Power ferrite material, preparation method thereof and automobile electronic product

By adjusting the composition ratio and additives of manganese-zeb ferrite materials, moving its valley point and reducing the inductance value, the problem of high AC resistance value in the prior art is solved, and the application performance of UF40 products in the automotive field is improved.

CN119019162AActive Publication Date: 2024-11-26HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411135034.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The prior art has failed to effectively reduce the alternating resistance (ACR) value of manganese-zeb ferrite materials, especially in the automotive field, where challenges exist in the special application environment of UF40 products.

Method used

By adjusting the composition ratio of the matrix material and additives, the valley point of the material is moved to the negative temperature direction, and by adding iron elements and matching Co2O3 components, the inductance value of the material is reduced, thereby reducing the AC resistance.

Benefits of technology

The AC resistance value reduction at 25℃, 200kHz and 0.5V conditions is achieved, and the application effect and reliability of UF40 products in automotive electronic equipment is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004999154810000091
    Figure BDA0004999154810000091
  • Figure BDA0004999154810000111
    Figure BDA0004999154810000111
  • Figure BDA0004999154810000131
    Figure BDA0004999154810000131
Patent Text Reader

Abstract

The invention provides a power ferrite material and a preparation method thereof, and an automobile electronic product, the power ferrite material comprises a base material and an additive, the base material comprises the following components by mole percentage: 52.95-53.25 mol% of Fe2O3; the content of MnO is 36.55 to 37.05 mol%; the content of ZnO is 9.7 to 10.5 mol%; the additive is prepared from the following components in percentage by mass: 0.13-0.18% of CaCO3, 0.18-0.18% of CaCO3, 0.18-0.18% of CaCO3, 0.18-0.18% And 0.2 to 0.33 percent of Co2O3. By regulating and controlling the composition of the power ferrite material, the alternating current resistance (ACR) value of the power ferrite material under the conditions of 25 DEG C, 200kHz and 0.5 V is reduced, so that the UF40 product can be conveniently applied to the field of automobiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ferrite materials, and in particular relates to a power ferrite material and a preparation method thereof, and an automotive electronic product. Background Art

[0002] In recent years, with the rapid development of the electronic information industry, the demand for manganese zinc ferrite has shown a steady growth trend. Especially in emerging fields such as new energy vehicles, 5G communications and industrial automation, the application prospects of manganese zinc ferrite are even broader. These fields have increasingly higher performance requirements for electronic components, and manganese zinc ferrite can meet these high requirements with its excellent magnetic properties.

[0003] The manganese-zinc ferrite used in the prior art is mainly divided into two categories: power manganese-zinc ferrite and high-conductivity manganese-zinc ferrite. Among them, power manganese-zinc ferrite materials are mainly used in electronic transformers of various switching power supplies to realize functions such as voltage conversion, current conversion and impedance conversion. The switching power supply transformer needs to maintain good electromagnetic properties at higher frequencies and larger currents, so it needs to have the characteristics of low power loss, high saturation magnetic induction intensity and wide temperature range. High-conductivity manganese-zinc ferrite materials are mainly used in broadband transformers and pulse transformers in the fields of digital networks and communication systems. The electronic transformers in the above fields have high requirements on the material volume and magnetic permeability, so they need to have characteristics such as broadband high magnetic permeability, high Curie temperature and high impedance.

[0004] For example, CN116283263A discloses that the power loss of ferrite material under the conditions of 100°C, 100kHz and 200mT is 268kW / m 3 CN114685154A discloses a high-frequency, wide-temperature, ultra-low-loss ferrite material with a power loss of 240-265kW / m at 100°C, 200kHz and 125mT. 3 .

[0005] However, in the automotive field, some special application environments require reducing the alternating current resistance (ACR) value of products (such as UF40), but the above technical solutions disclosed in the prior art do not involve how to reduce the ACR value of manganese-zinc ferrite materials.

