Powerful non-toxic antibacterial and antiviral nano functional material as well as preparation and application thereof
Through the preparation of nano-copper oxide and m-dichlorophenyl ketone composite materials, the problem of traditional textile antibacterial agents being harmful to the human body and weakening their effects is solved, and the textile maintains strong antibacterial properties after washing green health solutions.
Patent Information
- Application Number
- CN202411107133.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The chemical additives used in traditional textile antibacterial and antiviral methods are harmful to human health, and the antibacterial effect is weakened over time, making it difficult to remain effective after repeated use and washing.
Using nano-copper oxide and m-dichlorophenyl ketone composite materials, powerful non-toxic antibacterial and antiviral nanofunctional materials are prepared through borohydrogenation, electrocarboxylation and ultrasonic dispersion, and textiles are modified to improve Its antibacterial and antiviral properties.
It has achieved that textiles still maintain good antibacterial and antiviral effects after repeated use and washing, and the materials are natural, non-toxic, green and environmentally friendly, which significantly improves the antibacterial effects.
Smart Images

Figure CN119019443A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of nano materials, and particularly relates to a nano functional material with strong non-toxic antibacterial and antiviral properties and its preparation and application. Background Art
[0002] With the development of economy and society, people's awareness of self-care and environment is also increasing, and the demand for special functional textiles for various purposes is also growing sharply. Health is still one of the most concerned topics. However, bacteria are everywhere, and there are many harmful bacteria. Their spread and spread seriously threaten human health. Therefore, in order to control the growth and reproduction of harmful bacteria and reduce the harm that bacteria may cause, research and development of antibacterial functional textiles has become a hot spot in the field of scientific research and production. The traditional antibacterial and antiviral methods of textiles are mainly achieved by adding chemical antibacterial agents or antiviral agents, but these chemical additives may cause certain harm to human health, and the antibacterial effect on textiles will gradually weaken over time. Summary of the invention
[0003] The purpose of the present invention is to provide a strong, non-toxic, antibacterial and antiviral nano-functional material for modifying textiles, as well as its preparation and application.
[0004] Specifically, the present invention provides, on one hand, a potent, non-toxic, antibacterial and antiviral nano-functional material as described in formula (I).
[0005]
[0006] In one aspect, the present invention provides a method for preparing a potent, non-toxic, antibacterial and antiviral nano-functional material as described in formula (I):
[0007] S1: Formula (A) The product is subjected to hydroboration and oxidation reaction with pinacol diboron ester, ferrous chloride and alkaline organic solution, extracted, washed with saturated brine, dried, spin-dried, purified by column, and then evaporated to obtain the product of formula (B)
[0008] S2: Take formula (D) Put it into a reaction kettle, add acetonitrile and tetraethylammonium tetrafluoroborate, carry out electrocarboxylation reaction under constant voltage and CO2 conditions, extract, adjust pH value, and obtain formula (E) The formula (B) and the formula (E) described in step S1 are mixed, distilled water is added, and the formula (C) is obtained under the action of a catalyst.
[0009] S3: dissolving the compound (C) obtained in step S2 in an organic solvent, adding the pretreated nano copper oxide, ultrasonically dispersing, and rotary evaporating to obtain a potent, non-toxic, antibacterial and antiviral nano functional material of formula (I).
[0010] In one or more embodiments, the alkaline organic solution in step S1 is preferably one or more of triethylamine, triethylenediamine, lithium tert-butoxide, potassium tert-butoxide, and sodium tert-butoxide; the organic solvent in step S3 is one of ethanol, acetone, ether, or ethylene glycol.
[0011] In one or more embodiments, in step S1, the molar ratio of the ferrous chloride solution, the alkaline organic solution and the pinacol diboron ester is preferably 1:(15-18):(20-25); the reaction temperature of step S1 is 30-45°C; and the reaction time is 10-18h.
[0012] In one or more embodiments, step S1 further comprises a step of pumping and filling argon gas; the number of times of pumping and filling argon gas is preferably 2 to 5 times.
