Binder and preparation method thereof, negative pole piece, secondary battery and electric device

By using fluorescent binder of modified polybutadiene or polystyrene butadiene copolymer in the negative electrode sheet, the problem of difficulty in analyzing the distribution of negative electrode binder in the prior art is solved, and the adhesive is improved Adhesion force and cycle stability of secondary battery.

CN119019582AActive Publication Date: 2024-11-26CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310593605.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

The existing negative electrode binders are difficult to obtain distribution information in the negative electrode material through characterization methods, and it is impossible to judge the quality of the binder dispersion process and the secondary battery failure analysis.

Method used

Modified polybutadiene and/or modified polystyrene butadiene copolymers are used as binders to introduce functional side groups of fluorescence effect on the main chain of butadiene repeating units, and the bond is observed using fluorescence microscope. The distribution of the agent is determined to determine whether the binder has risen, and then analyze the failure of the secondary battery.

Benefits of technology

Direct in-situ characterization of the adhesive distribution in the negative electrode sheet is achieved, the adhesive force and dispersion performance of the adhesive are improved, and the cycle stability of the secondary battery is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019582A_ABST
    Figure CN119019582A_ABST
Patent Text Reader

Abstract

The invention provides a binder, which comprises modified polybutadiene and / or a modified polystyrene-butadiene copolymer, the main chain of the modified polybutadiene comprises a butadiene repeating unit and a modified butadiene repeating unit; a main chain of the modified polystyrene-butadiene copolymer comprises a styrene repeating unit, a butadiene repeating unit and a modified butadiene repeating unit, the modified butadiene repeating unit is obtained by grafting at least one functional side group on a main chain of butadiene, and the functional side group has a fluorescent effect. The invention also provides a preparation method of the binder, a negative pole piece, a secondary battery and an electric device. According to the binder provided by the invention, the distribution condition of the negative electrode binder in a negative electrode plate and whether the negative electrode binder floats upwards or not can be directly represented in situ through a fluorescence microscope, and then secondary battery failure analysis is carried out.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a binder and a preparation method thereof, a negative electrode sheet, a secondary battery and an electrical device. Background Art

[0002] Secondary batteries can enhance the battery's power endurance, significantly improve the economic benefits of power storage, and promote the upgrading and transformation of consumer electronic products, which is of great significance to human life. Secondary batteries mainly include positive electrodes, negative electrodes, separators and electrolytes. The electrodes of secondary batteries usually include active materials, conductive agents, binders, solvents, etc. Among them, the binder plays a role in bonding the active material to the current collector, the active material to the active material, and the active material to the conductive agent. Although the amount of binder used is very small, it has an important influence on the improvement of the energy density of lithium-ion batteries, the reduction of internal resistance, and the cycle life of the entire secondary battery. The distribution of the binder in the electrode material directly affects the size of its bonding force with the active material, conductive agent and current collector.

[0003] However, it is difficult to obtain the distribution information of the existing negative electrode binders in the negative electrode materials through characterization methods, and it is impossible to judge the quality of the negative electrode binder dispersion process and perform secondary battery failure analysis.

[0004] The above statements are only used to provide background information related to the present application and do not necessarily constitute prior art. Summary of the invention

[0005] In view of the above problems, the present application provides a binder and a preparation method thereof, a negative electrode plate, a secondary battery and an electrical device to solve the above technical problems existing in the secondary battery.

[0006] In the first aspect, the present application provides a binder including modified polybutadiene and / or modified polystyrene butadiene copolymer, wherein the main chain of the modified polybutadiene includes butadiene repeating units and modified butadiene repeating units; the main chain of the polystyrene butadiene copolymer includes styrene repeating units, butadiene repeating units and modified butadiene repeating units, wherein the modified butadiene repeating units are at least one functional side group grafted onto the butadiene main chain, and the functional side group has a fluorescent effect.

[0007] In the technical solution of the embodiment of the present application, by grafting at least one functional side group with a fluorescent effect on the main chain of the butadiene repeating unit, when ultraviolet light or visible light with a shorter wavelength irradiates the functional side group, the binder will emit visible light of various colors and different intensities, and when the light source stops irradiating, the light disappears. Therefore, the negative electrode sheet of the embodiment of the present application is under a fluorescence microscope, and the ultraviolet light source of the fluorescence microscope irradiates the negative electrode sheet, and the binder in the negative electrode sheet emits fluorescence, and the distribution of the binder in the negative electrode sheet can be directly observed under the fluorescence microscope, and then the distribution of the negative electrode binder in the negative electrode sheet can be directly characterized in situ by the fluorescence microscope, whether the negative electrode binder floats, etc., and then the secondary battery failure analysis can be performed.

[0008] In some embodiments of the present application, the functional side group includes a large π bond.

[0009] In the technical solution of the embodiment of the present application, the functional side group includes a large π bond, which can produce a π-π conjugation effect with negative electrode materials such as graphite negative electrode and silicon-based negative electrode, thereby increasing the interaction between the negative electrode binder and the negative electrode material and improving the binding force of the negative electrode binder; and it can also improve the dispersion performance of negative electrode materials such as graphite negative electrode and silicon-based negative electrode, so that the dispersion of negative electrode materials in the negative electrode binder is more uniform, and thus the dispersion of negative electrode materials in the negative electrode electrode sheet is more uniform.

[0010] In some embodiments of the present application, the functional side group includes at least one of a condensed aromatic hydrocarbon free radical, a condensed aromatic hydrocarbon derivative free radical, a naphthalene diimide free radical, a naphthalene diimide derivative free radical, a triphenylamine free radical, or a triphenylamine derivative free radical.

[0011] In the technical solution of the embodiment of the present application, the condensed aromatic hydrocarbon free radical, the condensed aromatic hydrocarbon derivative free radical, the naphthalimide free radical, the naphthalimide derivative free radical, the triphenylamine free radical, or the triphenylamine derivative free radical all have good fluorescence effect. Therefore, the negative electrode sheet of the embodiment of the present application is under a fluorescence microscope, and the ultraviolet light source of the fluorescence microscope irradiates the negative electrode sheet, and the binder in the negative electrode sheet can quickly emit fluorescence, and the distribution of the binder in the negative electrode sheet can be directly observed under the fluorescence microscope, and then the distribution of the negative electrode binder in the negative electrode sheet can be characterized in situ.

[0012] Moreover, the condensed aromatic hydrocarbon radical, condensed aromatic hydrocarbon derivative radical, naphthalene diimide radical, naphthalene diimide derivative radical, triphenylamine radical, or triphenylamine derivative radical all contain a benzene ring, so the functional side group has high stability and high rigidity, thereby improving the mechanical properties of the adhesive.

[0013] In some embodiments of the present application, the functional side groups include At least one of the free radicals.

[0014] In the technical solution of the embodiment of the present application, The free radicals have good fluorescence effect, and the distribution of the binder in the negative electrode sheet can be directly observed under a fluorescence microscope, thereby in situ characterizing the distribution of the negative electrode binder in the negative electrode sheet.

[0015] and, The free radicals all contain multiple benzene rings, which are large in size. Therefore, the volume of the group containing multiple benzene rings is also relatively large, which can effectively improve the mechanical strength of the binder. At the same time, the large volume of benzene rings can reduce the agglomeration of binder molecules, swell less in the electrolyte, have a strong bonding effect, and improve the cycle stability of the secondary battery. The free radicals are easier to obtain, reducing the cost.

