Preparation method and application of protonated perovskite anode additive and membrane electrode
By combining the protonated perovskite anode additive HCa2Nb3O10 and Pt/C catalyst, the conduction ability and durability of oxide materials in the anode catalytic layer in the prior art is solved, and efficient proton conduction and anti-reverse properties are achieved. Extends battery life and improves performance stability.
Patent Information
- Application Number
- CN202410922456.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-26
AI Technical Summary
Although the addition of oxide materials to the anode catalytic layer by existing proton exchange membrane fuel cells (PEMFCs) improves the proton conduction ability, excessive addition will affect electron conduction and easily lead to carbon corrosion and membrane perforation, affecting the durability of the battery and stability.
The protonated perovskite anode additive HCa2Nb3O10 is prepared by solid phase synthesis method and mixed with Pt/C catalyst to form a layered structure, which improves the hydrophilicity and proton conduction ability of the anode, prevents electrolyte overdrying and cathode water flooding. At the same time, hydrogen protons are generated through OER reactions to avoid carbon corrosion.
It significantly improves the proton conduction rate of the anode catalyst, extends the service life of the battery, improves the peak power density and stability of the membrane electrode, reduces the risk of carbon corrosion, and improves the overall performance of the battery.
Smart Images

Figure CN119018935A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a protonated perovskite anode additive, a preparation method of a membrane electrode and application thereof, and belongs to the technical field of proton exchange membrane fuel cells. Background Art
[0002] At present, the world is facing resource shortages and environmental pollution. Hydrogen, as a clean and pollution-free energy source, has attracted widespread attention and has been vigorously developed. People are gradually moving towards the hydrogen economy era. Proton exchange membrane fuel cells (PEMFCs), as an environmentally friendly and efficient energy conversion technology, have incomparable advantages compared to traditional energy sources.
[0003] Proton exchange membrane fuel cells use hydrogen (H 2 ) and oxygen (O 2 ) is used as fuel, and the hydrogen molecules on the anode side are oxidized into hydrogen protons (H + ) and electron, H + The electrons are transported to the cathode through the Nafion membrane. At the same time, the electrons reach the cathode and O through the external circuit. 2 and H + Oxygen reduction reaction occurs to generate water. During the whole process, H + The transfer rate is particularly important. + The transfer mechanism of H on the polymer side chain mainly includes the transition mechanism and the onboard mechanism. Among them, the transition mechanism refers to the transfer of H on the polymer side chain in the presence of liquid water. + From the sulfonate (-SO 3 H) and combines with water to form hydrated protons (H 3 O + ), H + Through the breaking and forming of hydrogen bonds, it quickly jumps to the next water molecule to achieve the conduction of hydrogen protons. 3 O + The water molecules migrate to the cathode through net electrical attraction and potential difference, and the excess water molecules diffuse back to the anode due to the concentration difference. Therefore, it is particularly important to seek anode materials with certain hydrophilicity and proton conductivity.
[0004] In recent years, many researchers have added hygroscopic materials to the anode catalyst layer to improve the proton conductivity of PEM fuel cells, promote reverse diffusion of the membrane, reduce cathode flooding and reduce mass transfer resistance. For example, materials such as metal oxides. Wen-Kai Chao and Chih-Ming Lee et al. used aluminum isopropoxide as a precursor and synthesized γ-Al by a sol-gel three-step method in an alkaline medium. 2 O 3The particles were mixed with commercial Pt / C to prepare the anode catalyst layer slurry by a simple ultrasonic method. 2 O 3 The current density is better than commercial Pt / C. Xiaoqian Guo's team used the photosensitive hygroscopic material TiO 2 Added to the anode catalyst layer, the anode self-humidification is achieved by ultraviolet light irradiation. At a voltage of 0.6 V, adding TiO 2 The current density of the membrane electrode is that without adding TiO 2 2.3 times the electrical conductivity of the membrane electrode, 1200mA / cm 2 When TiO is added, the ohmic resistance and mass transfer resistance are lower than those without adding TiO 2 Yufang Shen et al. added ZnO particles to the anode catalyst layer by simple ultrasound. When the anode humidifier temperature was 25, 45 and 65 °C, the power density was 0.26 W / cm 2 , 0.33W / cm 2 and 0.34W / cm 2 , 30%, 37.5% and 36% higher than MEA without ZnO particles, respectively. Although the addition of oxides can improve the proton conductivity to a certain extent, when the amount is too much, it will affect the electronic conduction of the battery. The COF network has good water retention capacity and also has a certain proton transmission capacity. To this end, Xie Zheng et al. loaded COF on phosphoric acid H 3 PO 4 SNW-1COF was obtained and ultrasonically mixed with commercial Pt / C as the anode catalyst layer. The peak power density was 582 mW / cm at a humidity of 10 wt%. 2 , which is 7 times that of commercial Pt / C under the same conditions. However, simple ultrasonic mixing will lead to uneven distribution of COF materials and increase the interfacial contact resistance.
[0005] In addition, most of the research on proton exchange membrane fuel cells (PEMFC) is focused on cathode catalysts, and the performance and durability of proton exchange membrane fuel cells are improved by modifying and optimizing cathode catalysts. The operation of PEMFC is mainly to transfer the hydrogen protons produced by hydrogen oxidation on the anode side through the Nafion membrane to the cathode for oxygen reduction reaction. At the same time, electrons reach the cathode from the external circuit to realize operation. Therefore, the proton conduction rate of the anode catalyst layer is particularly important for battery performance. In addition, during the start-stop process of the battery, the phenomenon of insufficient hydrogen supply will occur, and the flatness of the membrane electrode will also cause local lack of hydrogen, which will cause reverse polarity, leading to oxidation of carbon and water at the anode, causing carbon corrosion problems and then causing membrane perforation, which will reduce the performance and stability of the battery. Therefore, in view of the above problems, it is essential to develop an anode catalyst with proton conduction ability and anti-reverse polarity ability.