[0013] In one or more embodiments, in step S2, the CO2 passing time is 0.5 to 1 h. The concentration of tetraethylammonium tetrafluoroborate is preferably 0.1 to 0.3 mol / L; the reaction temperature of formula (B) and formula (E) is 70 to 80°C; the reaction time is 4 to 6 h; the pH value is 5.0 to 5.6; the volume ratio of acetonitrile to tetraethylammonium tetrafluoroborate is (10 to 20):1.
[0014] In one or more embodiments, step S2 further comprises a low-temperature water washing step, the water washing temperature is 5 to 10° C., and the number of water washing times is 2 to 4 times.
[0015] In one or more embodiments, in step S3, the nano copper oxide is preferably one of rod-shaped nano copper oxide, needle-shaped nano copper oxide and flake-shaped nano copper oxide; the size of the nano copper oxide is preferably one or more of 20 nm, 50 nm and 100 nm.
[0016] In one or more embodiments, in step S3, the ultrasonic frequency in the ultrasonic dispersion is 20 to 30 KHz, the ultrasonic power is 12 to 39 W, and the ultrasonic time is 10 to 20 min.
[0017] In one or more embodiments, the pretreatment process in step S3 includes: exposing the nano-copper oxide to 254nm ultraviolet light, and then placing the nano-copper oxide after ultraviolet light exposure in a glass dryer containing a beaker containing a saturated potassium nitrate solution for surface treatment; the ultraviolet light exposure time is 2 to 5 hours; the surface treatment time is 3 to 6 hours.
[0018] On one hand, the present invention provides the application of a strong and non-toxic antibacterial and antiviral nano-functional material in textiles, which is used for preparing strong and non-toxic antibacterial and antiviral textiles.
[0019] This patent proposes to use strong and non-toxic antibacterial and antiviral nano-functional materials to improve the antibacterial and antiviral properties of textiles and better protect people's health. This patent prepares a strong and non-toxic antibacterial and antiviral nano-functional material by compounding nano-copper oxide with meta-dichlorostyrene meta-dichlorophenyl ketone. Both have excellent antibacterial effects and after nano-copper oxide is grafted with meta-dichlorostyrene meta-dichlorophenyl ketone, the textiles treated with strong and non-toxic antibacterial and antiviral nano-functional materials will be more resistant to washing and have better antibacterial and antiviral effects. And the raw material meta-dichlorostyrene meta-dichlorophenyl ketone used is one of the natural antibacterial agents, which can ensure that the product is non-toxic and harmless to the human body, green and healthy.
[0020] The present invention has the following advantages over the prior art:
[0021] The composite product of nano copper oxide and meta-dichlorostyrene and meta-dichlorophenyl ketone in the present invention has better antibacterial effect.
[0022] The raw materials in the present invention are green and environmentally friendly. Meta-dichlorostyrene meta-dichlorophenyl ketone is a natural plant-derived antibacterial agent, which is non-toxic and harmless to the human body, and is green and healthy compared to chemical antibacterial agents.
[0023] The invention connects the composite product of nano copper oxide and meta-dichlorostyrene and meta-dichlorophenyl ketone to various places of the textile, so that the textile can still maintain good antibacterial and antiviral effects after repeated use and washing. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The chemical reaction formula of the nano-functional material of the embodiment of the present invention;
[0025] Figure 2 This is a process flow chart of the nano functional material according to an embodiment of the present invention;
[0026] Figure 3 The antibacterial and antiviral performance of the experimental cloth pieces with different doping amounts of the nano-functional material of the embodiment of the present invention before washing is compared;
[0027] Figure 4 The antibacterial and antiviral performance of the experimental cloth pieces with different doping amounts after being washed 50 times with the nano-functional material of the embodiment of the present invention is compared;
[0028] Figure 5 This is a comparison chart of the antibacterial and antiviral properties of nanomaterials using different pretreatment methods of the present invention. DETAILED DESCRIPTION
[0029] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.