[0016] In some embodiments of the present application, the functional side group is formed by a functional molecule, which includes a thiol group, the sulfur atom in the thiol group is connected to the carbon atom in the modified butadiene repeating unit, and the hydrogen atom in the thiol group is replaced.

[0017] In the technical solution of the embodiment of the present application, the functional molecule includes a thiol group, which can undergo a click reaction with the chain segment of butadiene in the main chain. The click reaction has the advantages of high efficiency, mild reaction conditions, easy product purification, and simple post-processing, thereby allowing the functional side group to be quickly grafted onto the main chain of butadiene.

[0018] In some embodiments of the present application, the general formula of the functional side group is: R includes at least one of alkyl groups, and R' includes at least one of condensed aromatic hydrocarbon radicals, condensed aromatic hydrocarbon derivative radicals, naphthalene dicarboximide radicals, naphthalene dicarboximide derivative radicals, triphenylamine radicals, or triphenylamine derivative radicals.

[0019] In the technical solution of the embodiment of the present application, the condensed aromatic hydrocarbon free radical, the condensed aromatic hydrocarbon derivative free radical, the naphthalene imide free radical, the naphthalene imide derivative free radical, the triphenylamine free radical, or the triphenylamine derivative free radical all contain a benzene ring, so the functional side group has high stability and high rigidity, thereby improving the mechanical properties of the binder. Moreover, the condensed aromatic hydrocarbon free radical, the condensed aromatic hydrocarbon derivative free radical, the naphthalene imide free radical, the naphthalene imide derivative free radical, the triphenylamine free radical, or the triphenylamine derivative free radical has good fluorescence, and the distribution of the negative electrode binder in the negative electrode sheet can be directly observed using a fluorescence microscope.

[0020] In some embodiments of the present application, R includes x is greater than or equal to 1 and less than or equal to 9.

[0021] For linear side chains, within a certain range, as the length of the side chain increases, the flexibility of the polymer increases, which is beneficial to polymer diffusion and surface wetting, thus facilitating adhesion. However, if the side chain is too long, it will lead to entanglement between molecules, which is not conducive to cohesion, and reduce the flexibility and adhesion of the polymer.

[0022] In the technical solution of the embodiment of the present application, by controlling x to be greater than or equal to 1 and less than or equal to 9, the side chain in the modified polybutadiene or modified polystyrene butadiene copolymer is within a reasonable length range, thereby improving the flexibility and bonding performance of the adhesive.

[0023] In some embodiments of the present application, R' includes At least one of the free radicals.

[0024] In the technical solution of the embodiment of the present application, The free radicals contain multiple benzene rings, which are relatively large in size. Therefore, the volume of the group containing multiple benzene rings is also relatively large, which can effectively improve the mechanical strength of the binder. At the same time, the large volume of benzene rings can reduce the agglomeration of binder molecules, swell less in the electrolyte, have a strong bonding effect, and improve the cycle stability of the secondary battery.

[0025] In some embodiments of the present application, the modified polystyrene butadiene copolymer is a block copolymer or a random copolymer.

[0026] In the technical solution of the embodiment of the present application, the styrene-butadiene random copolymer and the styrene-butadiene block copolymer have the advantages of excellent tensile strength, elasticity and electrical properties, small permanent deformation, good flexibility and resilience, etc., which can improve the mechanical strength and flexibility of the adhesive.

[0027] In some embodiments of the present application, the number average molecular weight of the modified polybutadiene is 10,000-1,000,000, and the number average molecular weight of the modified polystyrene butadiene copolymer is 10,000-1,000,000.

[0028] If the number average molecular weight of the modified polybutadiene and the modified polystyrene butadiene copolymer is too small, for example, less than 10,000, the mechanical properties of the binder are poor and it is easy to break. If the molecular weight of the modified polybutadiene and the modified polystyrene butadiene copolymer is too large, for example, greater than 1 million, the flexibility of the binder is reduced, and it is not conducive to the dispersion of the binder. The binder cannot quickly diffuse into the negative electrode active material, and the negative electrode active materials cannot be fully bonded. Moreover, too large a molecular weight will also affect the wettability of the electrolyte.

[0029] In the technical solution of the embodiment of the present application, by controlling the number average molecular weight of the modified polybutadiene to be 10,000-1,000,000 and the number average molecular weight of the modified polystyrene butadiene copolymer to be 10,000-1,000,000, the mechanical properties of the binder are improved while ensuring the flexibility, dispersibility and electrolyte wettability of the binder.

[0030] In some embodiments of the present application, the modified polybutadiene includes modified cis-1,4-polybutadiene.

[0031] In the technical solution of the embodiment of the present application, the distance between the molecular chains in cis-1,4-polybutadiene is large, which makes it easier to modify. In addition, the modified cis-1,4-polybutadiene has the characteristics of high elasticity and low hysteresis, high tensile strength and wear resistance, thereby improving the performance of the adhesive.

[0032] In a second aspect, the present application provides a method for preparing the binder in any of the above embodiments, comprising:

[0033] The functional molecule is mixed with polybutadiene and / or polystyrene butadiene copolymer, the functional molecule reacts with the polybutadiene and / or polystyrene butadiene copolymer, and the functional molecule is grafted onto the main chain of the butadiene repeating unit in the polybutadiene and / or the polystyrene butadiene copolymer to form a functional side group;

[0034] The reaction product of the above reaction is extracted to obtain the binder.

[0035] In the technical solution of the embodiment of the present application, by mixing the functional molecule with polybutadiene and / or polystyrene butadiene copolymer, at least one functional side group with a fluorescent effect is grafted on the main chain of the butadiene repeating unit, and the distribution of the negative electrode binder in the negative electrode sheet, whether the negative electrode binder floats, etc. can be directly characterized in situ by a fluorescence microscope, and then secondary battery failure analysis can be performed. Moreover, the preparation method is simple and fast.

[0036] In some embodiments of the present application, the method for preparing the binder includes:

[0037] adding the functional molecule and polybutadiene and / or polystyrene butadiene copolymer into a solvent and mixing them to obtain a mixed solution;

[0038] Performing photoinitiation or thermal initiation on the mixed solution to allow the functional molecules to react with the polybutadiene and / or polystyrene butadiene copolymer;

[0039] A precipitant is added to extract the reaction product of the above reaction to obtain a binder.

[0040] In the technical solution of the embodiment of the present application, the functional molecule and the polybutadiene and / or polystyrene butadiene copolymer are added to the solvent, so that the functional molecule and the polybutadiene and / or polystyrene butadiene copolymer are mixed more evenly and are more conducive to the reaction; through photo-initiation or thermal-initiation, the functional molecule and the polybutadiene and / or polystyrene butadiene copolymer react quickly, and the reaction product is purified by adding a precipitant. The method is simple, the product is easy to purify, and the cost is low.

[0041] In some embodiments of the present application, the functional molecule includes a thiol group, and the thiol group undergoes a click reaction with polybutadiene and / or polystyrene butadiene copolymer.

[0042] In the technical solution of the embodiment of the present application, the functional molecule includes a thiol group. Under light initiation or heat initiation, the thiol group can undergo a click reaction with the double bond in the butadiene repeating unit. The click reaction has high efficiency, so that the functional side group can be quickly grafted onto the side chain of the butadiene segment. In addition, the click reaction conditions are mild, the product is easy to purify, and the post-processing is simple.

[0043] In some embodiments of the present application, the molar ratio of polybutadiene and / or polystyrene butadiene copolymer to the functional molecule is greater than or equal to 2:1 and less than or equal to 3:1.