[0006] In PEMFC, proton conductivity is one of the key factors affecting membrane electrode performance. In the past, many researchers have applied oxidized proton conductors to fuel cells to improve the proton conductivity. 0.8 Zr 0.2 O 3-δ BCZYG-Pr was synthesized by doping gadolinium (Gd), yttrium (Y) and praseodymium (Pr) at the B site of (BCZ). 0.1 The proton conductivity of the anode catalyst layer of the fuel cell was improved through the synergistic effect of the three dopants. The proton conductivity measured at 400°C and 50% humidified argon atmosphere was 3.11 mS / cm, which is much higher than the proton conductivity of BCZ. 0.1 Ce 0.7 Y 0.1 Yb 0.4 O 3-δ (BZCYYb) prepared Ni-BZCYYb anode catalysts with different porosities and explored the effect of porosity on proton conductivity. Among them, the best porosity was 37%, and the proton conductivity was measured at 500℃ and reducing atmosphere to be about 2.41×10 3 Jun Zhang, Bin Hu and others further applied the perovskite BZCYYb to proton exchange membrane fuel cells, using carbon (C) and BZCYYb as a composite carrier to load metal platinum, with a peak power density of 1.7 W / cm 2 , which is 3.75 times that of commercial Pt / C (JM 20%). In addition, under high temperature and low humidity conditions, due to the water retention of the composite catalyst, it can promote the diffusion of water from the cathode catalyst layer to the membrane, preventing the membrane electrode from drying out.
[0007] The problems of carbon corrosion and membrane perforation caused by the anode reversal phenomenon greatly affect the durability and activity of the battery. In order to avoid damage caused by the reversal of the positive and negative electrodes of the battery, it is usually necessary to optimize the system control strategy, such as continuous monitoring of voltage and exhaust, anode purge, etc. to delay the rise of anode voltage, which increases the operating cost of the battery. For this reason, many researchers have done a lot of research on anode carriers. Among them, one solution is to use an anti-reversal material with OER catalytic activity to preferentially oxidize the water accumulated in the anode chamber to replenish protons, thereby delaying the occurrence of carbon corrosion. At present, iridium oxide (IrO 2 ) to accelerate the water electrolysis reaction to avoid carbon oxidation. Jianhua Liao made his own IrO 2 Added in the anode catalyst layer, where IrO 2 The membrane electrode has a reverse polarity resistance of 132.2 minutes, which is 66 times that of commercial Pt / C. 2 At a current density of 1.34 W, the voltage dropped by only 22.12%, proving that IrO 2 It has excellent anti-reverse polarity ability. In order to avoid carbon corrosion caused by contact between carbon and water, Hee-Eun Kim, Sangyong Shin and Hyunjoo Lee used iridium oxide (IrO x ) was deposited on commercial Pt / C to synthesize Pt-IrO x / C, where IrO x It can be anchored on carbon with defects to better protect carbon. x When loaded onto a carbon carrier, the particle size is large and difficult to disperse. Therefore, people began to seek anode catalysts without carbon carriers.
[0008] Jianhua Liao et al. used thermal reduction method to 2 ) doped with niobium (Nb) to increase the 2 Conductivity. Then IrO x Deposited on Nb 0.1 Ti 0.9 O 2-x IrO x / Nb 0.1 Ti 0.9 O 2-x Compared with traditional carbon supports, TiO 2 Has higher stability, which is beneficial to IrO x Although the anti-reverse polarity time is 14 times longer than that of commercial Pt / C, the battery performance is much lower than that of commercial Pt / C. 2 Ti with higher conductivity4 O 7 As the anode carrier, metal Pt is loaded and doped with a very small amount of IrO 2 Hae Wook Park et al. used tungsten oxide (WO 3 ) Loaded metal Pt, WO 3 Generate H through hydrogen spillover effect x WO y , H x WO y It can decompose to provide hydrogen protons and electrons to prevent carbon corrosion.
[0009] In order to prevent carbon corrosion, one method is to use metal oxides as anode carriers to avoid carbon corrosion, but metal oxides with poor conductivity will affect battery performance; another method is to add OER catalysts (such as IrO 2 ) promotes the oxidation of water to provide hydrogen protons, but iridium oxide particles are difficult to disperse evenly, which will reduce the stability of the battery. Summary of the invention
[0010] The purpose of the present invention is to provide a protonated perovskite anode additive, a preparation method of a membrane electrode and its application. The obtained anode additive has hydrophilicity and excellent proton conductivity. When applied to a membrane electrode, it can increase the proton conduction rate of the catalyst and effectively prevent electrolyte dryness and cathode flooding. The hydrophilicity can promote the back diffusion of water by the membrane, diffuse the water accumulated on the cathode side to the anode, generate hydrogen protons and electrons through OER reaction, make up for the supply of anode protons, and avoid carbon corrosion.
[0011] In order to achieve the above object, the technical solution adopted by the present invention is:
[0012] A method for preparing a protonated perovskite anode additive, specifically: preparing KCa by solid phase synthesis 2 Nb 3 O 10 Then carry out acid replacement to obtain HCa 2 Nb 3 O 10 That is the protonated perovskite anode additive.
[0013] Preferably, KCa 2 Nb 3 O 10 The preparation method is: K 2 CO 3 、CaCO 3 and Nb 2 O 5 The mixed product is ball-milled, dried, calcined, ground and re-fired to obtain the product.
[0014] Preferably, K 2 CO 3 、CaCO 3 and Nb 2 O 5 The mass ratio is (0.5-1.2):(1.5-3):(3-6).
[0015] Preferably, the ball milling conditions are: 200-500 rpm, 0.5-2 h;
[0016] The calcination conditions are: 1000-1500°C, 10-15h;
[0017] The conditions for re-firing are: 1000-1500℃, 10-15h.
[0018] Preferably, KCa 2 Nb 3 O 10 The specific method of acid replacement is: KCa 2 Nb 3 O 10 After soaking in HCl at room temperature, it is obtained by centrifugation and drying.
[0019] Preferably, KCa 2 Nb 3 O 10 The ratio with HCl is (2-5) g: (80-150) ml, and the HCl concentration is 5-10 mol / L.
[0020] Preferably, the soaking time is 40-50 hours, and the HCl is replaced once every 20-25 hours;
[0021] Drying conditions: 60-80℃.