[0006] Therefore, in the art, there is an urgent need to develop a product for reducing the ACR value of manganese-zinc ferrite materials and a preparation method thereof. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention aims to provide a power ferrite material and a preparation method thereof and an automotive electronic product. The present invention adjusts the composition of the power ferrite material to reduce its AC resistance (ACR) value under the conditions of 25°C, 200kHz and 0.5V, thereby facilitating the application of UF40 products in the automotive field.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a power ferrite material, wherein the power ferrite material is composed of a base material and an additive:

[0010] In terms of mole percentage, the matrix material comprises:

[0011] Fe2O3 52.95-53.25mol%;

[0012] MnO 36.55-37.05mol%;

[0013] ZnO 9.7-10.5mol%;

[0014] Taking the total mass of the matrix material as 100%, the additive comprises:

[0015] CaCO3 0.13-0.18%;

[0016] Co2O3 0.2-0.33%.

[0017] The present invention adjusts the content ratio of each component in the matrix material and the additive so that the valley point moves toward the negative temperature direction, so that the power ferrite material not only has high saturation magnetic induction intensity (Bs), high magnetic permeability and low loss performance, but also further reduces its AC resistance (ACR) value under 25°C, 200kHz and 0.5V conditions, so that the UF40 product can better adapt to various special environments in the automotive field, thereby improving its application effect and reliability in automotive electronic equipment.

[0018] The principle of the present invention is that: the present invention finds that reducing the AC resistance (ACR) of a material or the AC resistance (ACR) value of a product can be achieved by reducing the inductance value (L) of the material. The specific principle is referred to the following formula: ACR=2πfL / Q, where f is the frequency, the unit is Hz; L is the inductance value, the unit is H; and Q value is the quality factor.

[0019] In terms of reducing the inductance of the material, the present invention moves the valley point of the material outside the required temperature point. For example, the present invention requires reducing the AC resistance (ACR) value of the UF40 product at 25°C, 200kHz and 0.5V. The present invention moves the valley point to less than 25°C, for example, adjusts it at 10°C, thereby reducing the inductance of the material at 25°C.

[0020] In addition, the present invention also found that by increasing the content of iron, the valley point of the material can be moved toward the negative temperature direction, but this requires the combination of Co2O3 components to achieve the above effect. In summary, on the one hand, the present invention reduces the resistivity of the material, and on the other hand, it also uses the valley point of the mobile material to a suitable range, and finally reduces the inductance of the material at 25°C, so that the AC resistance (ACR) value of the UF40 product at 25°C, 200kHz and 0.5V is correspondingly reduced. In addition, the inductance of the material is closely related to its physical properties, such as the thickness of the grain boundary, which can affect the electronic transmission characteristics and magnetic properties of the material. If the amount of CaCO3 component precipitated at the grain boundary is too small, the inductance value of the material increases, so the AC resistance of the material will also increase accordingly.

[0021] In the present invention, the molar percentage of Fe2O3 is 52.95-53.25 mol%, for example, it can be 52.95 mol%, 53.0 mol%, 53.05 mol%, 53.08 mol%, 53.1 mol%, 53.15 mol%, 53.18 mol%, 53.2 mol%, 53.25 mol%, etc.

[0022] In the present invention, the molar percentage of MnO is 36.55-37.05 mol%, for example, it can be 36.55 mol%, 36.58 mol%, 36.6 mol%, 36.65 mol%, 36.7 mol%, 36.8 mol%, 36.9 mol%, 37.0 mol%, 37.05 mol%, etc.

[0023] In the present invention, the molar percentage of ZnO is 9.7-10.5 mol%, for example, it can be 9.7 mol%, 9.8 mol%, 9.9 mol%, 10.0 mol%, 10.2 mol%, 10.5 mol%, etc.

[0024] In the present invention, based on the total mass of the matrix material as 100%, the mass percentage of the CaCO3 is 0.13-0.18%, for example, it can be 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, etc.

[0025] In the present invention, based on the total mass of the matrix material as 100%, the mass percentage of the Co2O3 is 0.2-0.33%, for example, it can be 0.2%, 0.22%, 0.25%, 0.28%, 0.3%, 0.33%, etc.