[0030] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All raw materials, reagents, etc., whose manufacturers are not specified, are conventional products that can be purchased commercially.
[0031] The compound of formula A, 5-vinyl-3-hexanone trimethoxysilane, is synthesized according to the following steps: 1. Add hydrogen peroxide solution and hydrogen bromide solution to vinyl trimethoxysilane, and stir to react to obtain 1-bromoethyl trimethoxysilane. 2. Heat reflux 3-butenoic acid and excess thionyl chloride in an organic solvent, and evaporate excess thionyl chloride and organic solvent after the reaction to obtain 3-butenoyl chloride. 3. Add 1-bromoethyl trimethoxysilane and 3-butenoyl chloride to anhydrous ether, and react after nitrogen is introduced to obtain formula A.
[0032] References:
[0033] [1] Zhang Heng, Xing Zhirong, Liu Dong, Zhou Zhibin, Feng Wenfang. Improvement of the synthetic experiment of Grignard reagent[J]. University Chemistry, 2023, 38(2): 177-184
[0034] [2] Xin Jianfeng, Ma Jihai, Zhang Shufen, Chen Shaorui, Li Haiyu. Review of preparation methods of acyl chlorides[J]. Hebei Chemical Industry, 2006, 29(11): 16-1820
[0035] [3]Fiandanese V, Marchese G, Martina V, et al.Iron catalyzed cross-coupling reactions of acyl chlorides with Grignard reagents.A mild, general, and convenient synthesis of aliphatic and aromatic ketones[J].Tetrahedronletters,1984,25(42):4805-4808.
[0036] The compound of formula D, 2,6-dichlorostyryl 2,6-dichlorophenyl ketone, was prepared by referring to the following literature: A. KAISER, P. BIELMEIER, W. WIEGREBE, 1,3-Diphenylpropane-1,3-diamines. Part 11. Conversion of a 3-Hydroxy-1,3-diphenylpropan-1-one to
[0037] 1,3-Diphenylpropane-1,3-diamines.,Monatsh.Chem.,1997,128,1247-1254.
[0038] Embodiment 1
[0039] Step 1
[0040]
[0041] According to the molar ratio of ferrous chloride, alkaline organic solvent and pinacol diboron ester of 1:15:20, 10 mL of 5 mmol / L ferrous chloride solution, 0.061 g of lithium tert-butyl alcohol and 0.25 g of pinacol diboron ester were weighed and put into a Schlenk reaction tube. Under the condition of ensuring airtightness, argon gas was pumped and filled twice, and 50 mL of methyl tert-butyl ether and 1.9 g of formula (A) were added. After heating to 30°C and stirring for 10 hours, the organic phase was extracted with ethyl acetate, and 25 mL of 2 mol / L sodium hydroxide solution and 25 mL of 30% hydrogen peroxide solution were added to the organic phase and stirred. After extraction, the organic phase was washed with saturated brine, dried with anhydrous magnesium sulfate, dried by spin drying, purified by column, and 2.05 g of formula (B) was obtained after spin evaporation.
[0042] Step 2
[0043]
[0044] Take 2.54g of formula (D), 25mL of acetonitrile and 2.5mL of 0.1mol / L tetraethylammonium tetrafluoroborate solution and place them in an electrolytic cell. After passing CO2 at normal pressure for 0.5h, perform constant voltage electrolysis at an electrolysis potential of -1.75V. After the reaction, the obtained mixture is extracted with acetone, the aqueous phase is acidified to pH 5.0 by adding 4mol / L hydrochloric acid, the aqueous layer is extracted again with an organic solvent, the organic phase is dried with anhydrous magnesium sulfate, and 2.86g of formula (E) is obtained after rotary evaporation. Formula (E) and formula (B) are placed in a reaction kettle, distilled water is added, stirred evenly, formic acid is added, heated to 70℃ for reaction for 4h, and cooled for 3h after the reaction is completed to obtain a reaction solution. The obtained reaction solution is extracted with an organic solvent, the organic phase is washed twice with 5℃ distilled water at low temperature, separated, dehydrated, filtered, distilled and purified, and formula (C) is obtained after rotary evaporation.