[0022] A method for preparing an anode catalyst is to prepare a protonated perovskite anode additive HCa by any of the above methods. 2 Nb 3 O 10 The catalyst is mixed with a Pt / C catalyst having a Pt content of 40 wt% in a mass ratio of 1:(0.8-1.5), ball-milled for 0.5-1.5 hours, and then dried and ground to obtain the catalyst.
[0023] A method for preparing a membrane electrode comprises dispersing the anode catalyst prepared by the above method, 5wt% Nafion solution and conductive carbon in an alcohol solution in a mass ratio of 1:(5-8):(0.8-1.5) to prepare an anode slurry, and then spraying the anode slurry on an electrolyte membrane at 70-85°C and hot pressing to obtain the anode slurry.
[0024] The membrane electrode prepared by the above method is used as an anode in a proton exchange membrane fuel cell.
[0025] The beneficial effects of the present invention are:
[0026] 1. Protonated perovskite anode additive HCa 2 Nb 3 O 10 It has a layered structure and an increased specific surface area. The contact angle of HCNO is 63.3°, showing strong hydrophilicity. Therefore, the anode used in PEMFC can effectively prevent electrolyte membrane perforation caused by reverse polarity phenomenon. It is also beneficial to promote the reverse diffusion of water to the membrane and reduce the occurrence of water flooding on the cathode side.
[0027] 2. HCa 2 Nb 3 O 10 For sandwich experiments, 2 -O 2 The peak power density of a single cell test was 540 mW / cm 2 , which is 1.26 times that of KCNO and 36 times that of BZCYYb, showing excellent proton conductivity. Applying it to the anode catalyst layer can quickly improve the proton transfer rate of the anode catalyst layer, providing a new research idea for the development of anode catalysts;
[0028] 3. By adding conductive carbon to make up for the lack of conductivity of the anode catalyst, 2 -O 2 The single cell test was carried out under the same conditions, and 1.12W / cm was achieved at 0.45V. 2 The peak power density at H 2 -Under Air conditions, it also reached 717mW / cm 2 The peak power density is higher than that of commercial Pt / C;
[0029] 4. Pt / C-HCNO was synthesized by physically mixing commercial Pt / C with HCNO using ball milling, which simplified the synthesis method and ensured the uniform dispersion of the noble metal Pt. 2 -O 2 and H 2 - Single cell test under Air conditions, the peak power density is 1.31W / cm 2 and 847.5mW / cm 2 , which is 1.17 and 1.18 times that of Pt / HCNO tested under the same conditions, and 1.37 and 1.35 times that of commercial Pt / C. In the constant voltage steady-state test, the current density loss was within 3%, proving that the catalyst has good catalytic performance and stability;
[0030] 5. In the anti-reverse polarity test and impedance test, Pt / C-HCNO reaches the cutoff voltage later than commercial Pt / C, and its impedance change before and after the reverse polarity is much smaller than that of commercial Pt / C, which proves that HCNO has a certain anti-reverse polarity ability. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 (a) XRD patterns of KCNO synthesized with different K contents, (b) a local enlarged view of (a), (c) XRD patterns of KCNO synthesized with different sintering temperatures, (d) a local enlarged view of (c);
[0032] Figure 2 SEM images of KCNO at different calcination temperatures, (a) 1000℃, (b) 1100℃, (c) 1200℃, (d) 1300℃;
[0033] Figure 3 N for KCNO synthesized at different calcination temperatures 2 Adsorption-desorption isotherm curves, the inset shows the pore size distribution based on the BET method, (a) 1000 °C, (b) 1100 °C, (c) 1200 °C, (d) 1300 °C;
[0034] Figure 4 XRD patterns of HCNO prepared by soaking KCNO in 6M and 7M HCl for different time periods;
[0035] Figure 5 SEM images of HCNO at different magnifications;
[0036] Figure 6 (a) N of HCNO 2 Adsorption-desorption isotherm curve, the inset shows the pore size distribution based on the BET method, (b) TG graph of HCNO, (cd) contact angle test of HCNO;
[0037] Figure 7 (a) Schematic diagram of membrane electrode assembly and proton conduction for the sandwich experiment, (b) SEM image of the cross-section of the membrane electrode with HCNO as the sandwich;
[0038] Figure 8 (ab) Polarization curves of different samples as interlayer batteries, (c) Impedance diagram of 0.25g HCNO as interlayer batteries and double-layer Nafion membrane batteries, (d) Proton conductivity of 0.25g HCNO as interlayer batteries and double-layer Nafion membrane batteries;
[0039] Fig. 9(a) SEM image of Pt / HCNO, (b) HR-TEM morphology of Pt / HCNO, (ce) lattice fringes of Pt in Pt / HCNO;
[0040] Fig.10 (a) XRD spectrum of Pt / HCNO, (b) Pt4fXPS result of Pt / HCNO;
[0041] Fig.11 Cell polarization curves of adding different types of conductive carbon in the same proportion to the anode catalyst Pt / HCNO (a), (b) adding different proportions of SuperP to the anode catalyst Pt / HCNO.
[0042] Fig.12 SEM images of Pt / HCNO film electrode at different magnifications;
[0043] Fig.13 (a) SEM morphology of Pt / C-HCNO, (b, c) HR-TEM morphology at different magnifications, (d) Pt nanoparticle size distribution, (ef) HCNO lattice fringes, (gh) lattice fringes;
[0044] Fig.14 (a) XRD pattern of Pt / C-HCNO, (b) XPS result of Pt / C-HCNO;
[0045] Fig.15 Pt / HCNO, TZPt / C and Pt / C-HCNO(a) in H 2 -O 2 Polarization curves under H 2 -Air conditions, (c) 24h constant voltage (0.6V) steady-state test results, (d) H 2 -O 2 Peak power density bar graph under the conditions, (e) under H 2 -Polarization curve under Air condition, (f) Current density bar graph before and after steady-state test;
[0046] Fig.16 (a) Voltage-time curves of Pt / C(TZ) and Pt / C-HCNO reverse polarity tests, (b) polarization curves of Pt / C-HCNO before and after reverse polarity tests, (c) polarization curves of Pt / C(TZ) before and after reverse polarity tests;
[0047] Fig.17 (a) and (b) are the impedance diagrams of Pt / C(TZ) and Pt / C-HCNO before reversal of electrode, (c) and (d) are the impedance diagrams of Pt / C(TZ) and Pt / C-HCNO before reversal of electrode. DETAILED DESCRIPTION
[0048] The present invention will be specifically described below in conjunction with the accompanying drawings and embodiments.
