aging may be performed by heating the slurry to a temperature of about 80° C. to about 130° C., about 90° C. to about 100° C., about 85° C. to about 95° C., or about 80° C. to about 90° C. Other suitable temperatures include about 80° C., 85° C., 90° C., 95° C., 100° C., 105° C., 110° C., 115° C., 120° C., 125° C., and 130° C.

[0051] In embodiments, the slurry may be aged for about 2 hours to about 8 hours, about 2 hours to about 4 hours, about 3 hours to about 7 hours, about 5 hours to about 8 hours, or about 3 hours to about 6 hours. Other suitable times include about 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, or 8 hours.

[0052] In embodiments, the first slurry may include sodium carbonate of about 20% by weight to about 40% by weight based on the total weight of the first slurry. Other suitable amounts of sodium carbonate include about 25% by weight to about 40% by weight, about 30% by weight to about 35% by weight, about 20% by weight to about 30% by weight, or about 25% by weight to about 35% by weight. For example, the first slurry may include about 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38% by weight, or 40% by weight based on the total weight of the first slurry.

[0053] In embodiments, the first slurry may include lime mud of about 5 wt % to about 30 wt % based on the gross weight of the first slurry. Other suitable amounts of lime mud include about 5 wt % to about 15 wt %, about 10 wt % to about 20 wt %, about 15 wt % to about 30 wt %. For example, the first slurry may include about 5 wt %, 6 wt %, 7 wt %, 8 wt %, 9 wt %, 10 wt %, 11 wt %, 12 wt %, 13 wt %, 14 wt %, 15 wt %, 16 wt %, 17 wt %, 18 wt %, 19 wt %, 20 wt %, 21 wt %, 22 wt %, 23 wt %, 24 wt %, 25 wt %, 26 wt %, 27 wt %, 28 wt %, 29 wt % or 30 wt %.

[0054] In embodiments, after separation from the aged slurry, the solid portion is washed with water. The washing can be performed by passing water through the filter cake or paste using known equipment. For example, a filter press can be used. Alternatively, the solid portion can be resuspended in water and the separation process can be repeated. Other known washing techniques and equipment can be used.

[0055] In embodiments, the sodium carbonate used in the process may be recycled for subsequent use. However, prior to recycling in the process, dissolved silica present in the sodium carbonate from the process must be removed. This may be done, for example, by lowering the pH of the recovered sodium carbonate to about 9.5 to precipitate silica and filtering out the precipitated silica using any suitable filtering method. In embodiments, dissolved silica may be removed by mixing the recovered sodium carbonate with a sodium aluminate solution to precipitate aluminosilicates, and then filtering out the aluminosilicates using any suitable filtering method known in the art.

[0056] Phase separation method

[0057] According to an embodiment, a method for preparing purified precipitated calcium carbonate from lime mud may include using phase separation to remove high specific surface area impurities. Advantageously, it has been found that high specific surface area impurities can be separated from calcium carbonate and removed to produce a purified precipitated calcium carbonate product.

[0058] In embodiments, the method may include mixing the lime mud cake with water and a dispersant to form a dispersed slurry having a viscosity of less than about 1000 cps at 100 rpm, adjusting the pH of the dispersed slurry to a pH of about 8 to about 10.5. In embodiments, the dispersed slurry may have a viscosity of less than about 100 cps at 100 rpm. The method may also include grinding the dispersed slurry to a median particle size of about 0.5 microns to about 5 microns. After grinding, if necessary, the pH may be readjusted to a pH of about 8 to about 10.5. The method may then include causing phase separation in the ground slurry using conditions sufficient to obtain a slurry containing impurity particles and a paste containing purified calcium carbonate. The paste may be separated from the centrate and dispersed in water to a target solid content, thereby producing precipitated calcium carbonate.

[0059] In an embodiment, the method may include mixing the lime mud cake with water to form a first slurry, and the pH of the first slurry may be adjusted to about 10 to about 11, then inducing phase separation to separate impurities and produce a paste containing purified calcium carbonate. The paste may then be separated and mixed with water and a dispersant to form a dispersed slurry having a viscosity of less than about 1000cps at 100rpm. In an embodiment, the dispersed slurry may have a viscosity of less than about 100cps at 100rpm. The dispersed slurry may be ground to a particle size of about 0.5 microns to about 5 microns and the pH may be adjusted to about 9 to about 10.5. In such embodiments where grinding is performed after the phase separation step, it is found that a dispersant is not required in the first slurry, but a dispersant may be added when forming a dispersed slurry of purified precipitated calcium carbonate.