[0045] Step 3
[0046]
[0047] Take 2.5g of 20nm nano copper oxide and expose it to 254nm ultraviolet light for 2h, and then put the nano copper oxide exposed to ultraviolet light into a glass dryer containing a beaker of saturated potassium nitrate solution for surface treatment for 3h. In the acetone solution, add the pretreated nano copper oxide and formula (C) in sequence, adjust the ultrasonic frequency to 20KHz, adjust the ultrasonic power to 12W for ultrasonic dispersion for 10min, and then put the solid into a vacuum drying oven at 80℃ for 24h to obtain a strong non-toxic antibacterial and antiviral nano functional material of formula (I) for modifying textiles.
[0048] Embodiment 2
[0049] Step 1
[0050] According to the molar ratio of ferrous chloride, alkaline organic solvent and pinacol diboron ester of 1:16:23, 10 mL of 5 mmol / L ferrous chloride solution, 0.064 g of lithium tert-butyl alcohol and 0.292 g of pinacol diboron ester were weighed and put into a Schlenk reaction tube. Under the condition of ensuring airtightness, argon gas was pumped and filled for 3 times, and 50 mL of methyl tert-butyl ether and 4 g of formula (A) were added. After heating to 40°C and stirring for 12 hours, the organic phase was extracted with ethyl acetate, and 25 mL of 2 mol / L sodium hydroxide solution and 25 mL of 30% hydrogen peroxide solution were added to the organic phase and stirred. After extraction, the organic phase was washed with saturated brine, dried with anhydrous magnesium sulfate, dried by spin drying, purified by column, and 4.2 g of formula (B) was obtained after spin evaporation.
[0051] Step 2
[0052] Take 4.08g of formula (D), 25mL of acetonitrile and 1.67mL of 0.2mol / L tetraethylammonium tetrafluoroborate solution and place them in an electrolytic cell. After passing CO2 at normal pressure for 0.7h, perform constant voltage electrolysis at an electrolysis potential of -1.75V. After the reaction, the resulting mixture is extracted with acetone, the aqueous phase is acidified to pH 5.3 by adding 4mol / L hydrochloric acid, the aqueous layer is extracted again with an organic solvent, the organic phase is dried with anhydrous magnesium sulfate, and 5.65g of formula (E) is obtained after rotary evaporation. Formula (E) and formula (B) are placed in a reaction kettle, distilled water is added, stirred evenly, formic acid is added, heated to 75℃ for reaction for 5h, and cooled for 3h after the reaction is completed to obtain a reaction solution. The obtained reaction solution is extracted with an organic solvent, the organic phase is washed with 7℃ distilled water for 3 times, separated, dehydrated, filtered, distilled and purified, and formula (C) is obtained after rotary evaporation.
[0053] Step 3
[0054] Take 6g of 50nm nano copper oxide and expose it to 254nm ultraviolet light for 3h, and put the nano copper oxide exposed to ultraviolet light into a glass dryer with a beaker containing a saturated potassium nitrate solution for surface treatment for 4h. In the ether solution, add the pretreated nano copper oxide and formula (C) in turn, adjust the ultrasonic frequency to 30KHz, adjust the ultrasonic power to 39W for ultrasonic dispersion for 15min, and put the solid into a vacuum drying oven at 80℃ for 24h after filtration to obtain a strong non-toxic antibacterial and antiviral nano functional material of formula (I) for modifying textiles.