[0049] Example 1
[0050] Protonated perovskite HCa 2 Nb 3 O 10 Synthesis
[0051] K 2 Nb 3 O 10 Preparation
[0052] Layered perovskite KCa was synthesized by solid phase method. 2 Nb 3 O 10 (KCNO), K 2 CO 3 (0.86 mg), CaCO 3 (2.00mg), Nb 2 O 5 (3.99 mg) and an appropriate amount of deionized water were added to a ball mill, ball milled at 400 rpm for 1 h, and then dried under a sodium lamp to obtain a precursor. The precursor was calcined in a high-temperature furnace at 1200°C for 12 h, taken out and ground once, and calcined again for 12 h to finally obtain KCNO.
[0053] HCa 2 Nb 3 O 10 Preparation
[0054] Take 2.5 g of KCNO and place it in 100 ml of concentrated HCl (7 mol / L), soak it at room temperature for 48 h, replace the concentrated HCl once every 24 h, collect the white precipitate by centrifugation, and dry it in a vacuum drying oven at 70 ° C overnight to obtain HCNO.
[0055] BZ 0.01 Ce 0.7 Y 0.1 Yb 0.1 O 3-σ Preparation
[0056] The synthesis method of BaZr was consistent with that of KCNO. 0.01 Ce 0.7 Y 0.1 Yb 0.1 O 3-σ (BZCYYb).
[0057] Preparation of membrane electrode
[0058] The membrane electrode was prepared by CCM method with an area of 2×2cm 2 30 mg of HCNO was dissolved in 2 mL of isopropanol solution and ultrasonically homogenized, then sprayed on one side of the Nafion membrane and combined with another Nafion membrane by short hot pressing to prepare a composite electrolyte. Commercial Pt / C (JM, 20%) was used as the anode and cathode of the membrane electrode, with the Pt loading of the anode and cathode being 0.2 mg respectively. Pt / cm 2 and 0.1g Pt / cm 2 . Take Pt / C (6 mg) and 1.5 ml of 5 wt% Nafion solution (39.93 mg) and dissolve them in isopropanol and ultrasonically mix them as anode slurry. Similarly, take Pt / C (11 mg) and 5 wt% Nafion (73.22 mg) and dissolve them in 1.5 mL of isopropanol and ultrasonically mix them as cathode slurry. At 75°C, the anode and cathode slurries were sprayed on both sides of the composite electrolyte, and finally the membrane electrode was obtained by hot pressing.
[0059] Characterization and analysis of KCNO
[0060] Since potassium (K) is volatile at high temperatures, the synthesis temperature was first controlled to be 1200°C and the amount of K added to the precursor was screened. Figure 1 As shown in the (a) and (b) regions, KCNO was synthesized using four kinds of K contents, namely, no excess K and 10%, 20%, and 30% excess K. Compared with the standard characteristic peak of KCNO (the dotted line in the figure is the standard PDF card peak position), the peak intensity of KCNO synthesized under different K contents is similar to the standard peak intensity, indicating that the synthesized perovskite phase structure is good. Among them, KCNO prepared under the conditions of no excess K and 10% excess K respectively, compared with the standard peak position, has different degrees of deviation to high angles. This is because K volatilizes severely at high temperature, resulting in a small K content at the A position in the synthesized KCNO, resulting in lattice compression. At the same time, KCNO synthesized with 30% and 20% excess K are consistent with the standard characteristic peak position of KCNO, indicating that KCNO with a good phase structure can be synthesized using the conditions of 30% and 20% excess K. Considering the cost issue, 20% excess K was finally used as the final synthesis condition.
[0061] Then, the synthesis temperature was further screened. Figure 1As shown in the middle (c) and (d) regions, the precursor was sintered at 1000℃, 1100℃, 1200℃ and 1300℃, respectively. From the XRD characteristic peaks in the figure, it can be seen that when the synthesis temperature is 1000℃, the XRD peak intensity is small, much smaller than the standard peak intensity of KCNO, indicating that the phase structure of KCNO synthesized at this temperature is poor. At the same time, when the synthesis temperature is 1100℃, 1200℃ and 1300℃, the peak intensity of the synthesized KCNO is similar to the standard peak intensity, indicating that the KCNO synthesized at 1100℃, 1200℃ and 1300℃ has a good phase structure. However, the peak position of KCNO synthesized at 1100℃ shifts to a higher angle compared with the standard peak, which is caused by the slightly lower A-position K content in KCNO synthesized at 1100℃. Finally, considering the preparation cost, 1200℃ is taken as the optimal synthesis temperature.
[0062] In summary, the final synthesis conditions were 20% excess K in the precursor and a sintering temperature of 1200°C.
[0063] like Figure 2 As shown in Figure 2, KCNO synthesized at sintering temperatures of 1000°C, 1100°C, and 1200°C were characterized by SEM. Figure 2 It can be seen that KCNO is a block oxide with a smooth surface, which is stacked up in multiple layers. In addition, it can be observed that the particle size of KCNO increases with the increase of sintering temperature. Table 1 shows the average particle size of KCNO at different sintering temperatures. The calcination temperature increases from 1000℃ to 1300℃, and the corresponding particle size also increases from 0.67μm to 1.48μm. This is because the surface atoms of the particles decomposed by the high temperature of the precursor diffuse to the adjacent surface and bond with the corresponding atoms to form stable chemical bonds, thereby forming agglomerations and increasing the size of the particles.
