Antibacterial ion exchange resin as well as preparation method and application thereof
By acidizing and aminating the ion exchange resin, an antibacterial ion exchange resin was prepared, which solved the problem of difficult balance between antibacterial effect and immersion requirements of existing resin materials, and achieved stable antibacterial effect and low cost. Solution.
Patent Information
- Application Number
- CN202310600387.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
It is difficult to achieve a balance between antibacterial effect and soaking requirements during use of existing ion exchange resin materials, resulting in the possibility of excessive colonies in drinking water.
By acidizing and aminating the ion exchange resin, antibacterial ions are uniformly introduced to make them evenly distributed on the surface, and an antibacterial ion exchange resin is prepared to ensure that it is not easy to lose during use and soaking, and a stable antibacterial effect is achieved.
The balance between antibacterial effect and soaking requirements is achieved, avoiding the excessive colony standard during use and soaking, and the preparation method is simple, the cost is low, and the service life is extended.
Smart Images

Figure BDA0004248720740000061 
Figure BDA0004248720740000071
Abstract
Description
Technical Field
[0001] The invention specifically relates to an antibacterial ion exchange resin and a preparation method and application thereof. Background Art
[0002] Ion exchange resins are widely used in household water filter jugs and the end filter of household water purifiers to remove water hardness and reduce the possibility of scaling. However, during the use of ion exchange resins, since the material itself does not have antibacterial properties, bacteria may grow, causing the total colony count and bacterial metabolites (such as nitrite) in drinking water to exceed the standard.
[0003] In the field of water purification, the commonly used inorganic antimicrobial agents are mainly zinc and silver. However, due to the limitation of sanitary standards for domestic water supply and distribution (refer to the requirements of Appendix B of Document No. 161 issued by the Ministry of Health, ... Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the defect that the existing resin materials are difficult to achieve a balance between the antibacterial effect and the soaking requirement, and to provide an antibacterial ion exchange resin and a preparation method and application thereof.
[0005] The present invention introduces amine groups uniformly to the surface of the acidified ion exchange resin under soaking conditions, so that the antibacterial ions are evenly distributed on the surface of the ion exchange resin and are not easily lost during use. The prepared antibacterial ion exchange resin has a stable and reliable antibacterial effect. During use and soaking, no ions are precipitated, and the excessive bacterial colony during use and soaking can be effectively avoided, achieving a balance between the antibacterial effect and the soaking requirements. The preparation method of the antibacterial ion exchange resin of the present invention is simple in process and low in cost.
[0006] The present invention solves the above technical problems through the following technical solutions.
[0007] The present invention provides a method for preparing an antibacterial ion exchange resin, which comprises the following steps:
[0008] ① Acidifying the ion exchange resin to obtain ion exchange resin A;
[0009] ② subjecting the ion exchange resin A to an amination treatment to obtain an ion exchange resin B;
[0010] ③ The ion exchange resin B is connected with antibacterial ions to obtain the antibacterial ion exchange resin.
[0011] In step ①, the volume exchange capacity of the ion exchange resin may be greater than 1.4 mmol / mL, preferably 2-10 mmol / mL, such as 3 mmol / mL, 4 mmol / mL, 4.3 mmol / mL, 5 mmol / mL, 6 mmol / mL, 7 mmol / mL, 8 mmol / mL or 9 mmol / mL.
[0012] In step ①, the density of the ion exchange resin may be 0.7-1.2 g / mL, preferably 0.7-1.19 g / mL, such as 0.72 g / mL, 0.75 g / mL, 0.8 g / mL, 0.9 g / mL, 1.1 g / mL, 1.15 g / mL or 1.18 g / mL.
[0013] In step ①, the particle size of the ion exchange resin may be 0.3-1.2 mm, preferably 0.3-1.0 mm, such as 0.5 mm, 0.7 mm or 0.9 mm.
[0014] In step ①, the water content of the ion exchange resin is generally 40%-60%, for example 50%.
[0015] In step ①, the ion exchange resin is preferably a weakly acidic ion exchange resin of model Lewatit S-8227 (particle size 0.7 mm, volume exchange capacity 4.3 mmol / mL, water content 50%, density 1.18 g / mL) purchased from Lanxess Chemical.
[0016] In step ①, the ion exchange resin A is preferably a weakly acidic ion exchange resin.