[0044] If the molar ratio of polybutadiene and / or polystyrene-butadiene copolymer to functional side groups is too small, for example, less than 2:1, it is easy to cause too many functional side groups, resulting in too low flexibility of the binder; if the molar ratio of polybutadiene and / or polystyrene-butadiene copolymer to functional side groups is too large, for example, greater than 3:1, there are too few functional side groups, the fluorescence effect is not obvious, and the mechanical properties of the binder are low. In the technical scheme of the embodiment of the present application, when the molar ratio of polybutadiene and / or polystyrene-butadiene copolymer to functional side groups is controlled to be greater than or equal to 2:1 and less than or equal to 3:1, the adhesion, flexibility and mechanical properties of the binder are relatively good, and the fluorescence effect is obvious.

[0045] In some embodiments of the present application, the solvent includes at least one of chloroform, cyclohexane and benzene.

[0046] In the technical solution of the embodiment of the present application, chloroform, cyclohexane and benzene have relatively good solubility, and functional molecules, polybutadiene, and polystyrene butadiene copolymer can be quickly dissolved in the above solvents, and the cost of the above solvents is relatively low.

[0047] In some embodiments of the present application, the precipitant includes at least one of methanol, water, and acetone.

[0048] In the technical solution of the embodiment of the present application, the above-mentioned precipitant can quickly form a precipitate with the reaction product of the functional molecule and polybutadiene and / or polystyrene butadiene copolymer, and then extract the reaction product.

[0049] In some embodiments of the present application, after adding a precipitant to extract the reaction product of the above reaction, the extracted reaction product is further freeze-dried.

[0050] In the technical solution of the embodiment of the present application, freeze drying can quickly remove the solvent and has little effect on the performance of the reaction product.

[0051] In a third aspect, the present application provides a negative electrode plate, comprising the binder of any one of the above embodiments or a binder prepared by the method for preparing the binder of any one of the above embodiments.

[0052] In a fourth aspect, the present application provides a secondary battery, comprising the negative electrode sheet of any of the above embodiments.

[0053] In a fifth aspect, the present application provides an electrical device, comprising a secondary battery according to any of the above embodiments.

[0054] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without paying creative work.

[0056] Figure 1 A schematic diagram of the structure of an electric device in some embodiments of the present application;

[0057] Figure 2 A schematic diagram of the exploded structure of a battery according to some embodiments of the present application;

[0058] Figure 3 A schematic diagram of the exploded structure of a battery cell according to some embodiments of the present application;

[0059] Figure 4 A flow chart of a method for preparing an adhesive according to some embodiments of the present application;

[0060] Figure 5 This is a flow chart of a method for preparing an adhesive according to some embodiments of the present application.

[0061] In the drawings, the drawings are not drawn to scale.

[0062] Marking description: electrical device 1000;

[0063] Battery 100, controller 200, motor 300;

[0064] Box body 10, first part 11, second part 12;

[0065] Battery cell 20, end cover 21, electrode terminal 21a, shell 22, battery cell assembly 23, and tab 23a. DETAILED DESCRIPTION

[0066] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0067] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0068] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0069] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0070] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of the associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0071] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0072] It is difficult to obtain the distribution information of the existing negative electrode binders in the negative electrode materials through characterization methods, and it is impossible to judge the quality of the negative electrode binder dispersion process and perform secondary battery failure analysis.

[0073] In order to solve the above-mentioned technical problems existing in secondary batteries, the present invention designs a binder, including modified polybutadiene and / or modified polystyrene butadiene copolymer, and grafts at least one functional side group with a fluorescent effect on the main chain of the butadiene repeating unit to achieve in situ characterization of the distribution of the negative electrode binder in the negative electrode pole piece through a fluorescence microscope, and judges whether the binder floating occurs in the negative electrode pole piece, judges the quality of the negative electrode binder dispersion process, and performs secondary battery failure analysis.

[0074] Based on the above considerations, in order to solve the problems that it is difficult to obtain the distribution information of the existing negative electrode binder in the negative electrode material through characterization methods, it is impossible to judge the quality of the negative electrode binder dispersion process, and to perform secondary battery failure analysis, a binder is designed, including modified polybutadiene and / or modified polystyrene butadiene copolymer, the main chain of the modified polybutadiene includes butadiene repeating units and modified butadiene repeating units; the main chain of the polystyrene butadiene copolymer includes styrene repeating units, butadiene repeating units and modified butadiene repeating units, and the modified butadiene repeating unit is a butadiene main chain grafted with at least one functional side group, and the functional side group has a fluorescent effect.

[0075] By grafting at least one functional side group with a fluorescent effect on the main chain of the butadiene repeating unit, the distribution of the negative electrode binder in the negative electrode plate and whether the negative electrode binder floats can be directly characterized in situ by fluorescence microscopy, thereby judging the quality of the negative electrode binder dispersion process and performing secondary battery failure analysis.

[0076] The adhesive disclosed in the embodiments of the present application can be applied to battery cells, and the battery cells can be used in electrical devices that use batteries as power sources or various energy storage systems that use batteries as energy storage elements. Electrical devices can be, but are not limited to, mobile phones, tablets, laptops, electric toys, electric tools, battery cars, electric cars, ships, spacecraft, etc. Among them, electric toys can include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc., and spacecraft can include airplanes, rockets, space shuttles, and spacecraft, etc.

[0077] For the convenience of description, the following embodiments are described by taking an electric device 1000 of an embodiment of the present application as a vehicle as an example.

[0078] Please refer to Figure 1 , Figure 1 A schematic diagram of the structure of an electric device 1000 provided for some embodiments of the present application. The electric device 1000 may be a fuel vehicle, a gas vehicle or a new energy vehicle. The new energy vehicle may be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. A battery 100 is arranged inside the electric device 1000, and the battery 100 may be arranged at the bottom, head or tail of the electric device 1000. The battery 100 may be used to power the electric device 1000. For example, the battery 100 may be used as an operating power source for the electric device 1000. The electric device 1000 may also include a controller 200 and a motor 300. The controller 200 is used to control the battery 100 to power the motor 300, for example, for starting, navigating and driving the electric device 1000.

[0079] In some embodiments of the present application, the battery 100 can not only serve as an operating power source for the electrical device 1000, but also serve as a driving power source for the electrical device 1000, replacing or partially replacing fuel or natural gas to provide driving power for the electrical device 1000.

[0080] Please refer to Figure 2 , Figure 2 Schematic diagram of the exploded structure of the battery 100 provided for some embodiments of the present application. The battery 100 includes a box 10 and a battery cell 20, and the battery cell 20 is contained in the box 10. Among them, the box 10 is used to provide a storage space for the battery cell 20, and the box 10 can adopt a variety of structures. In some embodiments, the box 10 may include a first part 11 and a second part 12, the first part 11 and the second part 12 cover each other, and the first part 11 and the second part 12 jointly define a storage space for accommodating the battery cell 20. The second part 12 can be a hollow structure with one end open, the first part 11 can be a plate-like structure, and the first part 11 covers the open side of the second part 12, so that the first part 11 and the second part 12 jointly define a storage space; the first part 11 and the second part 12 can also be hollow structures with one side open, and the open side of the first part 11 covers the open side of the second part 12. Of course, the box 10 formed by the first part 11 and the second part 12 can be in a variety of shapes, such as a cylinder, a cuboid, etc.