[0064] Table 1 Average particle size of KCNO at different calcination temperatures
[0065]
[0066]
[0067] In order to analyze the effect of sintering temperature on the specific surface area of KCNO, BET tests were performed on KCNO sintered at different temperatures. Figure 3 As shown in Figure 2, the sintering temperature not only affects the particle size of the catalyst, but also affects the specific surface area of the catalyst. When the sintering temperature is 1000°C, the specific surface area of KCNO is 4.479 m 2 / g, and the specific surface area when the sintering temperature is increased to 1100℃ is 1.9941m 2 / g, the specific surface area decreased by about 60%. When the temperature was 1200℃, the specific surface area decreased by about 20% compared with that of KCNO at 1100℃. Compared with KCNO at 1200℃, the specific surface area of KCNO synthesized at 1300℃ was only reduced by about 1%. Therefore, it was found that when it was higher than 1000℃, the temperature had little effect on the specific surface area of KCNO. Combining XRD and SEM characterization, the synthesis temperature of KCNO was finally screened as 1200℃.
[0068] Characterization and analysis of HCNO
[0069] HCNO is obtained by acid substitution of KCNO, and the concentration and duration of the acid are screened. Figure 4 As shown in the figure, under the condition of 72h of acid soaking, KCNO was acid-displaced with 6mol and 7mol concentrated hydrochloric acid, respectively. Among them, the HCNO obtained by substitution with 7mol concentrated hydrochloric acid was basically consistent with the standard PDF card, and compared with the standard PDF card of HCNO (the dotted line in the figure is the standard peak position), the peak position of HCNO obtained by substitution with 6mol concentrated hydrochloric acid was cheaper to a low angle. This is because the acid concentration is too low, resulting in K not being completely replaced, so 7mol concentrated hydrochloric acid was selected. In order to shorten the synthesis cycle, KCNO was soaked in 7mol concentrated hydrochloric acid for acid substitution, soaking for 72h, 48h and 24h respectively. The peak intensity and peak position of 48h and 72h were completely consistent with the standard PDF card of HCNO, while the peak position of HCNO obtained by soaking for 24h shifted to a low angle, and the peak intensity was weakened. This is because the speed of H and K substitution is slow, and the time is too short, resulting in H not being able to completely replace K. HCNO contains trace amounts of K elements, which affects the phase structure of HCNO.
[0070] Subsequently, the acid-substituted HCNO was characterized by SEM. Figure 5 As shown, acid replacement did not destroy the original morphology of KCNO, and HCNO still maintained a block morphology composed of multilayer flakes.
[0071] In order to explore the effect of acid replacement on the specific surface area of KCNO, the BET test was performed on the HCNO obtained by acid replacement. Figure 6 As shown in area (a), the specific surface area of HCNO is 4.583 m 2 / g, compared to Figure 3 In the middle (c) region, the specific surface area of HCNO is about three times that of KCNO. This is because the radius of the hydrogen atom (H) is much smaller than that of the K atom. H replaces K at the A position, which reduces the interlayer van der Waals force and increases the interlayer spacing.
[0072] In order to further understand the physical properties of HCNO, TG test was carried out on HCNO. Figure 6The middle (b) region is HCNO in nitrogen (N 2 The mass change curve of the temperature rising from room temperature to 700℃ under the atmosphere of ) was shown in Figure 2. It was found that HCNO began to decompose at nearly 250℃, indicating that HCNO can be applied to the actual operating temperature conditions of PEMFC (generally 80℃).
[0073] Then, Figure 6 ((c) area and (d) area) are the contact angle test diagrams of HCNO. The contact angles of HCNO and XC-72R are 63.3° and 141.1° respectively. Compared with the traditional carbon carrier XC-72R, HCNO shows stronger hydrophilicity. Therefore, HCNO used in the anode of PEMFC can effectively prevent the electrolyte membrane perforation caused by the reverse polarity phenomenon, and it is also beneficial to promote the reverse diffusion of water to the membrane and reduce the occurrence of water flooding on the cathode side.
[0074] Sandwich experiment
[0075] Figure 7 The middle (a) area is a schematic diagram of the membrane electrode assembly and proton conduction of the sandwich experiment. Figure 7 In the middle (a) area, 30 mg of HCNO, KCNO, and BZCYYb were used as interlayers to assemble the battery, and the single cell test was carried out at 80 °C (H 2 -O 2 ), the battery performance depends on the proton conductivity of the interlayer. In addition, SEM images of the membrane electrode cross section after the test were taken. Figure 7 As shown in the middle (b), the Nafion membranes on both sides of HCNO did not adhere to each other, ensuring that H + Conduction is only carried out through the middle layer.
[0076] In the single cell test ( Figure 8 In the middle (a) area, the peak power density of the battery with HCNO, KCNO and BZCYYb as interlayer and the double Nafion membrane battery without interlayer are 540mW / cm 2 、430mW / cm 2 、15mW / cm 2 and 857mW / cm 2 , the peak power density of HCNO is significantly higher than that of KCNO and BZCYYb, showing better proton conductivity. Figure 8 As shown in the middle (b) area, in order to ensure the reliability of the experimental data, the middle HCNO interlayer is increased from 30 mg to 0.25 g, and its peak power density can still reach 162 mW / cm 2 .also, Figure 8The middle (c) area is the battery impedance diagram of 0.25g interlayer HCNO and double-layer Nafion membrane. The battery impedance of 0.25g HCNO interlayer is 1.59Ωcm 2 , while the impedance of the double-layer Nafion membrane is 0.303Ωcm 2 . Figure 8 The middle (d) area is the corresponding proton conductivity bar graph. It can be seen intuitively that although the proton conductivity of HCNO is lower than that of Nafion membrane, it still has a certain proton conductivity, which is an advantage that traditional carbon substrates do not have.
[0077] In summary, this embodiment uses a simple solid phase method to synthesize protonated layered perovskite KCNO, and synthesizes HCNO by simple acid replacement. In addition, HCNO has a certain proton conductivity, and its application in the anode can greatly improve the proton conductivity rate of the anode catalyst. Due to the hydrophilicity of HCNO, it can also effectively prevent the problem of electrolyte over-drying and the occurrence of cathode flooding, and has a good application prospect. The summary is as follows:
[0078] (1) The K content in the KCNO precursor was screened by XRD, and it was found that too little K addition would cause the peak position of KCNO to shift to a high angle, resulting in lattice compression.