[0026] In the present invention, the ratio of the matrix material components needs to be controlled within the above content range. If the iron content is too high, the material's valley point will move to a negative temperature, causing the Q value to decrease, and ultimately increasing the material's AC resistance; if the iron content is too low, the material's ACR will also be too high, because the material's inductance is too large.

[0027] In addition, the present invention adjusts the MnO content range so that the valley point of the material is within an appropriate range. If the MnO content is too low, the valley point of the material will move toward 25°C, and the inductance of the material will increase, and the ACR will also increase accordingly.

[0028] In the present invention, the content of the Co2O3 additive is regulated so that the material has a smaller AC resistance. If the amount of Co2O3 added is too high, the Q value of the material will become smaller, and the AC resistance will increase accordingly; if the amount of Co2O3 added is too low, the Q value will also become smaller, and the AC resistance will increase accordingly.

[0029] Preferably, the valley point of the power ferrite material is 15°C.

[0030] Preferably, the AC resistance of the power ferrite material under the conditions of 25° C., 200 kHz and 0.5 V is less than 235 mΩ.

[0031] The invention reduces the AC resistance of the power ferrite material under the conditions of 25° C., 200 kHz and 0.5V by regulating the valley point of the power ferrite material.

[0032] In a second aspect, the present invention provides a method for preparing the power ferrite material according to the first aspect, the method comprising the following steps:

[0033] (1) subjecting the base material to a first sand grinding treatment, a first spray granulation treatment and a pre-calcining treatment in sequence according to the formula amount to obtain a pre-calcined material;

[0034] (2) subjecting the additives and the pre-burnt material obtained in step (1) to a second sand grinding treatment, a second spray granulation treatment, a press molding treatment and a sintering treatment in sequence according to the formula amount to obtain the power ferrite material.

[0035] Preferably, the mass ratio of the first powder, the first sanding balls and the first grinding aid in the first sanding treatment in step (1) is 1:(6-8):(0.6-0.7), for example, it can be 1:6:0.6, 1:6.5:0.65, 1:7:0.65, 1:7.5:0.6, 1:8:0.7, etc.

[0036] Preferably, the first grinding aid comprises water.

[0037] Preferably, the time of the first sanding treatment in step (1) is 60-70 min, for example, 60 min, 62 min, 65 min, 68 min, 70 min, etc.

[0038] Preferably, the average particle size of the powder after the first sand grinding treatment in step (1) is 0.65 μm-0.9 μm, for example, it can be 0.66 μm, 0.68 μm, 0.72 μm, 0.78 μm, 0.81 μm, 0.85 μm, 0.9 μm, etc.

[0039] Preferably, the mass concentration of the first glue used in the first spray granulation treatment in step (1) is 5%-15%, for example, it can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 11%, 12%, 13%, 14%, 15%, etc.

[0040] Preferably, based on the total mass of the pre-sintered material in step (1) being 100%, the mass percentage of the first glue is 10%.

[0041] Preferably, the temperature of the pre-calcination treatment in step (1) is 850° C., and the time is 1-5 h, for example, 1 h, 2 h, 3 h, 4 h, 5 h, etc.

[0042] Preferably, the mass ratio of the second powder, the second sanding balls and the second grinding aid in the second sanding treatment in step (2) is 1:(6-8):(0.6-0.7), for example, it can be 1:6:0.6, 1:6.5:0.65, 1:7:0.65, 1:7.5:0.6, 1:8:0.7, etc.

[0043] Preferably, the second grinding aid comprises water.

[0044] Preferably, the time for the second sanding treatment in step (2) is 150-240 min, for example, it can be 150 min, 165 min, 185 min, 200 min, 220 min, 240 min, etc.

[0045] Preferably, the average particle size of the powder after the second sand milling treatment in step (2) is 0.95 μm-1.15 μm, for example, it can be 0.98 μm, 1.01 μm, 1.05 μm, 1.1 μm, 1.12 μm, 1.15 μm, etc.

[0046] Preferably, the mass concentration of the second glue used in the second spray granulation treatment in step (2) is 5%-15%, for example, it can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 11%, 12%, 13%, 14%, 15%, etc.