[0081] In the battery 100, there may be multiple battery cells 20, and the multiple battery cells 20 may be connected in series, in parallel, or in a mixed connection. A mixed connection means that the multiple battery cells 20 are both connected in series and in parallel. The multiple battery cells 20 may be directly connected in series, in parallel, or in a mixed connection, and then the whole formed by the multiple battery cells 20 is accommodated in the box 10; of course, the battery 100 may also be a battery module formed by connecting multiple battery cells 20 in series, in parallel, or in a mixed connection, and then the multiple battery modules are connected in series, in parallel, or in a mixed connection to form a whole, and accommodated in the box 10. The battery 100 may also include other structures, for example, the battery 100 may also include a busbar component for realizing electrical connection between the multiple battery cells 20.

[0082] Each battery cell 20 may be a secondary battery, a lithium-sulfur battery, a lithium-ion battery or a lithium metal battery, but is not limited thereto. The battery cell 20 may be cylindrical, flat, rectangular or in other shapes.

[0083] Please refer to Figure 3 , Figure 3 The schematic diagram of the exploded structure of the battery cell 20 provided in some embodiments of the present application. The battery cell 20 refers to the smallest unit that constitutes the battery. Figure 3 The battery cell 20 includes an end cover 21, a shell 22, a battery cell assembly 23 and other functional components.

[0084] The end cap 21 refers to a component that covers the opening of the shell 22 to isolate the internal environment of the battery cell 20 from the external environment. Without limitation, the shape of the end cap 21 can be adapted to the shape of the shell 22 to match the shell 22. The end cap 21 can be made of a material with a certain hardness and strength (such as aluminum alloy), so that the end cap 21 is not easily deformed when squeezed and collided, so that the battery cell 20 can have a higher structural strength and the safety performance can also be improved. Functional components such as electrode terminals 21a can be provided on the end cap 21. The electrode terminal 21a can be used to electrically connect to the battery cell assembly 23 for outputting or inputting electrical energy of the battery cell 20. In some embodiments, the end cap 21 can also be provided with a pressure relief mechanism for releasing the internal pressure when the internal pressure or temperature of the battery cell 20 reaches a threshold. The material of the end cap 21 can also be a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiments of the present application do not impose special restrictions on this. In some embodiments, an insulating member may be provided inside the end cap 21, and the insulating member may be used to isolate the electrical connection components in the housing 22 from the end cap 21 to reduce the risk of short circuit. For example, the insulating member may be plastic, rubber, or the like.

[0085] The shell 22 is a component used to cooperate with the end cover 21 to form the internal environment of the battery cell 20, wherein the formed internal environment can be used to accommodate the battery cell assembly 23, electrolyte and other components. The shell 22 and the end cover 21 can be independent components, and an opening can be set on the shell 22, and the internal environment of the battery cell 20 is formed by covering the opening with the end cover 21 at the opening. Without limitation, the end cover 21 and the shell 22 can also be integrated. Specifically, the end cover 21 and the shell 22 can form a common connection surface before other components are put into the shell, and when the interior of the shell 22 needs to be encapsulated, the end cover 21 covers the shell 22. The shell 22 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shape of the shell 22 can be determined according to the specific shape and size of the battery cell assembly 23. The material of the shell 22 can be various, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiment of the present application does not impose any special restrictions on this.

[0086] The battery cell assembly 23 is a component in the battery cell 100 where electrochemical reactions occur. One or more battery cell assemblies 23 may be included in the housing 22. The battery cell assembly 23 is mainly formed by winding or stacking cathode sheets and anode sheets, and a separator is usually provided between the cathode sheets and the anode sheets. The parts of the cathode sheets and the anode sheets with active substances constitute the main body of the battery cell assembly, and the parts of the cathode sheets and the anode sheets without active substances each constitute a tab 23a. The cathode tab and the anode tab may be located together at one end of the main body or respectively at both ends of the main body. During the charge and discharge process of the battery, the cathode active substance and the anode active substance react with the electrolyte, and the tab 23a connects the electrode terminals to form a current loop.

[0087] According to some embodiments of the present application, the present application provides a binder including modified polybutadiene and / or modified polystyrene butadiene copolymer, wherein the main chain of the modified polybutadiene includes butadiene repeating units and modified butadiene repeating units; the main chain of the polystyrene butadiene copolymer includes styrene repeating units, butadiene repeating units and modified butadiene repeating units, wherein the modified butadiene repeating units are at least one functional side group grafted onto the butadiene main chain, and the functional side group has a fluorescent effect.

[0088] The fluorescence effect of the functional side group means that when ultraviolet light or visible light with a shorter wavelength irradiates the functional side group of the compound, the functional side group of the compound will emit visible light of various colors and intensities, and when the light source stops irradiating, the light disappears.

[0089] In some embodiments, the binder includes only modified polybutadiene. In some embodiments, the binder includes only modified polystyrene butadiene copolymer. In some embodiments, the binder includes a mixture of modified polybutadiene and modified polystyrene butadiene copolymer.

[0090] As an example, the structural formula of the binder can be, but is not limited to, represented by: When k is equal to 0, it is a modified polybutadiene, and when k is greater than 0, it is a modified polystyrene butadiene copolymer. The functional side groups are not limited to those in the above exemplary formula. It can also be other functional side groups with fluorescent effects.

[0091] By grafting at least one functional side group with a fluorescent effect on the main chain of the butadiene repeating unit, when ultraviolet light or visible light with a shorter wavelength irradiates the functional side group, the binder will emit visible light of various colors and different intensities, and when the light source stops irradiating, the light disappears. Therefore, the negative electrode sheet of the embodiment of the present application is under a fluorescent microscope, and the ultraviolet light source of the fluorescent microscope irradiates the negative electrode sheet, and the binder in the negative electrode sheet emits fluorescence, and the distribution of the binder in the negative electrode sheet can be directly observed under the fluorescent microscope, and then the fluorescent microscope is used to directly characterize the distribution of the negative electrode binder in the negative electrode sheet in situ, whether the negative electrode binder floats, etc., to judge the quality of the negative electrode binder dispersion process, and to perform secondary battery failure analysis.

[0092] Moreover, the butadiene repeating unit is a flexible segment, which is easy to process and can form a flexible negative electrode sheet with the negative electrode material.

[0093] According to some embodiments of the present application, the functional side group includes a large π bond.

[0094] In polyatomic molecules, if there are parallel p orbitals, they overlap and connect to form a whole. The p electrons move between multiple atoms to form a π-type chemical bond. This π bond that is not limited to two atoms is called a delocalized π bond, or a conjugated large π bond, or a large π bond for short. It can form a π-π conjugation with molecules containing π bonds.

[0095] The large π bond in the functional side group in the embodiment of the present application can produce π-π conjugation with negative electrode materials such as graphite negative electrode and silicon-based negative electrode, increase the interaction between the negative electrode binder and the negative electrode material, and improve the binding force of the negative electrode binder; and can also improve the dispersion performance of negative electrode materials such as graphite negative electrode and silicon-based negative electrode, so that the dispersion of negative electrode materials in the negative electrode sheet is more uniform. This solves the technical problem that the existing binder has a small binding force with negative electrode materials such as graphite negative electrode and silicon-based negative electrode, and the dispersion performance of negative electrode materials such as graphite negative electrode and silicon-based negative electrode is poor.

[0096] Furthermore, since the adhesive has both a flexible segment (a segment of polybutadiene) and a rigid segment (including a functional side group of a large π bond), the adhesive of the present application can adjust the degree of adhesion and mechanical properties according to requirements.