[0017] In step ①, during the acidification process, the main reaction that occurs is R-COONa+H + =R-COOH+Na + "R-COONa" represents the unacidified ion exchange resin, and "R-COOH" represents the acidified ion exchange resin, that is, the hydrogen-type ion exchange resin.
[0018] In step ①, the acidification treatment generally includes the following steps: placing the ion exchange resin in an acid solution for soaking once to obtain ion exchange resin A.
[0019] The acid in the acid solution may be a conventional acid in the art, such as one or more of hydrochloric acid, sulfuric acid and nitric acid, preferably hydrochloric acid, sulfuric acid or nitric acid.
[0020] The pH of the acid solution may be conventional in the art, such as 3-6, preferably 4 or 5.
[0021] Wherein, the solvent of the acid solution is generally water.
[0022] The soaking time may be conventional in the art, generally sufficient to allow the ion exchange resin to be completely converted into ion exchange resin A. Generally, the acid-base titration method may be used to determine whether the ion exchange resin is completely converted into ion exchange resin A.
[0023] After the soaking step, a washing step is generally included. The washing step can be conventional in the art, for example, the ion exchange resin A is washed with distilled water. The washing time can be conventional in the art, for example, 30 minutes.
[0024] In step ②, the amination treatment generally includes the following steps: reacting the ion exchange resin A with an amine compound in the presence of a solvent to obtain the ion exchange resin B.
[0025] Among them, the mass ratio of the ion exchange resin A to the amine compound can be 100:(0.8-10), for example, 100:1, 100:1.5, 100:2, 100:2.5, 100:3, 100:3.5, 100:4, 100:5, 100:6, 100:7, 100:8 or 100:9.
[0026] In the amination process, the mass concentration of the amine compound can be a conventional mass concentration in the art, such as 0.8-10wt%, such as 2wt%, 4wt%, 6wt% or 8wt%.
[0027] Among them, the amine compound can be a conventional amine compound in the art, such as one or more of diethylenetriamine, pentaethylenehexamine, tetraethylenepentamine, triethylenetetramine, tetraethylenepentamine, triethylenetetramine, ethylenediamine, polyvinylpyrrolidone, chitosan, N-carboxymethylchitosan, polyvinylimidazole, polyethyleneimine, polyallylamine, piperazine, p-aminobenzene and m-aminobenzene, preferably polyethyleneimine, triethylenetetramine or tetraethylenepentamine.
[0028] In the amination process, the solvent may be a conventional solvent in the art, such as one or more of water, acetone, methanol and ethanol, preferably a mixture of at least one of acetone, methanol and ethanol and water.
[0029] The reaction temperature may be a conventional temperature in the art, generally 30-60° C., such as 45° C. The reaction temperature is generally reached by heating in a water bath.
[0030] The reaction time may be conventional in the art, generally 10-30 h, such as 20 h.
[0031] Wherein, the reaction generally includes washing and drying steps, which can be conventional in the art.
[0032] In step ③, the introduction of antibacterial ions generally includes the following steps: placing ion exchange resin B in an antibacterial ion solution for secondary immersion to obtain the antibacterial ion exchange resin.
[0033] Among them, the mass ratio of the ion exchange resin B to the antibacterial ions can be 100:(0.5-5), for example, 100:1, 100:1.5, 100:2, 100:2.5, 100:3, 100:3.5, 100:4, 100:4.5 or 100:4.8, preferably 100:(0.5-2).
[0034] The mass concentration of the antibacterial ion solution may be conventional in the art, preferably 0.5-5%, such as 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%.
[0035] The antibacterial ion solution may be a conventional salt solution containing antibacterial ions in the art. The salt containing antibacterial ions may be conventional in the art, such as one or more of zinc sulfate, zinc nitrate, zinc chloride and silver nitrate, preferably zinc sulfate, zinc nitrate, zinc chloride or silver nitrate.
[0036] The solvent of the antibacterial ion solution may be a conventional solvent in the art, generally water.
[0037] The temperature of the secondary immersion may be a conventional temperature in the art, generally 20-45°C, such as 30°C or 40°C, preferably 20-30°C, such as 25°C.
[0038] The secondary immersion time may be a conventional time in the art, generally 10-80 min, preferably 15-80 min, for example 20 min, 30 min, 40 min, 50 min, 60 min or 70 min.
[0039] In the present invention, in the preparation method, the antibacterial ion exchange resin is generally washed and dried. The washing and drying methods and conditions can be conventional in the art.