[0060] In any phase separation method disclosed herein, centrifugation can be used as a phase separation method. For example, the method can include centrifuging the ground slurry for a residence time of about 1 minute to about 10 minutes under conditions sufficient to achieve a g-force of about 500 g to about 2000 g to obtain a centrate slurry containing impurity particles and a paste containing purified calcium carbonate. Depending on the end use of the purified precipitated carbonate product, the paste can be separated from the centrate and dispersed in water to a target solids content.

[0061] In any phase separation method disclosed herein, gravity separation or other known phase separation techniques may be used to separate impurities from the calcium carbonate phase.Gravity settling parameters such as settling time and vertical liquid depth may be adjusted for a given slurry.

[0062] The first slurry may have a solid content of about 10% by weight to about 35% by weight based on the total weight of the slurry. Other suitable amounts include about 15% by weight to about 30% by weight, about 10% by weight to about 20% by weight, about 20% by weight to about 25% by weight, or about 10% by weight to about 30% by weight. For example, the first slurry may have a solid content of about 10%, 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34% by weight, or 35% by weight.

[0063] In any of the foregoing embodiments, when the paste or slurry is diluted to form a dispersed slurry of purified precipitated calcium carbonate, the dispersed slurry may have a solid content of about 25% to about 50% by weight based on the total weight of the dispersed slurry. Other suitable solid contents include about 25% to about 40% by weight, about 30% to about 45% by weight, about 30% to about 50% by weight, or about 40% to about 50% by weight, based on the total weight of the dispersed slurry. For example, the dispersed slurry may have a solid content of about 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, 41 wt%, 42 wt%, 43 wt%, 44 wt%, 45 wt%, 46 wt%, 47 wt%, 48 wt%, 49 wt% and 50 wt%, based on the total weight of the dispersed slurry.

[0064] In any of the foregoing embodiments, the dispersant can be one or more of sodium poly(acrylic acid), polycarboxylate homopolymers or copolymers comprising monomer units of acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, hydroxyacrylic acid, and maleic anhydride.

[0065] Hydrocyclone treatment for black carbon removal

[0066] Hydrocyclone treatment can be used alone or in combination with any method for removing high specific surface area materials to remove black carbon from lime mud. When used in combination with a method for removing high specific surface area materials, the removal of black carbon can be performed after the removal of the high specific surface area materials.

[0067] As described above, the method for removing black carbon can be carried out on the precipitated calcium carbonate produced by the treatment to remove high specific surface area impurities or on the lime mud cake. When used for purified precipitated calcium carbonate after removing high specific surface area impurities, the resulting product is generally a slurry of purified precipitated calcium carbonate with water and a dispersant. When used with lime mud cake, the lime mud cake can optionally be dispersed in water with a dispersant to form a slurry for treatment by the black carbon removal method. Any of the dispersants described above can be used. For ease of reference, the term "black carbon removal starting slurry" will be used herein and should be understood to refer to a slurry of previously treated precipitated calcium carbonate in which high specific surface area impurities are removed or a slurry formed from lime mud cake.

[0068] A carbon black removal starting slurry containing water and a dispersant and carbon black impurities can be passed through an apparatus containing one to four hydrocyclones configured in series and / or parallel. As the slurry passes through the apparatus, the carbon black impurities float to the top of the slurry and can be removed. Figure 2 , in an embodiment having four hydrocyclones, for example, the method may include passing the slurry through a first hydrocyclone with the overflow (lighter particles) passing to a third hydrocyclone and the underflow (heavier particles) passing to a second hydrocyclone. In the second hydrocyclone, the overflow flows to the first hydrocyclone and the underflow flows to a recovery chamber. In the third hydrocyclone, the overflow flows to the fourth hydrocyclone and the underflow flows to the first hydrocyclone. In the fourth hydrocyclone, the overflow flows to the waste and the underflow flows to the third hydrocyclone.

[0069] Catch Can Treatment for Black Carbon Removal

[0070] As an alternative to hydrocyclone treatment, the catch tank method can be used to remove black carbon. Figure 1A and Figure 1B , shows a schematic diagram of a catch tank. The catch tank may have a generally conical shape. Figure 1A and Figure 1B In the embodiment shown in , the catch tank has a top cylindrical portion disposed on a frustoconical bottom. The catch tank may also include an overflow valve, a rotating blade, and an outlet. The overflow valve may be disposed in the top region of the catch tank, where the slurry is fed into the catch tank to collect any overflow that may occur, such as by having a feed rate that is higher than the output rate. Without intending to be bound by theory, it is believed that the catch tank design balances the tendency of the black carbon to move upward to the surface in the slurry against the slow downward flow of the slurry. Agitation near the slurry surface enhances the separation of the black carbon from the lime mud particles.