[0079] (2) The optimal synthesis temperature of KCNO was screened out by XRD, BET and SEM to be 1200℃. When the sintering temperature was too low, although the particle size of the synthesized KCNO was small and the specific surface area was relatively large, the phase structure of the synthesized KCNO was poor. When the temperature was too high, the particle size increased and the specific surface area decreased, but the phase structure was good.
[0080] (3) Characterizations such as XRD, BET, SEM, and contact angle confirmed that HCNO has a layered structure. Compared with KCNO, the specific surface area of HCNO is slightly increased. The contact angle proves that HCNO has a certain degree of hydrophilicity.
[0081] (4) Interlayer experiment on HCNO 2 -O 2 The peak power density of a single cell test was 540 mW / cm 2 , which is 1.26 times that of KCNO and 36 times that of BZCYYb, showing excellent proton conduction ability. Applying it to the anode catalyst layer can quickly improve the proton transfer rate of the anode catalyst layer, providing a new research idea for the development of anode catalysts.
[0082] Example 2
[0083] Preparation of Pt / HCNO
[0084] HCNO (80 mg), 4 mg Pt / mL H 2 PtCl 6 6H 2 0.213 g of sodium borohydride (NaBH) was then slowly added to the mixture. 4 ), stirred for 4 hours, centrifuged, dried in a vacuum oven at 70°C overnight, and finally collected the sample Pt / HCNO. The Pt content was 20wt% (ICP).
[0085] Preparation of Pt / C-HCNO
[0086] 100 mg of commercial Pt / C (JM, 40 wt%), 100 mg of HCNO and an appropriate amount of deionized water were poured into a ball mill and milled for 1 h. The mixed solution was then dried under a sodium lamp and finally ground to collect the sample Pt / C-HCNO. The Pt content was 20 wt% (ICP).
[0087] Preparation of membrane electrode
[0088] The membrane electrode was prepared by CCM method, with Pt / HCNO or Pt / C-HCNO as the anode catalyst and commercial Pt / C (JM, 20wt%) as the cathode, and the Pt loading of the anode and cathode was 0.2mg, respectively. Pt / cm 2 and 0.1mg Pt / cm 2 . Take Pt / HCNO or Pt / C-HCNO (6 mg), 5wt% Nafion (41.93 mg) and a certain proportion (the mass ratio of Pt / HCNO and conductive carbon is 1:1.2, 1:1, 1.2:1, 1.5:1) of conductive carbon (XC-72R or SuperP) and dissolve them in 2mL of isopropanol for ultrasonic mixing as anode slurry. Take 11mgPt / C (JM, 20wt%) and 71.236mgNafion solution (5wt%) and dissolve them in 1.5mL of isopropanol for ultrasonic mixing to prepare cathode slurry. At 75°C, the anode and cathode slurries are sprayed on the electrolyte membrane and prepared into membrane electrodes by hot pressing.
[0089] Pt / HCNO Characterization Analysis
[0090] from Fig. 9 It can be seen from the (a) and (b) regions that HCNO is a layered structure and the precious metal Pt is loaded on HCNO. However, due to the small specific surface area of the oxide HCNO, a part of the metal Pt is slightly agglomerated. HRTEM image ( Fig. 9The lattice spacings of regions (c), (d), and (e) are 0.228 nm and 0.230 nm, representing the Pt (111) crystal plane.
[0091] Subsequently, XRD analysis of Pt / HCNO was performed. Fig.10 As shown in the middle (a) area, compared with the standard XRD peak of HCNO, it is found that Pt / HCNO still retains the characteristic peaks of HCNO. In addition, the characteristic peaks at 39.8°, 46.2°, 67.5°, and 81.2° are consistent with the standard PDF card of Pt (PDF#03-065-2868), corresponding to the (111), (200), (220), and (311) crystal planes of Pt, respectively, showing the face-centered cubic structure of Pt. In addition, it is observed that the characteristic peaks of Pt in the spectrum are sharper, which is caused by the agglomeration of Pt particles due to the small specific surface area of HCNO. Fig.10 The middle (b) area is the 4f spectrum of Pt. The two peaks at 74.98 eV and 71.67 eV correspond to Pt 0 4f 5 / 2 and 4f 7 / 2 Track, with standard Pt 0 The peaks (74.40eV, 71.13eV) have a larger binding energy than the peaks (74.40eV, 71.13eV), which is due to the interaction between the carrier and the carrier by providing electrons to the carrier. At the same time, the two peaks at 76.00eV and 72.57eV correspond to Pt 2+ 4f 5 / 2 and 4f 7 / 2 Track, with standard Pt 2+ The peaks (75.70 eV, 72.40 eV) also become larger than the binding energy.
[0092] Pt / HCNO conductive carbon type and ratio screening
[0093] Since the conductivity of oxide is poor, carbon black is added to the anode catalyst layer to assist conductivity. For this reason, the types of conductive carbon were screened, and XC-72R and SuperP were selected as conductive carbons to prepare batteries and used in H 2 -O 2 The test was carried out under the following conditions. The mass ratio of Pt / HCNO to the two conductive carbons was 1:1. Fig.11 As shown in the middle (a), Pt / HCNO-SuperP exhibits 460 mW / cm at 0.4 V. 2 The peak power density of Pt / HCNO-XC-72R is only 282 mW / cm 2, which is much lower than Pt / HCNO-SuperP, so SuperP was finally selected as the auxiliary conductive carbon of the anode catalyst layer. Subsequently, the addition amount of conductive carbon SuperP was explored, such as Fig.11 As shown in the middle (b), different mass ratios of Pt / HCNO and conductive carbon were used to perform H 2 -O 2 The single cell test has a mass ratio of 1.2:1, 1:1, 1:1.2, and 1:1.5. The results show that the best battery performance is achieved when the ratio is 1:1.2, with a peak power density of 1.12W / cm 2 ,and
[0094] Pt / HCNO-SuperP (1.2:1) exhibits the lowest peak power density, which is only 308 mW / cm 2 The peak power density of Pt / HCNO-SuperP (1:1) is only 460 mW / cm 2 , which is much lower than the peak power density of Pt / HCNO-SuperP (1:1.2) and Pt / HCNO-SuperP (1:1.5). This is because the amount of SuperP added is too small, resulting in low anode electronic conductivity, which affects the performance of the catalyst. The peak power density of Pt / HCNO-SuperP (1:1.5) is 817mW / cm 2 , lower than
[0095] Pt / HCNO-SuperP (1:1.2). This is due to excessive SuperP. When a large amount of SuperP is added to the anode catalyst layer, the active sites of Pt are coated with carbon black and cannot play a catalytic role. In summary, SuperP was finally selected as the auxiliary conductive carbon and the mass ratio of Pt / HCNO to it was 1:1.2.