[0097] According to some embodiments of the present application, the functional side group includes at least one of a condensed aromatic hydrocarbon free radical, a condensed aromatic hydrocarbon derivative free radical, a naphthalene diimide free radical, a naphthalene diimide derivative free radical, a triphenylamine free radical, or a triphenylamine derivative free radical.

[0098] The condensed ring aromatic hydrocarbon free radical, the condensed ring aromatic hydrocarbon derivative free radical, the naphthalene diimide free radical, the naphthalene diimide derivative free radical, the triphenylamine free radical, or the triphenylamine derivative free radical all have good fluorescence effect. Therefore, when the negative electrode sheet of the embodiment of the present application is under a fluorescence microscope and the ultraviolet light source of the fluorescence microscope irradiates the negative electrode sheet, the binder in the negative electrode sheet can quickly emit fluorescence, and the distribution of the binder in the negative electrode sheet can be directly observed under the fluorescence microscope, thereby characterizing the distribution of the negative electrode binder in the negative electrode sheet in situ.

[0099] Moreover, the condensed aromatic hydrocarbon radical, condensed aromatic hydrocarbon derivative radical, naphthalene diimide radical, naphthalene diimide derivative radical, triphenylamine radical, or triphenylamine derivative radical all contain a benzene ring, so the functional side group has high stability and high rigidity, thereby improving the mechanical properties of the adhesive.

[0100] According to some embodiments of the present application, the functional side groups include At least one of the free radicals.

[0101] The free radicals have good fluorescence effect, and the distribution of the binder in the negative electrode sheet can be directly observed under a fluorescence microscope, and then the distribution of the negative electrode binder in the negative electrode sheet can be characterized in situ.

[0102] and, The free radicals all contain multiple benzene rings, which are large in size. Therefore, the volume of the group containing multiple benzene rings is also relatively large, which can effectively improve the mechanical strength of the binder. At the same time, the large volume of benzene rings can reduce the agglomeration of binder molecules, swell less in the electrolyte, have a strong bonding effect, and improve the cycle stability of the secondary battery. The free radicals are easier to obtain, reducing the cost.

[0103] According to some embodiments of the present application, the functional side group is formed by a functional molecule, which includes a thiol group, the sulfur atom in the thiol group is connected to the carbon atom in the modified butadiene repeating unit, and the hydrogen atom in the thiol group is replaced.

[0104] The functional side groups are formed by functional molecules including thiol groups, which can undergo a click reaction with the chain segments of butadiene in the main chain. The click reaction has the advantages of high efficiency, mild reaction conditions, easy product purification, and simple post-treatment, thereby allowing the functional side groups to be quickly grafted onto the main chain of butadiene.

[0105] In some alternative embodiments, the functional side group includes a thiol group, and the sulfur atom in the thiol group is directly connected to a carbon atom in the modified butadiene repeating unit.

[0106] According to some embodiments of the present application, the general formula of the functional side group is: R includes at least one of alkyl groups, and R' includes at least one of condensed aromatic hydrocarbon radicals, condensed aromatic hydrocarbon derivatives, naphthalene dicarboxylic acid imide radicals, naphthalene dicarboxylic acid imide derivative radicals, triphenylamine radicals, or triphenylamine derivative radicals.

[0107] The condensed aromatic hydrocarbon free radical, the condensed aromatic hydrocarbon derivative free radical, the naphthalene imide free radical, the naphthalene imide derivative free radical, the triphenylamine free radical, or the triphenylamine derivative free radical all contain a benzene ring, which is large in size and highly stable, so the functional side group has high stability and high rigidity, thereby improving the mechanical properties of the binder. Moreover, the condensed aromatic hydrocarbon free radical, the condensed aromatic hydrocarbon derivative free radical, the naphthalene imide free radical, the naphthalene imide derivative free radical, the triphenylamine free radical, or the triphenylamine derivative free radical all have a good fluorescence effect, and a fluorescence microscope can be used to directly observe the distribution of the negative electrode binder in the negative electrode sheet.

[0108] The type and quantity of the alkyl group can be selected according to the implementation requirements. For example, the alkyl group can be, but is not limited to, a methyl group, an ethyl group, a propyl group, etc. Optionally, according to some embodiments of the present application, R includes x is greater than or equal to 1 and less than or equal to 9.

[0109] For linear side chains, within a certain range, as the length of the side chain increases, the flexibility of the polymer increases, which is beneficial to polymer diffusion and surface wetting, thus facilitating adhesion. However, if the side chain is too long, it will lead to entanglement between molecules, which is not conducive to cohesion, and reduce the flexibility and adhesion of the polymer.

[0110] In some embodiments of the present application, x is controlled to be greater than or equal to 1 and less than or equal to 9, so that the side chains in the modified polybutadiene or modified polystyrene butadiene copolymer are within a reasonable length range, thereby improving the flexibility and bonding performance of the adhesive.

[0111] Optionally, according to some embodiments of the present application, R' comprises At least one of the free radicals.

[0112] The free radicals of all contain multiple benzene rings, which are relatively large in size. Therefore, the above-mentioned groups containing multiple benzene rings can effectively improve the mechanical strength of the binder, while reducing the agglomeration of binder molecules, swelling less in the electrolyte, having a strong bonding effect, and improving the cycle stability of the secondary battery. The free radicals have good fluorescence, and the distribution of the negative electrode binder in the negative electrode sheet can be directly observed using a fluorescence microscope.

[0113] In some optional embodiments, the general formula of the functional side group is R' is of free radicals.

[0114] According to some embodiments of the present application, the number of butadiene repeating units in the main chain of the modified polybutadiene is m, the number of modified butadiene repeating units is n, and the ratio of m to n ranges from (1:100) to (100:1).

[0115] As an example, the ratio of m to n can range from 1, 5, 10, 10.5, 20, 27, 33.5, 40, 45.5, 50, 60.5, 70, 90, 99.9, 100, etc. The ratio of m to n can also range from 1-5, 5-10, 10-10.5, 10.5-20, 20-27, 27-33.5, 33.5-40, 40-45.5, 45.5-50, 50-60.5, 60.5-70, 70-90, 90-99.5, 99.5-100, etc. The ratio of m to n only needs to satisfy the range of (1:100)-(100:1).

[0116] By adjusting the content of functional side groups, the bonding degree and mechanical properties of the adhesive can be easily adjusted to meet customized needs.

[0117] According to some embodiments of the present application, the number of styrene repeating units in the main chain of the polystyrene butadiene copolymer is k, the number of butadiene repeating units is m, the number of modified butadiene repeating units is n, the ratio of m to n ranges from (1:100) to (100:1), and the ratio of k to m ranges from greater than 0 to less than or equal to (100:1).

[0118] As an example, the ratio of m to n can range from 1, 5, 10, 10.5, 20, 27, 33.5, 40, 45.5, 50, 60.5, 70, 90, 99.5, 100, etc. The ratio of m to n can also range from 1-5, 5-10, 10-10.5, 10.5-20, 20-27, 27-33.5, 33.5-40, 40-45.5, 45.5-50, 50-60.5, 60.5-70, 70-90, 90-99.5, 99.5-100, etc. It can be adjusted according to actual needs as long as it meets the range of (1:100)-(100:1).