[0055] Embodiment 3
[0056] Step 1
[0057] According to the molar ratio of ferrous chloride, alkaline organic solvent and pinacol diboron ester of 1:18:25, 10 mL of 5 mmol / L ferrous chloride solution, 0.072 g of lithium tert-butyl alcohol and 0.317 g of pinacol diboron ester were weighed and put into a Schlenk reaction tube. Under the condition of ensuring airtightness, argon gas was pumped and filled for 5 times, and 50 ml of methyl tert-butyl ether and 2.85 g of formula (A) were added. After heating to 45°C and stirring for 18 hours, the organic phase was extracted with ethyl acetate, and 25 ml of 2 mol / L sodium hydroxide solution and 25 ml of 30% hydrogen peroxide solution were added to the organic phase and stirred. After extraction, the organic phase was washed with saturated brine, dried with anhydrous magnesium sulfate, dried by spin drying, purified by column, and 3.1 g of formula (B) was obtained after spin evaporation.
[0058] Step 2
[0059] Take 3.79g of formula (D), 25mL of acetonitrile and 1.25mL of 0.3mol / L tetraethylammonium tetrafluoroborate solution and place them in an electrolytic cell. After passing CO2 at normal pressure for 1h, perform constant voltage electrolysis at a potential of -1.75V. After the reaction, the resulting mixture is extracted with acetone, the aqueous phase is acidified to pH 5.6 by adding 4mol / L hydrochloric acid, the aqueous layer is extracted again with an organic solvent, the organic phase is dried with anhydrous magnesium sulfate, and 4.25g of formula (E) is obtained after rotary evaporation. Formula (E) and formula (B) are placed in a reactor, distilled water is added, stirred evenly, formic acid is added, heated to 80℃ for reaction for 6h, and cooled for 3h after the reaction is completed to obtain a reaction solution. The obtained reaction solution is extracted with an organic solvent, the organic phase is washed with 10℃ distilled water for 3 times, separated, dehydrated, filtered, distilled and purified, and formula (C) is obtained after rotary evaporation.
[0060] Step 3
[0061] Take 5g of 100nm nano copper oxide and expose it to 254nm ultraviolet light for 5h, and put the nano copper oxide exposed to ultraviolet light into a glass dryer with a beaker containing a saturated potassium nitrate solution for surface treatment for 6h. In the ethanol solution, add the pretreated nano copper oxide and formula (C) in sequence, adjust the ultrasonic frequency to 25KHz, adjust the ultrasonic power to 30W for ultrasonic dispersion for 20min, and put the solid into a vacuum drying oven at 80℃ for 24h after filtration to obtain a strong non-toxic antibacterial and antiviral nano functional material of formula (I) for modifying textiles.
[0062] In order to evaluate the antibacterial and antiviral performance of the present invention, we used the cloth piece of the present invention to evaluate its antibacterial and antiviral performance according to national standards. The experimental results are listed in Table 1 and Figure 3 shown.
[0063] (1) The evaluation of antibacterial performance refers to the national standard: "Oscillating method for evaluation of antibacterial properties of textiles GB / T20944.3-2008".
[0064] Take 3 samples from the antibacterial fabric sample (each with a size of 10cm×10cm, cut into 2 pieces), wash according to the test condition A1M in GB / T 12490, and use ECE phosphorus-free standard detergent. Use water temperature 40℃±3℃, detergent concentration 0.2%, 150mL solution, 10 steel balls, and wash for 45min. After washing, take out the sample and wash it twice in 40℃±3℃ and 100mL water, 1min each time. Repeat this procedure until the specified number of washes. To prevent residual detergent from interfering with the antibacterial performance test, wash the sample thoroughly at the end of the last procedure, and then dry it or bake it.
[0065] Take 40 mL of E. coli solution prepared with PBS buffer, add the antibacterial and antiviral textile fabrics washed for different times and a blank sample, and culture at 37°C with shaking at 150 r / min for 18 hours. Use the nutrient agar plate method, count after culturing at 37°C for 24 hours, measure the concentration of E. coli and calculate the removal rate.
[0066] (2) Antiviral evaluation refers to the international standard: "Textiles - Determination of antiviral activity of textiles ISO 18184".