[0071] In such Figure 1A and Figure 1BIn the embodiment shown in, the cylindrical portion may include a feed line for feeding the black carbon removal starting slurry from a feed tank or other container and a rotating blade arranged at the bottom of the cylindrical portion to stir the slurry when the slurry is fed into the capture tank. When the slurry in the capture tank is stirred, the black carbon impurities rise to the surface and the purified sample is located at the bottom of the tank. The bottom of the capture tank may include an outlet pump to recover the purified sample. In an embodiment, the system can be operated to maintain a constant or substantially constant feed flow into the capture tank and the purified sample flows out of the capture tank. In an embodiment, the method may include passing the recovered sample through the capture tank 1 or more times, 2 or more times, 3 or more times, 4 or more times, or 5 or more times. For example, about 1 time to about 3 times, about 2 times to 5 times, about 1 time to 4 times and about 1 time to 5 times. Once the feed / recovered sample has passed the required number of times of the capture tank, it can be collected in the recovery chamber. If desired, the recovered product may be further processed to make it more suitable for use as a filler or pigment, such as by adjusting the pH and / or adjusting the solids content.

[0072] The agitator can be a flat disk blade, a dispersion blade, and / or a saw blade impeller. The agitator can be any blade capable of achieving laminar flow in the slurry. In an embodiment, the agitator can be a Cowles blade having a diameter equal to about 0.4 to about 0.95 times the diameter of the cylindrical portion of the catch tank.

[0073] The agitator may be rotated at a tip speed of about 0.1 m / sec to about 1.5 m / sec, maintaining laminar flow.

[0074] In an embodiment, the residence time of the slurry in the tank may be from about 2 minutes to about 10 minutes, from about 5 minutes to about 8 minutes, from about 4 minutes to about 6 minutes, from about 3 minutes to about 7 minutes, or from about 2 minutes to about 9 minutes. Other suitable residence times include about 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, or 10 minutes.

[0075] Ozone method for removing black carbon

[0076] In an embodiment, the black carbon removal starting slurry can be exposed to ozone treatment to remove black carbon. The black carbon removal starting slurry can be or include a purified form of precipitated calcium carbonate produced by any of the aforementioned methods. Exposure to ozone can be carried out while stirring the black carbon removal starting slurry. Without intending to be bound by theory, it is believed that ozone oxidizes the black carbon into carbon dioxide, which is then removed in the gas stream.

[0077] Any suitable device for generating ozone and flowing ozone through the black carbon removal starting slurry can be used. The generating device can use ultraviolet light, electric discharge or electrolysis. Ozone can be generated in flowing air or pure oxygen or any mixture of the two. The air or oxygen can flow at a flow rate of about 0.1 liters / minute to about 2 liters / minute per liter of lime mud slurry containing ozone gas. For example, a flow rate of about 1 liter / minute of dry air flow can be used to treat 675mL of 10% solid lime mud slurry. The concentration of ozone in the air or oxygen flow can be about 2g / m 3 Up to 50g / m 3 , about 25g / m 3 About 50g / m 3 , about 5g / m 3 About 12g / m 3 , about 2g / m 3 About 15g / m 3 , about 8g / m 3 About 15g / m 3 or about 35g / m 3 About 45g / m 3 Other suitable concentrations include about 2, 4, 6, 8, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, 32, 34, 36, 38, 40, 42, 44, 46, 48 and 50 g / m 3 .

[0078] The method can be completed using any agitator design suitable for maximizing the contact of the gas with the liquid. For example, a radial flow or Rushton impeller can be used at a tip speed of about 1m / sec to about 5m / sec. The ozone reaction can be carried out at an elevated temperature and an elevated pH. For example, a temperature of 40°C can be used. For example, a temperature of about 40°C to about 80°C, about 50°C to about 60°C, about 40°C to about 60°C, about 50°C to about 70°C, or about 45°C to about 65°C can be used. For example, a pH higher than pH 10 or higher than pH 11 can be used. A higher reaction rate with ozone is achieved under these higher temperature and pH conditions, thereby enabling a shorter reaction time to be achieved in a container.

[0079] Flotation method for removing black carbon

[0080] In embodiments, flotation can be used to remove carbon black. The carbon black removal starting slurry can be mixed with a frother and a flotation collector compound. The mixture can be mixed under air flow at a tip speed of about 150m / min to about 500m / min, about 200m / min to about 350m / min, about 300m / min to about 400m / min, or about 150m / min to about 250m / min for 1 minute to 10 minutes, and the foam is collected when it overflows. Carbon black is removed with foam. The remaining end slurry contains purified precipitated calcium carbonate.