[0047] Preferably, based on the total mass of the powder in the second sanding treatment in step (2) being 100%, the mass percentage of the second glue is 10%.

[0048] Preferably, the sintering temperature in step (2) is 1260°C-1300°C, for example, 1260°C, 1270°C, 1280°C, 1290°C, 1300°C, etc.; the sintering time is 5-7h, for example, 5h, 6h, 7h, etc.

[0049] In a third aspect, the present invention provides an automotive electronic product, comprising the power ferrite material according to the first aspect.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] The present invention provides a power ferrite material. By adjusting the content ratio of each component in a base material and an additive, the valley point is moved toward a negative temperature direction. Thus, the power ferrite material not only has high saturation magnetic induction intensity (Bs), high magnetic permeability and low loss performance, but also further reduces its AC resistance (ACR) value under the conditions of 25°C, 200kHz and 0.5V. Therefore, the UF40 product can better adapt to various special environments in the automotive field, thereby improving its application effect and reliability in automotive electronic equipment.

[0052] The principle of the present invention is that: the present invention finds that reducing the AC resistance (ACR) of a material or the AC resistance (ACR) value of a product can be achieved by reducing the inductance value (L) of the material. The specific principle is referred to the following formula: ACR=2πfL / Q, where f is the frequency, the unit is Hz; L is the inductance value, the unit is H; and Q value is the quality factor.

[0053] In terms of reducing the inductance of the material, the present invention moves the valley point of the material outside the required temperature point. For example, the present invention requires reducing the AC resistance (ACR) value of the UF40 product at 25°C, 200kHz and 0.5V. The present invention moves the valley point to less than 25°C, for example, adjusts it at 10°C, thereby reducing the inductance of the material at 25°C.

[0054] In addition, the present invention also found that by increasing the content of iron, the valley point of the material can be moved toward the negative temperature direction, but this requires the combination of Co2O3 components to achieve the above effect. In summary, on the one hand, the present invention reduces the resistivity of the material, and on the other hand, it also uses the valley point of the mobile material to a suitable range, and finally reduces the inductance of the material at 25°C, so that the AC resistance (ACR) value of the UF40 product at 25°C, 200kHz and 0.5V is correspondingly reduced. In addition, the inductance of the material is closely related to its physical properties, such as the thickness of the grain boundary, which can affect the electronic transmission characteristics and magnetic properties of the material. If the amount of CaCO3 component precipitated at the grain boundary is too small, the inductance value of the material increases, so the AC resistance of the material will also increase accordingly. DETAILED DESCRIPTION

[0055] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0056] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art.

[0057] Example 1

[0058] This embodiment provides a power ferrite material with a valley point of 15° C. The AC resistance of the power ferrite material under the conditions of 25° C., 200 kHz and 0.5 V is less than 235 mΩ. The power ferrite material is composed of a base material and an additive:

[0059] In terms of molar percentage, the matrix material includes: 52.95 mol% of Fe2O3, 36.55 mol% of MnO and 10.5 mol% of ZnO; based on the total mass of the matrix material being 100%, the additives include: 0.13% of CaCO3 and 0.3% of Co2O3.

[0060] This embodiment also provides a method for preparing the above-mentioned power ferrite material, which comprises the following steps:

[0061] (1) The base material is subjected to a first sand grinding treatment according to the formula, and the first sand grinding treatment is carried out for 70 minutes in a mass ratio of powder, sand grinding balls and water of 1:7:0.65 to obtain a powder with an average particle size of 0.75 μm; based on the total mass of the pre-burned material being 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a first spray granulation treatment and a pre-burning treatment at 850° C. in a rotary kiln for 3 hours to obtain a pre-burned material;

[0062] (2) subjecting the additives and the pre-burnt material obtained in step (1) to a second sand milling treatment according to the formula amount, and subjecting the second sand milling treatment to a mass ratio of powder, sand milling balls and water of 1:7:0.65 for 200 minutes to obtain a powder with an average particle size of 0.98 μm; taking the total mass of the powder in the second sand milling treatment as 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a second spray granulation treatment, a press molding treatment and a sintering treatment at 1280° C. for 6 hours in sequence to obtain the power ferrite material.