[0067] Take 40 mL of MS2 bacteriophage solution prepared with PBS buffer, add the above antibacterial and antiviral textile fabrics washed for different times and a blank sample, and culture at 37°C with shaking at 150 / min for 12 hours. Use the double-layer plate method, culture in a 37°C incubator for 6-8 hours, count, measure the MS2 bacteriophage concentration and calculate the removal rate.
[0068] We washed the experimental cloth pieces with different doping amounts fifty times and then tested their antibacterial and antiviral performance. Then we compared them with the cloth pieces before washing. The results in Table 2 and Figure 4 It can be seen that the antibacterial and antiviral effects of the modified cloth piece of the present invention are still very strong after being washed fifty times.
[0069] Table 1 shows the antibacterial and antiviral effects of each cloth piece before washing
[0070]
[0071] Table 2 Antibacterial and antiviral effects of each cloth piece after washing 50 times
[0072]
[0073] In order to determine the toxicity of the product, we evaluated the cytotoxicity with reference to ISO 10993, and the method is as follows: 50 μL of human epidermal cell suspension was taken from the stirred human epidermal cell suspension, inoculated on the culture medium for 24 hours and counted. 50 μL of human epidermal cell suspension of the same concentration was taken from the stirred human epidermal cell suspension and the nanomaterials obtained in the experiment were added. Three parallel samples were made for each portion, inoculated on the culture medium for 24 hours and counted. The number of surviving cells on the culture medium without the nanomaterials obtained in the experiment was compared with the number of surviving cells on the culture medium with the nanomaterials obtained in the experiment, and the survival rate was calculated.
[0074] Table 3 Cytotoxicity test
[0075]
[0076] As shown in Table 3, the antibacterial and antiviral nanomaterials obtained in the experiment have almost no effect on the growth and reproduction of human epidermal cells. According to the ISO 10993 standard, antibacterial and antiviral nanomaterials can be classified as non-cytotoxic. It can be seen that the antibacterial and antiviral nanomaterials synthesized in the experiment of the present invention are truly non-toxic, harmless, green and healthy.
[0077] In order to further verify that the antibacterial and antiviral nanomaterials synthesized in the present invention are non-toxic, harmless, green and healthy nanomaterials, the present invention conducted a sweat leaching experiment to determine the heavy metal dissolution content and TOC content in the leached sweat. The heavy metal dissolution determination refers to the national standard: "Determination of Heavy Metals in Textiles by Atomic Absorption Spectrophotometry GB / T17593.1-2006". The TOC determination method adopts the combustion oxidation-non-dispersive infrared absorption method.
[0078] Take a 5mm×5mm textile sample modified with the antibacterial and antiviral nanomaterial of the present invention, mix well, weigh two 4g samples (for parallel test), accurate to 0.01g, and place them in a stoppered conical flask. Add 80mL of the prepared simulated acid sweat to fully soak the fiber, put it in a constant temperature water bath oscillator for 60min, take it out, let it stand and cool to room temperature, and filter it as a sample liquid for analysis.
[0079] Dilute the prepared copper standard working solution with water step by step to a series of working solutions of appropriate concentrations. At a wavelength of 324.7nm (Cu), use a graphite furnace atomic absorption spectrophotometer to measure the absorbance of copper in the series of working solutions in order from low to high concentrations, and draw a working curve with absorbance as the ordinate and concentration (μg / mL) as the abscissa. Determine the absorbance of each element to be measured in the blank solution and the sample solution, and calculate the concentration of each element to be measured from the working curve.
[0080] Table 4 Metal copper leaching analysis
[0081] sample Copper precipitation content (mg / kg) Containing 5wt% of the product of Example 1 1.71 Containing 5wt% of the product of Example 2 1.65 Containing 5wt% of the product of Example 3 1.54 Containing 7.5wt% of the product of Example 1 1.70 Containing 7.5wt% of the product of Example 2 1.66 Containing 7.5wt% of the product of Example 3 1.60 Containing 10wt% of the product of Example 1 1.81 Containing 10wt% of the product of Example 2 1.70 A cloth sheet containing 10 wt% of the product of Example 3 1.59
[0082] As can be seen from Table 4, the heavy metal leaching content of the cloth after being subjected to simulated sweat is far lower than the national standard, which proves that the textile modified by the present invention is green, healthy, non-toxic and harmless.