[0081] Suitable frothers include standard alcohols with hydrocarbon chains of 5 to 10 carbon atoms, such as methyl isobutyl carbinol (MIBC), amyl alcohol, cresol and terpineol. Other frother types may also be used, such as polyalkoxy ethers and polyethylene glycol ethers. Any combination of one or more frothers may be used. The frother may be used at a level of 10 ppm to 250 ppm per dry mass of lime mud, or from about 10 ppm to about 100 ppm, from about 100 ppm to about 250 ppm of frother. Other suitable values ​​include about 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 125, 150, 175, 200, 225 and 250 pp frother per dry mass of lime mud.

[0082] Suitable flotation collector compounds include kerosene or other oily, water-immiscible compounds, such as diesel. Collectors can be used at 100ppm to 1000ppm, 200ppm to 500ppm, about 150ppm to about 350ppm, or about 700ppm to about 1000ppm collectors per dry mass lime mud. Other suitable values ​​include about 100, 125, 150, 175, 200, 225, 250, 275, 300, 325, 350, 375, 400, 425, 450, 475, 500, 525, 550, 575, 600, 625, 650, 675, 700, 725, 750, 775, 800, 825, 850, 875, 900, 925, 950, 975 and 1000ppm collectors.

[0083] The airflow can be about 1 standard liter per minute (SLPM) to about 6 SLPM, about 3 SLPM to about 5 SLPM, about 1 SLPM to about 2 SLPM, or about 4 SLPM to about 6 SLPM. Other suitable flow rates include about 1, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4, 3.6, 3.8, 4, 4.2, 4.4, 4.6, 4.8, 5, 5.2, 5.4, 5.8 and 6 SLPM.

[0084] In any embodiment herein, the precipitated calcium carbonate product and / or slurry, whether or not further processed to remove carbon black, may be mixed with any additives for formulating the precipitated calcium carbonate into a suitable formulation for use as a filler and / or pigment for a given papermaking application.

[0085] Example

[0086] Example 1: Heat Aging in Sodium Carbonate (HA)

[0087] Lime mud is treated to provide a precipitated calcium carbonate material having a reduced specific surface area and a reduced impurity content compared to the starting material. Lime mud cake is obtained as a waste product from a pulp mill. The lime mud cake is slurried in a 25%-30% sodium carbonate solution having a calcium carbonate solid content of 10%-20%. Specifically, in 1 kg of slurry, 200 g CaCO3 (20% CaCO3), 240 g Na2CO3, 560 g H2O (30% Na2CO3).

[0088] The slurry was then heat aged at 100°C for 8 hours to form a mixed salt, calcium hydroxide (Na2Ca(CO3)2·5H2O). A comparison was made to a process without the heat aging step and the results are listed in the table below.

[0089] The slurry is then filtered or separated into a solid phase and a liquid phase by vacuum filtration using a Buchner funnel and filter paper. The filter cake is washed with three portions of water in a Buchner funnel, each portion being equal to the solid mass of the original lime mud cake. The solid portion is washed with water to remove the sodium salt, which may optionally be recycled to the beginning of the method. This washing also decomposes the calcium water base into CaCO and NaCO.

[0090] The CaCO3 solids were separated and dispersed in water at 35% solids using sodium poly(acrylic acid) as a chemical dispersant. The dispersant was used to reduce the slurry viscosity to a Brookfield viscosity of less than about 100 cps at 100 rpm.

[0091] The pH of the milled slurry was adjusted to a pH of about 9.

[0092] In order to recycle the sodium carbonate solution, the dissolved silica must first be removed and the wash water needs to be separated. The silica can be removed by either: 1) lowering the pH to about 9.5 with carbon dioxide gas to form precipitated silica, which is then filtered off; or 2) precipitating as aluminosilicates with sodium aluminate solution, which is also filtered off. The water can be removed by evaporation or a membrane process such as reverse osmosis.

[0093] The resulting precipitated calcium carbonate formed by thermal aging exhibits a significant reduction in specific surface area and the amount of silica present compared to treatments without an aging step.

[0094] Precipitated calcium carbonate without thermal aging Precipitated calcium carbonate after thermal aging <![CDATA[Specific surface area (m 2 / g)]]> 13.2 6.4 <![CDATA[SiO2%]]> 3.47 1.44

[0095] Example 2: Removal of impurities using phase separation

[0096] The lime mud cake obtained as a waste product from a pulp mill was slurried in water at 20% solids. The slurry was processed using a filter press with a wash cycle to remove excess white liquor from the pulp mill. The filter press was used to first form a filter cake from the 20% solids slurry and then force water through the filter cake. The wash cycle was performed using four times the mass of dry solids.

[0097] The washed filter cake was dispersed in water at 20% solids using sodium poly(acrylic acid) as a chemical dispersant. The resulting dispersed slurry had a viscosity of about 10 cps at 100 rpm.