[0063] Comparative Example 1

[0064] This comparative example provides a power ferrite material, which is composed of a base material and an additive:

[0065] In terms of molar percentage, the matrix material includes: 52.3 mol% of Fe2O3, 37.2 mol% of MnO and 10.5 mol% of ZnO; based on the total mass of the matrix material being 100%, the additives include: 0.13% of CaCO3 and 0.3% of Co2O3.

[0066] This comparative example also provides a method for preparing the above-mentioned power ferrite material, which comprises the following steps:

[0067] (1) The base material is subjected to a first sand grinding treatment according to the formula, and the first sand grinding treatment is carried out for 70 minutes in a mass ratio of powder, sand grinding ball and water of 1:7:0.65 to obtain a powder with an average particle size of 0.78 μm; based on the total mass of the pre-burned material being 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a first spray granulation treatment and a pre-burning treatment at 850° C. in a rotary kiln for 3 hours to obtain a pre-burned material;

[0068] (2) subjecting the additives and the pre-burnt material obtained in step (1) to a second sand milling treatment according to the formula amount, and subjecting the second sand milling treatment to a mass ratio of powder, sand milling balls and water of 1:7:0.65 for 200 minutes to obtain a powder with an average particle size of 0.99 μm; taking the total mass of the powder in the second sand milling treatment as 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a second spray granulation treatment, a press molding treatment and a sintering treatment at 1280° C. for 6 hours in sequence to obtain the power ferrite material.

[0069] The AC resistance of the power ferrite materials obtained in Example 1 and Comparative Example 1 was measured, and the results are shown in Table 1:

[0070] Table 1

[0071]

[0072] From the results in Table 1, it can be seen that the low iron content leads to a high AC resistance of the power ferrite material at 25°C, 200kHz and 0.5V.

[0073] Example 2

[0074] This embodiment provides a power ferrite material with a valley point of 15° C. The AC resistance of the power ferrite material under the conditions of 25° C., 200 kHz and 0.5 V is less than 235 mΩ. The power ferrite material is composed of a base material and an additive:

[0075] In terms of molar percentage, the matrix material includes: 53.25 mol% of Fe2O3, 37.05 mol% of MnO and 9.7 mol% of ZnO; based on the total mass of the matrix material being 100%, the additives include: 0.18% of CaCO3 and 0.25% of Co2O3.

[0076] This embodiment also provides a method for preparing the above-mentioned power ferrite material, which comprises the following steps:

[0077] (1) The base material is subjected to a first sand grinding treatment according to the formula, and the first sand grinding treatment is carried out for 60 minutes in a mass ratio of powder, sand grinding balls and water of 1:7:0.65 to obtain a powder with an average particle size of 0.82 μm; based on the total mass of the pre-burned material being 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a first spray granulation treatment and a pre-burning treatment at 850° C. in a rotary kiln for 4 hours to obtain a pre-burned material;

[0078] (2) subjecting the additives and the pre-burnt material obtained in step (1) to a second sand milling treatment according to the formula amount, and subjecting the second sand milling treatment to a mass ratio of powder, sand milling balls and water of 1:7:0.65 for 190 minutes to obtain a powder with an average particle size of 0.99 μm; taking the total mass of the powder in the second sand milling treatment as 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a second spray granulation treatment, a press molding treatment and a sintering treatment at 1290° C. for 7 hours in sequence to obtain the power ferrite material.

[0079] Comparative Example 2

[0080] This comparative example provides a power ferrite material, which is composed of a base material and an additive:

[0081] In terms of molar percentage, the matrix material includes: 53.25 mol% of Fe2O3, 37.05 mol% of MnO and 9.7 mol% of ZnO; based on the total mass of the matrix material being 100%, the additives include: 0.18% of CaCO3 and 0.45% of Co2O3.