[0083] Prepare two identical sample solutions in the same manner as above. Inject the two sample solutions into the high-temperature combustion tube and the low-temperature reaction tube respectively to obtain the total carbon and inorganic carbon contents of the sample solutions, and subtract the two to obtain the organic carbon content.
[0084] Table 5 Organic carbon leaching analysis
[0085] sample Organic carbon content (μg / L) Containing 5wt% of the product of Example 1 45.12 Containing 5wt% of the product of Example 2 45.36 Containing 5wt% of the product of Example 3 46.67 Containing 7.5wt% of the product of Example 1 42.56 Containing 7.5wt% of the product of Example 2 43.99 Containing 7.5wt% of the product of Example 3 44.45 Containing 10wt% of the product of Example 1 46.67 Containing 10wt% of the product of Example 2 47.34 A cloth sheet containing 10 wt% of the product of Example 3 47.56
[0086] As can be seen from Table 5, the organic carbon leaching content of the cloth piece leached with simulated sweat is extremely low, which proves that the present invention is extremely stable and will not precipitate due to sweat to cause harm to the human body, once again proving that the present invention is green, healthy, non-toxic and harmless.
[0087] In order to verify that the pretreatment step of the nano copper oxide of the present invention can improve the antibacterial and antiviral effect of the final synthetic material, the present invention compares the antibacterial and antiviral properties of the final product synthesized by the nano copper oxide after different pretreatment steps. The experimental method is as follows: three identical nano copper oxides are subjected to four different pretreatments: 254nm ultraviolet light irradiation for 2h, placed in a glass dryer containing a beaker containing a saturated potassium nitrate solution for surface treatment, and placed in a glass dryer containing a beaker containing a saturated potassium nitrate solution after 254nm ultraviolet light for surface treatment. Three nano copper oxides after different pretreatments and nano copper oxides without pretreatment are synthesized into four antibacterial and antiviral nanomaterials, and then the four antibacterial and antiviral nanomaterials are tested for antibacterial and antiviral properties to compare their antibacterial and antiviral properties.
[0088] Figure 5 Middle: Experimental group: nanomaterials synthesized by nano-copper oxide after ultraviolet light irradiation + surface treatment with saturated potassium nitrate solution; surface treatment group: nanomaterials synthesized by nano-copper oxide without ultraviolet light irradiation + surface treatment with saturated potassium nitrate solution; UV irradiation group: nanomaterials synthesized by nano-copper oxide after ultraviolet light irradiation + surface treatment with saturated potassium nitrate solution; untreated group: nanomaterials synthesized by nano-copper oxide without ultraviolet light irradiation + surface treatment with saturated potassium nitrate solution; Log removal rate: Log removal rate of bacteria or viruses.
[0089] Table 6 Comparison of antibacterial and antiviral properties of nanomaterials by different pretreatment methods
[0090]
[0091]
[0092] From Table 6 and Figure 5It can be seen that the nano copper oxide treated by ultraviolet light + not treated by saturated potassium nitrate solution has an increased surface activity, resulting in a nano material generated by the reaction of the nano copper oxide treated by ultraviolet light + not treated by saturated potassium nitrate solution, which is about 60% higher than the nano material generated by the reaction of the nano copper oxide not treated by ultraviolet light + not treated by saturated potassium nitrate solution. The nano copper oxide that has not been treated by ultraviolet light + saturated potassium nitrate solution has more water molecules on the surface of the nano copper oxide, which increases the surface reaction sites of the nano copper oxide, resulting in a nano material generated by the reaction of the nano copper oxide that has not been treated by ultraviolet light + saturated potassium nitrate solution, which is about 65% higher than the nano material generated by the reaction of the nano copper oxide that has not been treated by ultraviolet light + not treated by saturated potassium nitrate solution. The nano-copper oxide treated with ultraviolet light + surface treated with saturated potassium nitrate solution not only increases the surface activity of the nano-copper oxide, but also increases the reaction sites on the surface of the nano-copper oxide, resulting in a performance improvement of about 100% in the nano-material generated by the nano-copper oxide treated with ultraviolet light + surface treated with saturated potassium nitrate solution compared to the nano-copper oxide not treated with ultraviolet light + surface treated with saturated potassium nitrate solution.