[0098] The dispersed slurry was then aerated with flue gas having a carbon dioxide content of about 15% to reduce the pH to a pH of about 10.5.

[0099] The pH adjusted slurry is then ground to a desired particle size suitable for use as a paper filler or coating pigment. In this example, the pH adjusted slurry is ground using a continuously operated and single pass vertical media mill. The resulting milled median particle size is about 3.5 microns.

[0100] The pH of the ground slurry was again adjusted to a pH of 9.5 by aeration with carbon dioxide gas. The slurry was then centrifuged continuously at 1400 rpm to 1500 rpm (see table) to obtain a g-force of 713 g or 819 g with a residence time of 4.8 min to 8.4 min. The centrifugal filtrate containing fine particulate impurities was removed and the paste containing the purified product was separated for further processing.

[0101] Four samples were prepared by the aforementioned method, and the resulting paste from each sample had the solid content shown in the table below. The resulting precipitated calcium carbonate was significantly reduced in impurity elements such as silicon, aluminum, magnesium and iron. The reduction in specific surface area and SiO2 content compared to the starting kiln lime mud is shown below.

[0102]

[0103] Example 3: Removal of impurities using phase separation of lime mud before grinding

[0104] The lime mud cake obtained as a waste product from a pulp mill was slurried in water at 20% solids. The slurry was treated using a horizontal filter press with a wash cycle to remove excess white liquor in the liquid phase. The filter press was used to first form a filter cake from the 20% solids slurry to produce a 65% solids filter cake, and then force water through the filter cake. The wash cycle was performed using four times the mass of dry solids.

[0105] The resulting washed filter cake was slurried in water at 23% solids and then treated by aeration with flue gas containing carbon dioxide to reduce the pH to 10.9.

[0106] The pH adjusted slurry was then centrifuged continuously at 1300 rpm to obtain a g-force of 615 with residence times varied as shown in the table. The centrate containing fine particulate impurities was removed and the paste containing the purified product was separated for further processing.

[0107] The resulting centrifuged paste was dispersed in water at 30% solids using sodium poly(acrylic acid) as a dispersant. The Brookfield viscosity of the dispersed slurry was 13 cps at 100 rpm. Four samples were prepared by the aforementioned method as shown in the following table.

[0108] The obtained product has lower impurity elements such as silicon, aluminum, magnesium and iron. It also has reduced impurity phases such as calcium silicate, hydrotalcite and black carbon; and lower specific surface area.

[0109]

[0110] Example 4: Removal of impurities using gravity settling

[0111] The method of Example 2 was repeated, except that a gravity sedimentation method was used instead of centrifugation after grinding. Specifically, the centrifugation step of Example 2 was replaced by allowing sedimentation in a test tube cylindrical container at a specified liquid height and a sedimentation time determined below. After the specified sedimentation time, the top layer was poured off, removed, and the bottom layer was tested.

[0112] The gravity sedimentation method results in some reduction in specific surface area, which is believed to be caused by the reduction of impurities such as silicates.

[0113]

[0114] Example 4: Flotation to remove impurities from lime mud

[0115] Lime mud cake obtained as a waste product from a pulp mill was slurried in water at 20% solids. The slurry was then aerated with pure carbon dioxide to lower the pH to the pH values ​​shown in the table.

[0116] As a silicate flotation collector 3135 (CLARIANT) or 1208 (ARRMAZ) was added to the pH adjusted slurry. The following table shows the dosage based on the dry mass of lime mud.

[0117] The slurry is then diluted with water to 8 wt% solids and processed through a flotation cell system to obtain a concentrated froth containing silicate particle impurities and a final slurry containing purified product.

[0118] The final pulp is then filtered using a vacuum filter and filter paper to remove excess soluble salts in the liquid phase. As a result of the treatment, a paste containing purified CaCO3 is obtained.

[0119] The resulting product contains lower impurity elements such as silicon, aluminum, magnesium and iron. It also has reduced impurity phases such as calcium silicate and hydrotalcite, and lower specific surface area. The following table shows the reduction of SiO2 achieved by this method.

[0120]

[0121] Example 5: Removal of black carbon using a hydrocyclone

[0122] The final product slurry consisting of 30% calcium carbonate aqueous solution, sodium poly(acrylic acid) as a dispersant, and black carbon impurities is further processed to remove the black carbon impurities. The slurry has a viscosity of 40 cps. The slurry is processed through a device comprising four hydrocyclones (HC), and as the slurry passes, the black carbon impurities float to the top of the slurry and can be processed or separated from the purified recovered product (see Figure 2 The overflow (lighter particles) and underflow (heavier particles) of each HC flows to the next as follows:

[0123]

[0124] Qualitative observations indicated that the underflow of HC2 had less black carbon than the feed product.