[0040] In some embodiments of the present invention, the cleaning and drying comprises the following steps: soaking the antibacterial ion exchange resin in pure water for 30 minutes, repeating this process three times, and drying to obtain the antibacterial ion exchange resin.
[0041] The present invention also provides an antibacterial ion exchange resin, which is prepared by the above-mentioned preparation method of the antibacterial ion exchange resin.
[0042] In the present invention, the volume exchange capacity of the antibacterial ion exchange resin may be greater than 1.4 mmol / mL, preferably 2-10 mmol / mL, such as 3 mmol / mL, 4 mmol / mL, 4.3 mmol / mL, 5 mmol / mL, 6 mmol / mL, 7 mmol / mL, 8 mmol / mL or 9 mmol / mL.
[0043] In the present invention, the density of the antibacterial ion exchange resin may be 0.7-1.2 g / mL, preferably 0.7-1.19 g / mL, such as 0.72 g / mL, 0.75 g / mL, 0.8 g / mL, 0.9 g / mL, 1.1 g / mL, 1.15 g / mL or 1.18 g / mL.
[0044] In the present invention, the particle size of the antibacterial ion exchange resin may be 0.3-1.2 mm, preferably 0.3-1.0 mm, such as 0.5 mm, 0.7 mm or 0.9 mm.
[0045] In the present invention, the water content of the antibacterial ion exchange resin is generally 40%-60%, for example 50%.
[0046] The present invention also provides an application of the above-mentioned antibacterial ion exchange resin as a filter material in the fields of food, chemical industry or medicine.
[0047] In the present invention, the application is preferably an application in the field of chemical water purification.
[0048] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0049] The reagents and raw materials used in the present invention are commercially available.
[0050] The positive and progressive effects of the present invention are:
[0051] 1. The antibacterial ion exchange resin of the present invention has a stable and reliable antibacterial effect and a long service life. During use and soaking, no ions will be precipitated, which can effectively avoid excessive colonies during use and soaking, and can achieve a balance between the antibacterial effect and the soaking requirements.
[0052] 2. The volume exchange capacity of the antibacterial ion exchange resin of the present invention is the same as the particle size, volume exchange capacity, water content and density of the ion exchange resin initially used, especially the volume exchange capacity will not decrease, while the volume exchange capacity of the antibacterial ion exchange resin rubber prepared by the prior art and the raw material (ion exchange resin) used will decrease by less than 5%.
[0053] 3. The preparation method of the ion exchange resin of the present invention has simple process and low cost. DETAILED DESCRIPTION
[0054] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0055] Example 1
[0056] The preparation method of antibacterial ion exchange resin comprises the following steps:
[0057] (1) Raw material modification: Weakly acidic ion exchange resin (manufacturer: LANXESS Chemical (China) Co., Ltd., model: Lewatit S-8227, particle size 0.7 mm, volume exchange capacity 4.3 mmol / mL, water content 50%, density 1.18 g / mL) was immersed in an acidic aqueous solution (solute is hydrochloric acid) at pH = 4 to convert the weakly acidic ion exchange resin into a hydrogen-type ion exchange resin (i.e., ion exchange resin A), and then washed with distilled water for 30 min. The degree of conversion of the weakly acidic ion exchange resin into the hydrogen-type ion exchange resin can be determined by acid-base titration. Generally, the subsequent steps are carried out after the resin is completely converted into the hydrogen-type ion exchange resin.
[0058] R-COONa+H + =R-COOH+Na +
[0059] (2) Surface amination:
[0060] Ion exchange resin A was placed in a 6wt% amine modification solution (solute is polyethyleneimine, solvent is water), heated in a 45°C water bath for 20h to initiate modification of the ion exchange resin, and then washed and dried to obtain a modified ion exchange resin (i.e., ion exchange resin B). The mass ratio of ion exchange resin A to amine compound is 100:6.
[0061] (3) Access to antibacterial ions: Ion exchange resin B was placed in a 1.5% zinc ion solution (solute: zinc nitrate, solvent: water) and soaked for 20 minutes at an ambient temperature of 20°C. In the system accessed with antibacterial ions, the mass ratio of ion exchange resin B to zinc ions was 100:1.5.
[0062] (4) Cleaning and drying: Soak the ion exchange resin infused with antibacterial ions in pure water for 30 min, repeat three times, and dry to obtain an antibacterial ion exchange resin (particle size 0.7 mm, volume exchange capacity 4.3 mmol / mL, water content 50%, density 1.18 g / mL).