Claims
1. A powerful, non-toxic, antibacterial and antiviral nano-functional material represented by formula (I) 2. The method for preparing the potent, non-toxic, antibacterial and antiviral nano-functional material according to claim 1, characterized in that: The following steps are involved: S1: Formula (A) The product is subjected to hydroboration and oxidation reaction with pinacol diboron ester, ferrous chloride and alkaline organic solution, extracted, washed with saturated brine, dried, spin-dried, purified by column, and then evaporated to obtain the product of formula (B) S2: Take formula (D) Put it into a reaction kettle, add acetonitrile and tetraethylammonium tetrafluoroborate, carry out electrocarboxylation reaction under constant voltage and CO2 conditions, extract, adjust pH value, and obtain formula (E) The formula (B) and the formula (E) described in step S1 are mixed, distilled water is added, and the formula (C) is obtained under the action of a catalyst. S3: dissolving the compound (C) obtained in step S2 in an organic solvent, adding the pretreated nano copper oxide, ultrasonically dispersing and continuously stirring, and rotary evaporating to obtain the potent, non-toxic, antibacterial and antiviral nano functional material of formula (I).
3. The preparation method according to claim 2, characterized in that: The alkaline organic solution in step S1 is one or more of triethylamine, triethylenediamine, lithium tert-butoxide, potassium tert-butoxide, and sodium tert-butoxide.
4. The preparation method according to claim 2, characterized in that: In step S1, the molar ratio of ferrous chloride, alkaline organic solution and pinacol diboron ester is 1:(15-18):(20-25); the reaction temperature of step S1 is 30-45°C; and the reaction time is 10-18h.
5. The preparation method according to claim 2, characterized in that: Step S1 also includes a step of pumping and filling argon gas; the number of times of pumping and filling argon gas is 2 to 5 times.
6. The preparation method according to claim 2, characterized in that: In step S2, the CO2 passing time is 0.5 to 1 h; the concentration of tetraethylammonium tetrafluoroborate is 0.1 to 0.3 mol / L; the reaction temperature of formula (B) and formula (E) is 70 to 80°C, and the reaction time is 4 to 6 h; the pH value is 5.0 to 5.6; the volume ratio of acetonitrile to tetraethylammonium tetrafluoroborate is (10 to 20):
1.
7. The preparation method according to claim 2, characterized in that: Step S2 also includes a low-temperature water washing step, the water washing temperature is 5 to 10° C., and the number of water washing times is 2 to 4 times.
8. The preparation method according to claim 2, characterized in that: In step S3, the ultrasonic frequency in the ultrasonic dispersion is 20 to 30 KHz, the ultrasonic power is 12 to 39 W, and the ultrasonic time is 10 to 20 min.
9. The preparation method according to claim 2, characterized in that: The pretreatment process in step S3 includes: exposing the nano copper oxide to 254nm ultraviolet light, and then placing the nano copper oxide after ultraviolet light exposure in a glass dryer containing a beaker containing a saturated potassium nitrate solution for surface treatment; the ultraviolet light exposure time is 2 to 5 hours; and the surface treatment time is 3 to 6 hours.
10. The use of a strong, non-toxic, antibacterial and antiviral nano-functional material in textiles according to claim 1, characterized in that: Used to prepare strong, non-toxic antibacterial and antiviral textiles.
Citation Information
Patent Citations
One-room type electrochemical synthesis method for alpha-phenyl-beta-benzoylpropionic acid
CN101260531A