[0125] Example 6: Removal of black carbon using a capture tank

[0126] like Figure 1A and Figure 1B The catch tank shown in is used to separate carbon black from the final product slurry containing 34.8% calcium carbonate aqueous solution, sodium poly(acrylic acid) as a dispersant, and carbon black impurities. The slurry has a Brookfield viscosity of 20 cps at 100 rpm.

[0127] The feed line in the catch tank is located just above the slurry level near the center of the agitator to maximize the residence time of the slurry above the blades. The feed and product stream pumps are adjusted to maintain a constant level in the catch tank. Dual-head peristaltic pumps are used for the feed and product streams.

[0128] Start the feed flow to fill the catch tank to the overflow, and use a double-head pump to recirculate the product line back to the catch tank during the filling period. Turn on the agitator and set to the rpm listed in the table below. Air flow was provided in some experiments as shown in the table below. As shown in the table below, air flow was not found to help separation. The table also provides the run time. In each experiment, the feed and product streams flowed for about 3 retention times. After the last pass, the product was collected in a clean beaker. Observe the product in the beaker to qualitatively determine the amount of black carbon present in the product compared to the catch tank and overflow tank.

[0129] All runs used a 1.65 liter catch tank with a 4.9 inch ID and either a 4.8 inch diameter flat blade or a 4.0 inch diameter Cowles blade agitator. These runs demonstrated the need for low rpm agitation and slow feed rates.

[0130]

[0131] Example 6: Removal of black carbon by ozone treatment

[0132] A 10% solids lime mud slurry was prepared from the lime mud by diluting with water.

[0133] Approximately 625 ml of the lime mud slurry was poured into a 1 liter bottle with a hole cutout in the lid for an R100 stirrer and another hole cutout in the top to deliver ozone through a SS tube. The slurry was mixed at 730 rpm. The valve on the dry gas cylinder was opened to feed the ozone generator at a pressure of 10 psi. A dry gas stream was supplied at 1 lpm. The ozone generator (model 1KNT purchased from Oxidation Technologies) was run to an ozone level of 100%. Without intending to be bound by theory, it is believed that the ozone reacts with the black carbon, oxidizing the black carbon into carbon dioxide, which is then removed with a gas stream.

[0134] After treatment, Hunter and ISO dry brightness were tested, and a picture of the slurry surface was taken with a camera to determine the black spot area % using Image J software. TGA-DSC analysis was performed.

[0135]

[0136] Example 7: Removal of black carbon using flotation

[0137] A 10% solids lime mud slurry was prepared by diluting the -70% solids filter cake with water.

[0138] 200 ppm or 500 ppm of kerosene collector was added to the slurry and mixed for 2 minutes.

[0139] Then 100 ppm or 250 ppm MIBC (methyl isobutyl carbinol) foaming agent was added and the mixture was mixed for 0.5 minutes.

[0140] The mixture was then mixed at 2000 rpm or 1500 rpm under an air flow of 4 standard liters / minute. Mixing was continued with aeration for 5 minutes or 10 minutes while collecting the overflowing foam.

[0141] The brightness of the collected foam was tested as an indicator of the black carbon content. The remaining final stage pulp contained purified CaCO3 with reduced black carbon.

[0142]

[0143] The use of "a / an" is used to describe elements and components of the embodiments herein. This is merely for convenience and to give a general description. The description should be understood to include one or at least one, and the singular also includes the plural, unless otherwise clearly indicated.

[0144] Furthermore, the drawings depict embodiments for illustrative purposes only. One of ordinary skill in the art will readily recognize from the following discussion that alternative embodiments of the structures and methods shown herein may be employed without departing from the principles described herein.

[0145] Therefore, although specific embodiments and applications have been illustrated and described, it should be understood that the disclosed embodiments are not limited to the precise configurations and components disclosed herein. Various modifications, changes and variations that are obvious to those skilled in the art may be made to the arrangement, operation and details of the methods and apparatus disclosed herein without departing from the spirit and scope defined in the appended claims.

Claims

1. A method for preparing purified precipitated calcium carbonate from lime mud, the method comprising: mixing the lime mud cake with water and a dispersant to form a first slurry having a Brookfield viscosity of less than about 1000 cps at 100 rpm; grinding the first slurry to a median particle size of about 0.4 microns to about 5 microns; phase separating the ground slurry under conditions sufficient to obtain a centrate slurry comprising impurity particles and a paste comprising purified calcium carbonate; as well as The paste is diluted in water to a target solids content, thereby producing a dispersed slurry containing the purified precipitated calcium carbonate.