[0063] Except for the conditions shown in Table 1, other conditions in Examples 2-8 and Comparative Examples 1-3 are the same as those in Example 1.
[0064] The particle size, volume exchange capacity, water content and density of the antibacterial ion exchange resins prepared in Examples 2-8 are the same as those in Example 1.
[0065] Table 1
[0066]
[0067]
[0068] Note: “ / ” in the above table means that the substance was not used for treatment.
[0069] Effect Example
[0070] (1) Antibacterial rate test
[0071] Test objects: antibacterial ion exchange resins prepared in Examples 1-8 and Comparative Examples 1-3.
[0072] Test method: Refer to Appendix B (absorption method) of GB 21551.2-2010 Special requirements for antibacterial materials with antibacterial, sterilization and purification functions for household and similar electrical appliances.
[0073] Test results: as shown in Table 1.
[0074] (2) Immersion effect test
[0075] Test objects: antibacterial ion exchange resins prepared in Examples 1-8 and Comparative Examples 1-3.
[0076] Test method: Refer to the method in Appendix B of Document No. 161 issued by the Ministry of Health (2001) (Annex 2) "Sanitary Safety Evaluation Standards for Drinking Water Transmission and Distribution Equipment and Protective Materials" (immersion time is 24 hours).
[0077] Test results: as shown in Table 1.
[0078] By comparing Example 1 with Comparative Examples 1-2, it can be seen that if the resin is only acidified without amino treatment, the antibacterial ion content in the water will exceed the standard after the immersion effect test of the obtained antibacterial ion exchange resin, and the immersion requirement will not be met.
[0079] By comparing Example 3 with Comparative Example 3, it can be seen that if the ion exchange resin is not subjected to acidification treatment, the antibacterial rate of the prepared antibacterial ion exchange resin is significantly reduced after the antibacterial rate test, and the antibacterial ability is limited.
[0080] Comparing Example 1 with Examples 4-8, it can be seen that different acid pH, antibacterial ion solution concentration, temperature and time of soaking the ion exchange resin in the antibacterial ion solution all have different degrees of influence on the antibacterial rate and soaking effect of the antibacterial ion exchange resin of the present invention.
[0081] In addition, during the research and development process, it was found that the antibacterial effect of the antibacterial resin made using ordinary resin (non-ion exchange resin) was poor.
Claims
1. A method for preparing an antibacterial ion exchange resin, characterized in that: It includes the following steps: ① Acidifying the ion exchange resin to obtain ion exchange resin A; ② subjecting the ion exchange resin A to an amination treatment to obtain an ion exchange resin B; ③ The ion exchange resin B is connected with antibacterial ions to obtain the antibacterial ion exchange resin.
2. The method for preparing the antibacterial ion exchange resin according to claim 1, characterized in that: It satisfies one or more of the following conditions ad; a. In step ①, the volume exchange capacity of the ion exchange resin is >1.4 mmol / mL, preferably 2-10 mmol / mL, such as 3 mmol / mL, 4 mmol / mL, 4.3 mmol / mL, 5 mmol / mL, 6 mmol / mL, 7 mmol / mL, 8 mmol / mL or 9 mmol / mL; b. In step ①, the density of the ion exchange resin is 0.7-1.2 g / mL, preferably 0.7-1.19 g / mL, such as 0.72 g / mL, 0.75 g / mL, 0.8 g / mL, 0.9 g / mL, 1.1 g / mL, 1.15 g / mL or 1.18 g / mL; c. In step ①, the particle size of the ion exchange resin is 0.3-1.2 mm, preferably 0.3-1.0 mm, such as 0.5 mm, 0.7 mm or 0.9 mm; d. In step ①, the water content of the ion exchange resin is 40%-60%, for example 50%; Preferably, the ion exchange resin is a weakly acidic ion exchange resin of model Lewatit S-8227 purchased from LANXESS Chemical.
3. The method for preparing the antibacterial ion exchange resin according to claim 1, characterized in that: In step ①, the acidification treatment comprises the following steps: placing the ion exchange resin in an acid solution for soaking once to obtain ion exchange resin A; Preferably, the solute in the acid solution is one or more of hydrochloric acid, sulfuric acid and nitric acid; Preferably, the pH of the acid solution is 3-6, preferably 4 or 5; Preferably, the soaking time is such that the ion exchange resin is completely converted into ion exchange resin A; Preferably, the ion exchange resin A is a hydrogen-type ion exchange resin.