[0082] This comparative example also provides a method for preparing the above-mentioned power ferrite material, which comprises the following steps:

[0083] (1) The base material is subjected to a first sand grinding treatment according to the formula, and the first sand grinding treatment is carried out for 60 minutes in a mass ratio of powder, sand grinding ball and water of 1:6:0.55 to obtain a powder with an average particle size of 0.85 μm; based on the total mass of the pre-burned material being 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a first spray granulation treatment and a pre-burning treatment at 850° C. in a rotary kiln for 4 hours to obtain a pre-burned material;

[0084] (2) subjecting the additives and the pre-burnt material obtained in step (1) to a second sand milling treatment according to the formula amount, and subjecting the second sand milling treatment to a mass ratio of powder, sand milling balls and water of 1:7:0.65 for 190 minutes to obtain a powder with an average particle size of 0.98 μm; taking the total mass of the powder in the second sand milling treatment as 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a second spray granulation treatment, a press molding treatment and a sintering treatment at 1290° C. for 7 hours in sequence to obtain the power ferrite material.

[0085] The AC resistance of the power ferrite materials obtained in Example 2 and Comparative Example 2 was measured, and the results are shown in Table 2:

[0086] Table 2

[0087]

[0088] It can be seen from the results in Table 2 that the content of Co2O3 is not within the preferred range of the present invention, resulting in a relatively high AC resistance of the power ferrite material under the conditions of 25°C, 200kHz and 0.5V.

[0089] Example 3

[0090] This embodiment provides a power ferrite material with a valley point of 15° C. The AC resistance of the power ferrite material under the conditions of 25° C., 200 kHz and 0.5 V is less than 235 mΩ. The power ferrite material is composed of a base material and an additive:

[0091] In terms of molar percentage, the matrix material includes: 53.0 mol% of Fe2O3, 37.0 mol% of MnO and 10.0 mol% of ZnO; based on the total mass of the matrix material being 100%, the additives include: 0.15% of CaCO3 and 0.2% of Co2O3.

[0092] This embodiment also provides a method for preparing the above-mentioned power ferrite material, which comprises the following steps:

[0093] (1) The base material is subjected to a first sand grinding treatment according to the formula, and the first sand grinding treatment is carried out for 60 minutes in a mass ratio of powder, sand grinding balls and water of 1:7:0.65 to obtain a powder with an average particle size of 0.86 μm; based on the total mass of the pre-burned material being 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a first spray granulation treatment and a pre-burning treatment at 850° C. in a rotary kiln for 3 hours to obtain a pre-burned material;

[0094] (2) subjecting the additives and the pre-burnt material obtained in step (1) to a second sand milling treatment according to the formula amount, and subjecting the second sand milling treatment to a mass ratio of powder, sand milling balls and water of 1:7:0.65 for 180 minutes to obtain a powder with an average particle size of 0.96 μm; taking the total mass of the powder in the second sand milling treatment as 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a second spray granulation treatment, a press molding treatment and a sintering treatment at 1290° C. for 6 hours in sequence to obtain the power ferrite material.

[0095] Comparative Example 3

[0096] This comparative example provides a power ferrite material, which is composed of a base material and an additive:

[0097] In terms of molar percentage, the matrix material includes: 53.0 mol% of Fe2O3, 37.0 mol% of MnO and 10.0 mol% of ZnO; based on the total mass of the matrix material being 100%, the additives include: 0.05% of CaCO3 and 0.2% of Co2O3.

[0098] This comparative example also provides a method for preparing the above-mentioned power ferrite material, which comprises the following steps:

[0099] (1) The base material is subjected to a first sand grinding treatment according to the formula, and the first sand grinding treatment is carried out for 60 minutes in a mass ratio of powder, sand grinding balls and water of 1:7:0.65 to obtain a powder with an average particle size of 0.84 μm; based on the total mass of the pre-burned material being 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a first spray granulation treatment and a pre-burning treatment at 850° C. in a rotary kiln for 3 hours to obtain a pre-burned material;

[0100] (2) subjecting the additives and the pre-burnt material obtained in step (1) to a second sand milling treatment according to the formula amount, and subjecting the second sand milling treatment to a mass ratio of powder, sand milling balls and water of 1:7:0.65 for 180 minutes to obtain a powder with an average particle size of 0.95 μm; taking the total mass of the powder in the second sand milling treatment as 100%, a polyvinyl alcohol solution with a mass percentage content of 10% (mass concentration of 7.5%) is then added to perform a second spray granulation treatment, a press molding treatment and a sintering treatment at 1290° C. for 6 hours in sequence to obtain the power ferrite material.