2. The method of claim 1, further comprising adjusting the pH of the dispersed slurry to a pH of about 8 to about 10 and / or adjusting the pH of the milled slurry to a pH of about 8 to about 10.

3. The method of claim 1 or claim 2, wherein the phase separation comprises centrifuging the milled slurry at a g-force of about 500 g to about 2000 g for a residence time of about 1 minute to about 10 minutes.

4. The method of claim 1 or claim 2, wherein phase separation comprises gravity settling of the milled slurry.

5. The method of claim 4, wherein the gravity settling is performed for a settling time of about 2 hours to 8 hours to a settling depth of about 2 cm to about 3000 cm.

6. The method of claim 1, further comprising, prior to forming the dispersed slurry, mixing the lime mud cake with water to form a first slurry and washing the first slurry to remove caustic soda present in the lime mud cake.

7. The method of any one of claims 1 to 6, wherein the first slurry has a solids content of about 25 wt% to about 50 wt%.

8. A method for preparing purified precipitated calcium carbonate from lime mud, the method comprising: mixing the lime mud cake with water to form a first slurry; adjusting the pH of the first slurry to about 10 to about 11; centrifuging the first slurry for a residence time of about 1 minute to about 10 minutes under conditions sufficient to achieve a g-force of about 500 g to about 2000 g to obtain a centrate slurry comprising impurity particles and a paste comprising purified calcium carbonate; and The paste is mixed with water and a dispersant to form a dispersed slurry having a Brookfield viscosity of less than about 1000 cps at 100 rpm and containing the purified precipitated calcium carbonate.

9. The method of claim 8, further comprising grinding the dispersed slurry to a median particle size of about 0.4 microns to about 5 microns.

10. The method of claim 9, further comprising adjusting the pH of the milled slurry to about 9 to about 10.

5.

11. The method of any one of claims 1 to 10, further comprising adjusting the pH of the dispersion slurry to about 9 to about 10.

5.

12. The method of any one of claims 8 to 11, wherein the first slurry has a solids content of about 10% to about 25%.

13. A method for preparing purified precipitated calcium carbonate from lime mud, the method comprising: mixing the lime mud cake with water to form a first slurry; adjusting the pH of the first slurry to about 8 to about 11; mixing the first slurry with a silicate flotation collector compound to form a second slurry; treating the second slurry through a flotation cell system under conditions sufficient to form a concentrated froth containing silicate particulate impurities and a final slurry containing CaCO3; Washing and separating the final pulp into a liquid phase containing excess soluble salts and a paste containing purified CaCO3; as well as The paste is mixed with water to form a dispersed slurry having a viscosity of less than about 100 cps at 100 rpm and containing the purified precipitated calcium carbonate.

14. The method of claim 13, wherein the first slurry is formed to have a solids content of about 5% to about 15%, or the second slurry is diluted with water to a solids content of about 5% to about 15% and then processed through the flotation cell system.

15. The method of claims 13-14, further comprising grinding the dispersed slurry to a median particle size of about 0.4 microns to about 5 microns.

16. The method of claim 15, further comprising adjusting the pH of the milled slurry to about 9 to about 10.

5.

17. The method of any one of claims 13 to 16, further comprising adjusting the pH of the dispersed slurry to about 9 to about 10.

5.

18. The method of any one of claims 13 to 17, wherein the first slurry has a solids content of about 20% to about 25%.

19. The method of any one of claims 13 to 18, wherein the silicate flotation collector compound is provided in an amount of about 0.1 wt% to about 0.3 wt% based on the dry mass of the lime mud cake.

20. The method of any one of claims 13 to 19, wherein the silicate flotation collector compound is amine based.

21. The method of claim 20, wherein the silicate flotation collector compound is one or more of a primary amine, a dialkyl amine, a tertiary amine, and a quaternary amine.

22. The method of claim 21, wherein the silicate flotation collector is one or more of tallow, coconut amine, hydroxyethyl alkyl imidazoline, lauryl amine, long chain alkyl pyridinium, and n-alkyl trimethyl ammonium.

23. The method of any one of the preceding claims, wherein the dispersed slurry has a solids content of about 25% to about 50%.

24. The method of any one of the preceding claims, wherein the dispersant is one or more of sodium poly(acrylic acid), a polycarboxylate homopolymer or copolymer comprising monomer units of acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, hydroxyacrylic acid, and maleic anhydride.

25. The method according to any one of the preceding claims, wherein the lime mud cake is produced as a pulp mill waste by-product, a sugar beet production by-product or a by-product of acetylene production.

26. The method according to any one of the preceding claims, further comprising adjusting the pH with carbon dioxide gas and / or a carbon dioxide containing gas.