[0096] SEM analysis of Pt / HCNO membrane electrode
[0097] In order to verify whether the SuperP in Pt / HCNO-SuperP (1:1.2) will also cover the metal Pt, SEM analysis of its membrane electrode was performed. Fig.12 As shown, although the addition of SuperP can increase the electronic conductivity, it covers the active sites of Pt. Therefore, in order to further improve the catalyst, the catalyst preparation process was optimized, HCNO was directly added to commercial Pt / C (JM, 40wt%), and the two were combined by high-energy ball milling.
[0098] Morphology Analysis of Pt / C-HCNO
[0099] Fig.13The middle (ad) area shows that the precious metal Pt in Pt / C-HCNO is exposed on the catalyst surface, and the particle size is mainly about 3.5 nm. Compared with the aforementioned Pt / HCNO-SuperP, it is not covered by the C carrier or HCNO. Fig.13 The middle (ef) and (gh) regions show the lattice spacing of HCNO and Pt supported thereon, which are 0.385 nm and 0.227 nm, respectively. This is consistent with the standard PDF cards of HCNO and Pt (PDF#00-040-0884 and PDF#01-087-0642), representing the (100) crystal plane of HCNO and the (111) crystal plane of Pt.
[0100] Further XRD analysis of Pt / C-HCNO was performed. Fig.14 In the middle (a) area, it can be seen that Pt / C-HCNO retains the characteristic peaks of HCNO. At the same time, the characteristic peaks of Pt are located at 39.6°, 46.1°, 67.2° and 80.9°, corresponding to the (111), (200), (220) and (311) crystal planes of Pt, respectively (PDF#01-087-0642). Compared with Pt / HCNO, the diffraction peaks of Pt in Pt / C-HCNO have weaker peak intensity and wider half-peak width, which proves that this method effectively reduces the occurrence of Pt agglomeration. Fig.14 The area (b) is the 4f spectrum of Pt, which is similar to the standard Pt 0 Peak (4f at 74.40 eV 5 / 2 orbital, 4f at 71.13 eV 7 / 2 orbital) compared to Pt 0 Peak (4f at 74.54 eV 5 / 2 orbital, 4f at 71.16 eV 7 / 2 The two peaks at 75.85eV and 72.54eV correspond to Pt 2+ 4f 5 / 2 and 4f 7 / 2 track, compared to the standard Pt 2+ The peaks (75.70 eV, 72.40 eV) shifted positively. This is because the Pt carrier migrated from the carbon support to the HCNO, and the Pt transferred electrons to the HCNO, forming a strong metal-support interaction.
[0101] Pt / C-HCNO single cell test
[0102] In order to verify the battery performance of Pt / HCNO, Pt / HCNO, TZPt / C and Pt / C-HCNO were respectively 2 -O 2 and H 2 - Single battery test was conducted under air condition. Fig.15 As shown in the (a) and (b) regions, in H 2 -O 2 Under these conditions, Pt / C-HCNO exhibited the best battery performance, with a peak power density of 1.31 W / cm 2 , which is 1.37 times that of commercial Pt / C and 1.17 times that of Pt / HCNO. At 0.6V, the current density of Pt / C-HCNO is 1.8A / cm 2 , higher than Pt / HCNO (1.57A / cm 2 ) and TZPt / C(1.37A / cm 2 ). Similarly in H 2 -Air condition, Fig.15 The peak power density of Pt / C-HCNO in the middle (c) and (d) regions is 847.5 mW / cm 2 , 0.6V corresponds to a current density of 1.16A / cm 2 , which is also better than
[0103] Pt / HCNO(717mW / cm 2 , 925mA / cm 2 ) and TZPt / C (327mW / cm 2 , 726mA / cm 2 ). Compared with commercial Pt / C, the addition of HCNO improves the proton transport capacity of the anode catalyst layer, thereby improving the battery performance. In order to further explore its stability, a constant voltage steady-state test was carried out at a voltage of 0.6V for 24h ( Fig.15 (c) and (f) in the middle). The current density of Pt / C-HCNO only decreased by 2%, showing good stability, which is mainly due to the fact that HCNO reduced the occurrence of carbon corrosion.
[0104] Anti-reverse polarity test
[0105] In order to further verify that the protonated layered perovskite HCNO has a certain anti-reverse polarity ability, the anode catalyst Pt / C(TZ) and Pt / C-HCNO were assembled into a battery for anti-reverse polarity test. Fig.16 The middle (a) area is the anti-reversal time of Pt / C (TZ) and Pt / C-HCNO. It is found that within the anti-reversal period of 0-20s, the voltage of commercial Pt / C drops faster than that of Pt / C-HCNO. The time for Pt / C-HCNO to reach the cut-off voltage is 32s, while the anti-reversal time of commercial Pt / C is 30s. Fig.16Regions (b) and (c) in the middle are the performance diagrams of Pt / C(TZ) and Pt / C-HCNO before and after reverse polarity. The power density of Pt / C-HCNO loses 85%, while the power density of Pt / C(TZ) loses 91%, which to some extent shows that HCNO has a certain ability to resist reverse polarity.
[0106] Since the anti-reverse polarity duration of the two is not much different, in order to further prove the anti-reverse polarity ability of HCNO, the impedance test of the membrane electrode before and after the reversal was carried out. Fig.17 As shown in the middle (a) and (c), the impedance of Pt / C (TZ) and Pt / C-HCNO before anti-reversal is not much different, proving that the insufficient conductivity of HCNO has no effect on the electronic conductivity of the membrane electrode. Then, the impedance of Pt / C (TZ) and Pt / C-HCNO after anti-reversal was tested, as shown in Figure 1. Fig.17 As shown in the middle (b) and (d) regions, it is found that the impedance of Pt / C(TZ) and Pt / C-HCNO both increase, but the impedance of Pt / C-HCNO is much smaller than that of Pt / C(TZ). This is because HCNO can transfer protons, making up for the insufficient proton supply at the reverse pole and preventing the occurrence of carbon corrosion.