[0101] The AC resistance of the power ferrite materials obtained in Example 3 and Comparative Example 3 was measured, and the results are shown in Table 3:

[0102] Table 3

[0103]

[0104] It can be seen from the results in Table 3 that the CaCO3 content is not within the preferred range of the present invention, resulting in a relatively high AC resistance of the power ferrite material under the conditions of 25°C, 200kHz and 0.5V.

[0105] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A power ferrite material, characterized in that: The power ferrite material is composed of a base material and additives: In terms of mole percentage, the matrix material comprises: Fe2O3 52.95-53.25mol%; MnO 36.55-37.05mol%; ZnO 9.7-10.5mol%; Taking the total mass of the matrix material as 100%, the additive comprises: CaCO3 0.13-0.18%; Co2O3 0.2-0.33%.

2. The power ferrite material according to claim 1, characterized in that: The valley point of the power ferrite material is 15°C.

3. The power ferrite material according to claim 1 or 2, characterized in that: The AC resistance of the power ferrite material under the conditions of 25° C., 200 kHz and 0.5 V is less than 235 mΩ.

4. A method for preparing a power ferrite material according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: (1) subjecting the base material to a first sand grinding treatment, a first spray granulation treatment and a pre-calcining treatment in sequence according to the formula amount to obtain a pre-calcined material; (2) subjecting the additives and the pre-burnt material obtained in step (1) to a second sand grinding treatment, a second spray granulation treatment, a press molding treatment and a sintering treatment in sequence according to the formula amount to obtain the power ferrite material.

5. The method according to claim 4, characterized in that In the first sanding treatment in step (1), the mass ratio of the first powder, the first sanding balls and the first grinding aid is 1:(6-8):(0.6-0.7); Preferably, the first grinding aid comprises water; Preferably, the first sanding treatment in step (1) is performed for 60-70 minutes; Preferably, the average particle size of the powder after the first sand grinding treatment in step (1) is 0.65 μm-0.9 μm.

6. The method according to claim 4 or 5, characterized in that: The mass concentration of the first glue used in the first spray granulation process in step (1) is 5%-15%; Preferably, based on the total mass of the pre-sintered material in step (1) being 100%, the mass percentage of the first glue is 10%.

7. The method according to any one of claims 4 to 6, characterized in that: The temperature of the pre-calcination treatment in step (1) is 850° C. and the time is 1-5 hours.

8. The method according to any one of claims 4 to 7, characterized in that: The mass ratio of the second powder, the second sanding balls and the second grinding aid in the second sanding treatment in step (2) is 1:(6-8):(0.6-0.7); Preferably, the second grinding aid comprises water; Preferably, the second sanding treatment in step (2) lasts for 150-240 minutes; Preferably, the average particle size of the powder after the second sand milling treatment in step (2) is 0.95 μm-1.15 μm.

9. The method according to any one of claims 4 to 8, characterized in that: The mass concentration of the second glue used in the second spray granulation process in step (2) is 5%-15%; Preferably, based on the total mass of the powder in the second sanding process in step (2) being 100%, the mass percentage of the second glue is 10%; Preferably, the sintering treatment in step (2) is carried out at a temperature of 1260° C.-1300° C. and for a time of 5-7 hours.

10. An automotive electronic product, characterized in that: The automotive electronic product comprises the power ferrite material according to any one of claims 1-3.

Citation Information

Patent Citations

  • Manganese zinc ferrite core

    CN104103394A

  • MnZn power ferrite for MHz-level switching mode power supply and preparation method of MnZn power ferrite

    CN108424136A

  • Power ferrite material as well as preparation method and application thereof

    CN115677337A

  • Wide-temperature material applied to low-frequency band and preparation method of wide-temperature material

    CN115745593A

  • Manganese-zinc-ferrite

    EP0763507A1