27. A method for removing black carbon from a starting slurry containing calcium carbonate and black carbon, the method comprising: flowing the starting slurry into a first hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a first overflow and to cause the calcium carbonate to remain at the bottom to form a first underflow; passing the first underflow into a second hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a second overflow and cause the calcium carbonate to remain at the bottom to form a second underflow; passing the first overflow into a third hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a third overflow and cause the calcium carbonate to remain at the bottom to form a third underflow; allowing the second underflow to flow into a recovery chamber; allowing the second overflow to flow into the first hydrocyclone; allowing the third underflow to flow into the first hydrocyclone; passing the third overflow into a fourth hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a fourth overflow and cause the calcium carbonate to remain at the bottom to form a fourth underflow; allowing the fourth overflow to flow into a waste container; as well as The fourth underflow is caused to flow into the third hydrocyclone.

28. A method for removing black carbon from a starting slurry containing calcium carbonate and black carbon, the method comprising: passing the starting slurry into a hydrocyclone under conditions sufficient to cause the carbon black particles to rise to the top and form an overflow and to cause the calcium carbonate to remain at the bottom to form an underflow; allowing the overflow to flow into waste; as well as The underflow is passed into a recovery chamber.

29. A method for removing black carbon from a starting slurry containing calcium carbonate and black carbon, the method comprising: flowing the starting slurry into a first hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a first overflow and to cause the calcium carbonate to remain at the bottom to form a first underflow; passing the first underflow into a second hydrocyclone under conditions sufficient to cause the black carbon particles to rise to the top and form a second overflow and cause the calcium carbonate to remain at the bottom to form a second underflow; allowing the first overflow and the second overflow to flow into waste material; as well as The second underflow is passed into a recovery chamber.

30. A method for removing black carbon from a starting slurry containing calcium carbonate and black carbon, the method comprising: loading the starting slurry into a catch tank using a continuous inflow at or near the center of the catch tank; agitating the starting slurry in the catch tank using an agitator at a tip speed of about 0.1 m / sec to about 1.5 m / sec and under conditions sufficient to cause the carbon black particles to rise to the top of the catch tank and cause the calcium carbonate to settle to the bottom of the catch tank, with a residence time of about 4 min to about 10 min; and The calcium carbonate is pumped from the bottom of the catch tank to a recovery vessel.

31. The method of claim 30, wherein the residence time is from about 6 min to about 10 min.

32. The method of claim 31, wherein the residence time is from about 8 min to about 10 min.

33. The method of any one of claims 30 to 32, wherein the tip speed is about 0.1 m / sec to about 0.2 m / sec.

34. A method for removing black carbon from a starting slurry containing calcium carbonate and black carbon, the method comprising: Ozone-containing gas is flowed through the starting slurry at a flow rate of about 0.1 liter / minute to about 2 liters / minute per liter of the starting slurry with an agitator at a tip speed of about 1 m / sec to about 5 m / sec, wherein the black carbon is oxidized by the ozone to form carbon dioxide gas and removed with the gas flow.

35. The method of claim 34, wherein the concentration of ozone in the ozone-containing gas is about 2 g / m 3 About 50g / m 3 .

36. The method according to claim 34 or 35, wherein the starting slurry is heated to an elevated temperature of about 40°C to about 60°C during the flow of the ozone-containing gas through the starting slurry.

37. The method according to any one of claims 34 to 36, wherein the pH of the starting slurry is adjusted to a pH above 10 during the flow of the ozone-containing gas through the starting slurry.

38. A method for removing black carbon from a starting slurry containing calcium carbonate and black carbon, the method comprising: mixing the starting slurry with a frother and a flotation collector compound to form a second slurry; processing the second slurry through a flotation device at an airflow of about 1 slpm to about 3 slpm per liter of second slurry and with an agitator at a tip speed of about 150 m / min to about 500 m / min for about 1 minute to about 10 minutes, with froth overflowing from the flotation device and a final stage slurry remaining in the flotation device, the froth comprising the carbon black and the final stage slurry comprising calcium carbonate; and The final slurry is collected and dispersed in water to form a dispersed slurry containing the calcium carbonate.

39. The method of claim 38, wherein the flotation collector is present in an amount of about 100 ppm to about 1000 ppm.

40. The method of claim 38 or 39, wherein the flotation collector compound is one or more of kerosene or diesel.

41. A method according to any one of claims 38 to 40, wherein the starting slurry is lime mud cake dispersed in water and optionally a dispersant.

42. A method according to any one of claims 27 to 41, wherein the starting slurry is a purified slurry containing calcium carbonate after treatment to remove high specific area impurities.