[0107] In summary, in this embodiment, the research is mainly carried out around two major purposes. One is to improve the proton transfer capacity of the anode catalyst layer to achieve the purpose of improving battery performance, and the other is to alleviate the carbon corrosion problem caused by anti-reverse polarity, thereby improving the durability of the battery. To this end, HCNO is used in the preparation of anode catalysts, and the preparation process is optimized. On the one hand, HCNO has a certain proton conduction ability, which can improve the proton transfer capacity of the anode catalyst, thereby further improving the catalyst performance. On the other hand, HCNO is an oxide and has a certain hydrophilicity. It can promote the reverse diffusion of water in the membrane, diffuse the water accumulated on the cathode side back to the anode, and generate hydrogen protons and electrons through the OER reaction, which makes up for the supply of anode protons and avoids the occurrence of carbon corrosion. The specific contents are summarized as follows:
[0108] (1) First, Pt / HCNO was obtained by loading the precious metal Pt with HCNO as the anode carrier through the sodium borohydride reduction method. Characterizations such as XRD and SEM showed that the surface Pt particles agglomerated, reducing the utilization rate of Pt. In addition, since HCNO is a metal oxide, carbon black was added to make up for the lack of conductivity. Therefore, different types of carbon black and addition ratios were screened, and finally SuperP was used as the auxiliary conductive carbon, with a mass ratio of Pt / HCNO to SuperP of 1.2:1. Subsequently, in order to verify its battery performance, Pt / HCNO was assembled into a membrane electrode and in H 2 -O 2The single cell test was carried out under the same conditions, and 1.12W / cm was achieved at 0.45V. 2 The peak power density at H 2 -Under Air conditions, it also reached 717mW / cm 2 The peak power density of Pt / C is higher than that of commercial Pt / C.
[0109] (2) Since the synthesis method of Pt / HCNO is relatively complicated and the surface Pt particles are prone to agglomeration, the performance of the catalyst is hindered. To this end, the catalyst preparation process was optimized, and commercial Pt / C and HCNO were physically mixed by simple ball milling to synthesize Pt / C-HCNO, which simplified the synthesis method and ensured the uniform dispersion of the precious metal Pt. This idea was also confirmed by XRD and SEM. In order to further evaluate the HOR performance of the catalyst, Pt / C-HCNO was prepared into a film electrode and heated to 40 ℃ for 2 h. 2 -O 2 and H 2 - Single cell test under Air conditions, the peak power density is 1.31W / cm 2 and 847.5mW / cm 2 , which is 1.17 and 1.18 times of Pt / HCNO tested under the same conditions, and 1.37 and 1.35 times of commercial Pt / C. Constant voltage steady-state test was also carried out on it, maintaining a constant voltage of 0.6V for 24 hours, and its current density loss was within 3%. It proves that the catalyst has good catalytic performance and stability.
[0110] (3) Finally, the Pt / C-HCNO was subjected to anti-reverse polarity test and impedance test. It was found that Pt / C-HCNO reached the cutoff voltage later than commercial Pt / C, and its impedance change before and after the reversal was much smaller than that of commercial Pt / C, which proved that HCNO has a certain anti-reversal ability.
[0111] The above is only a preferred implementation of the patent of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the patent of the present invention. These improvements and modifications should also be regarded as the scope of protection of the patent of the present invention.
Claims
1. A method for preparing a protonated perovskite anode additive, characterized in that: The preparation method is specifically as follows: solid phase synthesis method is used to prepare KCa2Nb3O 10 Then acid replacement was performed to obtain HCa2Nb3O 10 That is the protonated perovskite anode additive.
2. The method for preparing the protonated perovskite anode additive according to claim 1, characterized in that: KCa2Nb3O 10 The preparation method is as follows: K2CO3, CaCO3 and Nb2O5 are mixed and ball-milled, and then dried, calcined, ground and re-fired to obtain the mixture.
3. The method for preparing the protonated perovskite anode additive according to claim 2, characterized in that: The mass ratio of K2CO3, CaCO3 and Nb2O5 is (0.5-1.2):(1.5-3):(3-6).
4. The method for preparing the protonated perovskite anode additive according to claim 2, characterized in that: The conditions for ball milling are: 200-500 rpm, 0.5-2 h; The calcination conditions are: 1000-1500°C, 10-15h; The conditions for re-firing are: 1000-1500℃, 10-15h.
5. The method for preparing the protonated perovskite anode additive according to claim 1, characterized in that: KCa2Nb3O 10 The specific method of acid replacement is: KCa2Nb3O 10 After soaking in HCl at room temperature, it is obtained by centrifugation and drying.
6. The method for preparing the protonated perovskite anode additive according to claim 5, characterized in that: KCa2Nb3O 10 The ratio with HCl is (2-5) g: (80-150) ml, and the HCl concentration is 5-10 mol / L.
7. The method for preparing the protonated perovskite anode additive according to claim 5, characterized in that: The soaking time is 40-50 hours, and the HCl is replaced every 20-25 hours. Drying conditions: 60-80℃.
8. A method for preparing an anode catalyst, characterized in that: The protonated perovskite anode additive HCa2Nb3O prepared by any method of claims 1-7 10 The catalyst is mixed with a Pt / C catalyst having a Pt content of 40 wt% in a mass ratio of 1:(0.8-1.5), ball-milled for 0.5-1.5 hours, and then dried and ground to obtain the catalyst.
9. A method for preparing a membrane electrode, characterized in that: The anode catalyst prepared by the method described in claim 8, 5wt% Nafion solution and conductive carbon are dispersed in an alcohol solution in a mass ratio of 1:(5-8):(0.8-1.5) to prepare an anode slurry, and then the anode slurry is sprayed on the electrolyte membrane at 70-85°C and hot-pressed to obtain the anode slurry.
10. Use of the membrane electrode prepared by the method according to claim 9 as an anode in a proton exchange membrane fuel cell.