[0119] As an example, the ratio range of k to m can be 0.1, 1, 5, 10, 15.5, 20, 30.5, 40, 50.5, 70, 80, 90, 99.5, 100, etc. The ratio range of k to m can also be 0.1-1, 1-5, 5-10, 10-15.5, 15.5-20, 20-30.5, 30.5-40, 40-50.5, 50.5-70, 70-80, 80-90, 90-99.5, 99.5-100, etc., and can be adjusted according to actual needs as long as it satisfies the range greater than 0 and less than or equal to (100:1).

[0120] By adjusting the ratio of the number of styrene repeating units and butadiene repeating units, as well as the content of functional side groups, the bonding degree, elasticity and mechanical properties of the adhesive can be easily adjusted to customize to meet the needs.

[0121] According to some embodiments of the present application, the modified polystyrene butadiene copolymer is a block copolymer or a random copolymer.

[0122] Styrene-butadiene random copolymer and styrene-butadiene block copolymer have the advantages of excellent tensile strength, elasticity and electrical properties, small permanent deformation, good flexure and resilience, etc., which can improve the mechanical strength and flexibility of the adhesive.

[0123] According to some embodiments of the present application, the number average molecular weight of the modified polybutadiene is 10,000-1,000,000, and the number average molecular weight of the modified polystyrene butadiene copolymer is 10,000-1,000,000.

[0124] As an example, the number average molecular weight of the modified polybutadiene can be 10,000, 50,000, 100,000, 250,000, 360,000, 480,000, 600,000, 750,000, 900,000, 990,000, 1,000,000, etc., or it can be 10,000-50,000, 50,000-100,000, 100,000-250,000, 250,000-360,000, 360,000-480,000, 480,000-600,000, 600,000-750,000, 750,000-900,000, 900,000-990,000, 990,000-1,000,000, etc., and can be adjusted according to actual needs, as long as the number average molecular weight of the modified polybutadiene is 10,000-1,000,000.

[0125] The number average molecular weight of the modified polystyrene butadiene copolymer can be 10,000, 50,000, 100,000, 250,000, 360,000, 480,000, 600,000, 750,000, 900,000, 990,000, 1,000,000, etc., or can be 10,000-50,000, 50,000-100,000, 100,000-250,000, 250,000-360,000, 360,000-480,000, 480,000-600,000, 600,000-750,000, 750,000-900,000, 900,000-990,000, 990,000-1,000,000, etc., and can be adjusted according to actual needs, as long as the number average molecular weight of the modified polystyrene butadiene copolymer is 10,000-1,000,000.

[0126] If the number average molecular weight of the modified polybutadiene or modified polystyrene butadiene copolymer is too small, for example, less than 10,000, the flexibility of the polymer main chain is low, the mechanical strength of the polymer is poor, and the viscosity of the polymer is low, thereby making the flexibility, mechanical properties and viscosity of the binder low; if the number average molecular weight of the modified polybutadiene or modified polystyrene butadiene copolymer is too large, for example, greater than 1 million, the molecular chains of the polymer are easily entangled together, the flexibility of the polymer is reduced, and the fluidity is too low, which is not conducive to the dispersion of the binder. The binder cannot diffuse quickly into the interior of the negative electrode active material, and the negative electrode active materials cannot be fully bonded. In addition, too large a molecular weight will also affect the wettability of the electrolyte.

[0127] In the technical solution of the embodiment of the present application, by controlling the number average molecular weight of the modified polybutadiene to 10,000-1,000,000 and the number average molecular weight of the modified polystyrene butadiene copolymer to 10,000-1,000,000, the adhesive has good flexibility, dispersibility, adhesion, and mechanical properties.

[0128] According to some embodiments of the present application, the modified polybutadiene includes modified cis-1,4-polybutadiene.

[0129] The distance between the molecular chains of cis-1,4-polybutadiene is large, so it is easier to modify. In addition, the modified cis-1,4-polybutadiene has the characteristics of high elasticity and low hysteresis, high tensile strength and wear resistance, thereby improving the performance of the adhesive.

[0130] It is understood that the modified polybutadiene of the present application is not limited to modified cis-1,4-polybutadiene. In other embodiments, the modified polybutadiene may also include modified trans-1,4-polybutadiene, modified 1,3-polybutadiene, and / or modified 1,2-polybutadiene.

[0131] See also Figure 4 According to some embodiments of the present application, the present application also provides a method for preparing the binder of any of the above embodiments, comprising the following steps:

[0132] The functional molecule is mixed with polybutadiene and / or polystyrene butadiene copolymer, the functional molecule reacts with the polybutadiene and / or polystyrene butadiene copolymer, and the functional molecule is grafted onto the main chain of the butadiene repeating unit in the polybutadiene and / or the polystyrene butadiene copolymer to form a functional side group;

[0133] The reaction product of the above reaction is extracted to obtain the binder.

[0134] Polybutadiene corresponds to the above-mentioned modified polybutadiene, and polystyrene butadiene copolymer corresponds to the above-mentioned modified polystyrene butadiene copolymer, which will not be described again here.

[0135] The functional molecules refer to the groups before the functional side groups in the binder form free radicals.

[0136] In some embodiments, the general formula of the functional molecule can be: R includes at least one of alkyl groups, and R′ includes at least one of condensed aromatic hydrocarbons, condensed aromatic hydrocarbon derivatives, naphthalene dicarboximide, naphthalene dicarboximide derivatives, triphenylamine, or triphenylamine derivatives.

[0137] In some optional embodiments, R includes x is greater than or equal to 1 and less than or equal to 9.

[0138] In some optional embodiments, R' comprises At least one of .

[0139] See also Figure 5 According to some embodiments of the present application, the method for preparing the adhesive of any of the above embodiments includes: adding functional molecules and polybutadiene and / or polystyrene butadiene copolymer to a solvent and mixing them to obtain a mixed solution; performing photoinitiation or thermal initiation on the mixed solution to allow the functional molecules to react with the polybutadiene and / or polystyrene butadiene copolymer; adding a precipitant to extract the reaction product of the above reaction to obtain the adhesive.

[0140] The order in which the functional molecules and the polybutadiene and / or polystyrene butadiene copolymer are added to the solvent is not limited.

[0141] In some optional embodiments, the mixed solution is subjected to ultraviolet irradiation to allow the functional molecules to react with polybutadiene and / or polystyrene butadiene copolymer. The time of ultraviolet irradiation can be adjusted according to actual needs. Optionally, the mixed solution is subjected to ultraviolet irradiation for 4-12 hours. If the ultraviolet irradiation time is short, such as less than 4 hours, the fluorescence effect is not obvious, and the distribution of the binder cannot be well observed; if the ultraviolet irradiation time is too long, such as more than 12 hours, it is easy to cause the performance of the binder to deteriorate. The mixed solution is subjected to ultraviolet irradiation for 4-12 hours, while ensuring that the binder has good performance, the distribution of the binder can be better observed.

[0142] The wavelength of the ultraviolet light can be set according to actual needs. For example, in some optional embodiments, ultraviolet light is used for irradiation without adding a photoinitiator, and the wavelength of the ultraviolet light can be, but is not limited to, 254 nm. In other optional embodiments, ultraviolet light is used for irradiation and a photoinitiator benzophenone is added, and the wavelength of the ultraviolet light can be, but is not limited to, 254 nm or 365 nm.

[0143] In some other optional embodiments, the mixed solution is irradiated with white light so that the functional molecules react with polybutadiene and / or polystyrene butadiene copolymer. In some other optional embodiments, the mixed solution is thermally initiated so that the functional molecules react with polybutadiene and / or polystyrene butadiene copolymer. The initiator during thermal initiation may be, but is not limited to, azo initiators such as azobisisobutyronitrile, and the initiation temperature may be 55°C-75°C. In some other optional embodiments, the temperature during thermal initiation is 70°C, at which time the bond breaking speed of the initiator is more appropriate.