4. The method for preparing the antibacterial ion exchange resin according to claim 1, characterized in that: In step ②, the amination treatment comprises the following steps: reacting the ion exchange resin A with an amine compound in the presence of a solvent to obtain the ion exchange resin B.
5. The method for preparing the antibacterial ion exchange resin according to claim 4, characterized in that: It satisfies one or more of the following conditions ad; a. The mass ratio of the ion exchange resin A to the amine compound is 100:(0.8-10), for example, 100:1, 100:1.5, 100:2, 100:2.5, 100:3, 100:3.5, 100:4, 100:5, 100:6, 100:7, 100:8 or 100:9; b. During the amination process, the mass concentration of the amine compound is 0.8-10wt%, such as 2wt%, 4wt%, 6wt% or 8wt%; c. The amine compound is one or more of diethylenetriamine, pentaethylenehexamine, tetraethylenepentamine, triethylenetetramine, tetraethylenepentamine, triethylenetetramine, ethylenediamine, polyvinylpyrrolidone, chitosan, N-carboxymethylchitosan, polyvinylimidazole, polyethyleneimine, polyallylamine, piperazine, p-aminobenzene and m-aminobenzene, preferably polyethyleneimine, triethylenetetramine or tetraethylenepentamine; d. During the amination treatment, the solvent is one or more of water, acetone, methanol and ethanol, preferably a mixture of at least one of acetone, methanol and ethanol and water.
6. The method for preparing the antibacterial ion exchange resin according to claim 4, characterized in that: It satisfies the following conditions a and / or b; a. The reaction temperature is 30-60°C, for example 45°C; b. The reaction time is 10-30 h, for example 20 h.
7. The method for preparing the antibacterial ion exchange resin according to claim 1, characterized in that: In step ③, the method of introducing antibacterial ions comprises the following steps: placing the ion exchange resin B in an antibacterial ion solution for secondary immersion.
8. The method for preparing the antibacterial ion exchange resin according to claim 7, characterized in that: It satisfies one or more of the following conditions ae; a. The mass ratio of the ion exchange resin B to the antibacterial ion is 100:(0.5-5), for example, 100:1, 100:1.5, 100:2, 100:2.5, 100:3, 100:3.5, 100:4, 100:4.5 or 100:4.8, preferably 100:(0.5-2); b. The mass concentration of the antibacterial ion solution is 0.5-5%, for example, 1.5%, 2%, 2.5%, 3%, 3.5%, 4% or 4.5%; c. The antibacterial ion solution is a salt solution containing antibacterial ions, and the salt containing antibacterial ions is one or more of zinc sulfate, zinc nitrate, zinc chloride and silver nitrate, preferably zinc sulfate, zinc nitrate, zinc chloride or silver nitrate; d. The temperature of the secondary soaking is 20-45°C, such as 30°C or 40°C, preferably 20-30°C, such as 25°C; e. The secondary immersion time is 10-80 min, preferably 15-80 min, for example 20 min, 30 min, 40 min, 50 min, 60 min or 70 min.
9. An antibacterial ion exchange resin, characterized in that It is prepared by the preparation method of the antibacterial ion exchange resin according to any one of claims 1 to 8; Preferably, the volume exchange capacity of the antibacterial ion exchange resin is >1.4 mmol / mL, preferably 2-10 mmol / mL, such as 3 mmol / mL, 4 mmol / mL, 4.3 mmol / mL, 5 mmol / mL, 6 mmol / mL, 7 mmol / mL, 8 mmol / mL or 9 mmol / mL; Preferably, the density of the antimicrobial ion exchange resin is 0.7-1.2 g / mL, preferably 0.7-1.19 g / mL, such as 0.72 g / mL, 0.75 g / mL, 0.8 g / mL, 0.9 g / mL, 1.1 g / mL, 1.15 g / mL or 1.18 g / mL; Preferably, the particle size of the antibacterial ion exchange resin is 0.3-1.2 mm, preferably 0.3-1.0 mm, such as 0.5 mm, 0.7 mm or 0.9 mm; Preferably, the water content of the antibacterial ion exchange resin is 40%-60%, such as 50%.
10. Use of the antibacterial ion exchange resin as claimed in claim 9 as a filter material in the fields of food, chemical industry or medicine; The application is preferably in the field of chemical water purification.
Citation Information
Cited By
Anti-aging modified anion exchange resin and preparation method thereof
CN121824815A