[0144] In some embodiments of the present application, the ultraviolet irradiation can be performed by, but not limited to, an ultraviolet lamp or other instruments capable of emitting ultraviolet rays, and can be selected according to actual needs.

[0145] According to some embodiments of the present application, the functional molecule includes a thiol group, and the thiol group undergoes a click reaction with polybutadiene and / or polystyrene butadiene copolymer.

[0146] In the prior art, it is very difficult to graft a benzene ring-containing group onto the main chain of butadiene, and the method is very complicated.

[0147] In the embodiments of the present application, under the irradiation of ultraviolet light, the thiol group can undergo a click reaction with the double bond in the butadiene repeating unit. The click reaction has high efficiency, so that functional molecules, especially functional molecules including benzene rings, can be quickly grafted onto the side chains of the butadiene chain segments. In addition, the click reaction conditions are mild, the product is easy to purify, and the post-processing is simple.

[0148] The molar ratio of polybutadiene and / or polystyrene butadiene copolymer to the functional molecule can be adjusted according to actual needs. According to some embodiments of the present application, the molar ratio of polybutadiene and / or polystyrene butadiene copolymer to the functional molecule is greater than or equal to 2:1 and less than or equal to 3:1.

[0149] If the molar ratio of polybutadiene and / or polystyrene butadiene copolymer to the functional molecule is too small, for example, less than 2:1, it is easy to cause too many functional side groups, resulting in too low flexibility of the binder; if the molar ratio of polybutadiene and / or polystyrene butadiene copolymer to the functional molecule is too large, for example, greater than 3:1, there are too few functional side groups, the fluorescence effect is not obvious, and the mechanical properties of the binder are low. Therefore, when the molar ratio of polybutadiene and / or polystyrene butadiene copolymer to the functional molecule is greater than or equal to 2:1 and less than or equal to 3:1, the adhesive has better adhesion, flexibility and mechanical properties, and the fluorescence effect is obvious.

[0150] According to some embodiments of the present application, the solvent includes at least one of chloroform, cyclohexane and benzene.

[0151] Chloroform, cyclohexane and benzene all have relatively good solubility, and functional molecules, polybutadiene, and polystyrene butadiene copolymers can all be quickly dissolved in the above solvents, and the cost of the above solvents is relatively low.

[0152] According to some embodiments of the present application, the precipitant includes at least one of methanol, water, and acetone.

[0153] The precipitant can quickly form a precipitate with the reaction product of the functional molecule and the polybutadiene and / or polystyrene butadiene copolymer, and then extract the reaction product.

[0154] According to some embodiments of the present application, after the reaction product of the extraction reaction is extracted by adding a precipitant, the extracted reaction product is further freeze-dried.

[0155] The freeze drying temperature and time can be selected according to actual needs. In some optional embodiments, the freeze drying temperature is greater than or equal to -40°C, and the freezing time does not exceed 24 hours.

[0156] Freeze drying can remove the solvent quickly with little effect on the properties of the reaction product.

[0157] According to some embodiments of the present application, the present application provides a negative electrode plate, comprising a binder as described in any one of the embodiments above or a binder prepared by a method for preparing a binder as described in any one of the embodiments above.

[0158] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one side of the negative electrode current collector. The negative electrode film layer is formed by coating the negative electrode slurry on at least one side of the negative electrode current collector and drying it. The negative electrode slurry includes at least a negative electrode active material and a binder as described in any of the above embodiments or a binder prepared by the method for preparing the binder as described in any of the above embodiments.

[0159] In some embodiments, the negative electrode current collector may be a negative electrode current collector for a secondary battery known in the art, for example, copper foil, aluminum foil, etc.

[0160] In some embodiments, the negative electrode active material may adopt the negative electrode active material for secondary batteries known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0161] In some embodiments, the negative electrode slurry may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0162] In some embodiments, the negative electrode slurry may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0163] In some embodiments, the negative electrode slurry may further include a solvent, such as deionized water.

[0164] In some optional embodiments, the mass percentage of the binder in the negative electrode slurry is 1 wt%-3 wt%.

[0165] As an example, the mass percentage of the binder in the negative electrode slurry can be 1%wt, 1.2%wt, 1.5%wt, 2.0%wt, 2.3%wt, 2.6%wt, 3%wt, etc., or it can be 1%-1.2%wt, 1.2%wt-1.5%wt, 1.5%wt-2.0%wt, 2.0%wt-2.3%wt, 2.3%wt-2.6%wt, 2.6%wt-3%wt. It can be selected according to actual needs as long as the mass percentage of the binder in the negative electrode slurry is 1%wt-3%wt.

[0166] If the mass percentage of the binder in the negative electrode slurry is too small, for example, less than 1%wt, the bonding effect is poor, and if the mass percentage of the binder in the negative electrode slurry is too large, for example, greater than 3%wt, the conductive properties of the negative electrode sheet are greatly affected. In the embodiment of the present application, by controlling the mass percentage of the binder in the negative electrode slurry to 1%wt-3%wt, a good bonding effect can be achieved, and the conductive properties of the negative electrode sheet are less affected.

[0167] According to some embodiments of the present application, the present application provides a secondary battery, including a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet, and the negative electrode sheet is the negative electrode sheet of any of the embodiments described above. The secondary battery may be the battery 100 or the battery cell 20 described above.

[0168] According to some embodiments of the present application, the present application provides an electrical device, including a secondary battery provided by any of the embodiments described above, and the secondary battery is used to provide electrical energy to the electrical device.

[0169] The power-consuming device may be any of the aforementioned devices or systems using secondary batteries.

[0170] The preparation process and test data are introduced as follows:

[0171] Embodiment 1:

[0172] Preparation of binder:

[0173] Cis-1,4-polybutadiene with a number average molecular weight of 150,000 was mixed with functional molecules Add toluene solvent at a molar ratio of 2:1 and stir thoroughly to obtain a mixed solution;

[0174] The mixture was irradiated under UV light for 8 hours. Reacts with cis-1,4-polybutadiene;

[0175] Methanol is added as a precipitant to extract the reaction product of the above reaction to obtain a binder.

[0176] Preparation of negative electrode sheet:

[0177] 2%wt of the binder of Example 1, 95wt% of the negative electrode active material (micron silicon), 1.0wt% of the conductive agent (conductive carbon black), and 2.0wt% of the thickener (sodium carboxymethyl cellulose (CMC)) were mixed, deionized water was added, stirred, and dispersed to form a negative electrode slurry. Then, the negative electrode slurry was coated on the Cu foil, and after both sides were completed, it was dried, cold pressed, cut, and sliced ​​to prepare a negative electrode sheet.

[0178] Preparation of positive electrode:

[0179] 96wt% of positive electrode active material (lithium iron phosphate), 1.0wt% of conductive agent (conductive carbon black), 2.5wt% of binder (polyvinylidene fluoride), and 0.5wt% of dispersant are mixed, and then N-methylpyrrolidone is added, stirred, and dispersed to prepare positive electrode slurry. Double-sided coating, drying, cold pressing, slitting, and preparation of positive electrode sheets are performed.

[0180] Preparation of lithium-ion batteries:

[0181] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is placed between the positive and negative electrode sheets to play an isolating role. The bare battery cell is placed in an outer package, the prepared electrolyte is injected, and the steps of packaging, liquid injection, formation, exhaust, etc. are carried out to obtain a lithium-ion battery.

[0182] Embodiment 2:

[0183] This embodiment 2 is basically the same as embodiment 1, except that the functional molecule is

[0184] Embodiment 3:

[0185] This embodiment 3 is basically the same as embodiment 1, except that the functional molecule is

[0186] Embodiment 4:

[0187] This embodiment 4 is basically the same as embodiment 1, except that the polymer involved in the blending is a polystyrene butadiene copolymer (SBR) with a number average molecular weight of 150,000, wherein the molar ratio of the double bonds in the main chain of the SBR to the side phenyl groups is 2:1; and the polystyrene butadiene copolymer and the functional molecule The mixture was added to the solvent toluene at a molar ratio of 3:1 and stirred thoroughly to obtain a mixed solution.

[0188] Embodiment 5:

[0189] This embodiment 5 is basically the same as embodiment 4, except that the functional molecule is Polystyrene butadiene copolymer The mixture was added to the solvent toluene at a molar ratio of 3:1 and stirred thoroughly to obtain a mixed solution.

[0190] Embodiment 6:

[0191] This embodiment 5 is basically the same as embodiment 4, except that the functional molecule is Polystyrene butadiene copolymer The mixture was added to the solvent toluene at a molar ratio of 3:1 and stirred thoroughly to obtain a mixed solution.

[0192] Embodiment 7:

[0193] This Example 7 is basically the same as Example 1, except that the polymers involved in the blending are polystyrene butadiene copolymer (SBR) with a number average molecular weight of 150,000 and cis-1,4-polybutadiene with a number average molecular weight of 150,000, and SBR and cis-1,4-polybutadiene are fully mixed in a molar ratio of 1:1 to prepare a mixed polymer, wherein the molar ratio of the double bonds in the main chain of SBR to the side phenyl groups is 2:1. The mixed polymer is prepared according to the functional molecule The mixture was added into toluene solvent in a molar ratio of 3:1 and stirred thoroughly to obtain a mixed solution.

[0194] Embodiment 8:

[0195] This embodiment 8 is basically the same as embodiment 1, except that the preparation method of the binder is different. and 1,3-butadiene are uniformly mixed in toluene at a molar ratio of 1:1, and alkyl lithium is used as an initiator to cause copolymerization to produce a copolymer with a number average molecular weight of 150,000. Methanol is added as a precipitant to extract the reaction product of the above reaction to obtain a binder.

[0196] Embodiment 9:

[0197] This embodiment 9 is basically the same as embodiment 1, except that the preparation method of the binder is different. The mixture is added to the solvent toluene at a molar ratio of 2:1 and stirred thoroughly to obtain a mixed solution; under the catalysis of the acid, the hydroxyl groups on the functional molecules react with the double bonds on the polymer main chain.

[0198] Methanol is added as a precipitant to extract the reaction product of the above reaction to obtain a binder.

[0199] Comparative Example 1:

[0200] The only difference from Example 4 is that the binder is not modified with functional side groups, and the binder used is a polystyrene butadiene copolymer (SBR) with a number average molecular weight of 150,000, in which the molar ratio of double bonds in the main chain to the side group phenyl is 2:1.

[0201] Comparative Example 2:

[0202] The only difference from Example 1 is that the binder is not modified with functional side groups, and the binder is cis-1,4-polybutadiene with a number average molecular weight of 150,000.

[0203] Comparative Example 3:

[0204] The only difference from Example 7 is that the binder is not modified with functional side groups, and the binder is prepared by fully mixing a polystyrene butadiene copolymer (SBR) with a number average molecular weight of 150,000 and a cis-1,4-polybutadiene with a number average molecular weight of 150,000 in a molar ratio of 1:1, wherein the molar ratio of the double bonds in the SBR main chain to the side group phenyl is 2:1.

[0205] The negative electrode sheets and lithium ion batteries using the binders of Examples 1-9 and Comparative Examples 1-3 were subjected to a sheet peel strength test, a binder distribution characterization test, and a cycle stability test. The test methods are as follows:

[0206] Negative electrode peel strength test:

[0207] Equipment model: AG-X electronic universal material testing machine (made in Japan), specific test process: cut the negative electrode sheet into 25mm×100mm samples, fix the side of the sample coated with negative electrode slurry on the stainless steel plate of the peel strength tester with double-sided tape, fix one end of the peeled sample on the tensile probe, and perform 180° peeling at a constant speed of 300mm / min to test the peeling force during the peeling process.

[0208] Binder distribution characterization test:

[0209] The negative electrode sheets prepared in Examples 1-9 and Comparative Examples 1-3 were placed in a dark room and irradiated with a portable ultraviolet analyzer (Spectroline UV lamp EA-1610), and the distribution of the binder on the surface of the negative electrode sheets could be observed with the naked eye.

[0210] Cyclic stability test:

[0211] The lithium-ion battery was allowed to stand at 25°C for 30 minutes; charged at 0.05C constant current to 3.65V; allowed to stand at 25°C for 10 minutes; discharged at 0.33C constant current to 2.5V, and discharged at 0.05C constant current to 2.5V; charged at 25°C at 0.1C constant current to 3.65V; allowed to stand at 25°C for 10 minutes; discharged at 25°C at 0.1C constant current to 2.5V; allowed to stand at 25°C for 10 minutes; repeated the above charge and discharge steps until the capacity value reached 80% of the initial value and the test was terminated.

[0212] Table 1: Negative electrode sheets and lithium-ion battery performance parameters of Examples 1-9 and Comparative Examples 1-3

[0213]

[0214]

[0215] From the comparison of the results of Examples 1-9 and Comparative Examples 1-3 in Table 1, it can be seen that the binders modified by functional side groups in the examples of the present application can characterize the distribution of the binder on the surface of the negative electrode sheet, while the binders not modified by functional side groups cannot characterize the distribution of the binder on the surface of the negative electrode sheet. Moreover, compared with the binding properties and the cycle stability of the binders of Examples 1-9, the binding properties and the cycle stability of the lithium ion battery of the binders of Comparative Examples 1-3 are relatively poor.

[0216] Comparison of the results of Examples 1-3, 9 with those of Comparative Example 2 shows that by introducing functional side groups into the main chain of cis-1,4-polybutadiene, not only the bonding strength of the cis-1,4-polybutadiene binder and the cycle stability of the lithium-ion battery using the binder can be improved; but also by introducing fluorescent groups into the binder, it becomes possible to characterize the distribution of the binder.

[0217] Comparison of the results of Examples 4-6 with those of Comparative Example 1 shows that by grafting functional side groups on the main chain of the polystyrene butadiene copolymer, not only can the bonding strength of the polystyrene butadiene copolymer binder and the cycle stability of the lithium-ion battery using the binder be improved; it is also possible to characterize the distribution of the binder by introducing fluorescent groups into the binder.

[0218] Comparison of the results of Example 7 with those of Comparative Example 3 indicates that by grafting functional side groups onto the main chain of the copolymer formed by cis-1,4-polybutadiene and polystyrene butadiene copolymer, not only can the bonding strength of the copolymer binder and the cycle stability of the lithium-ion battery using the binder be improved; it is also possible to characterize the distribution of the binder by introducing fluorescent groups into the binder.

[0219] By comparing the results of Examples 1-3 and 4-6, it can be seen that when the functional molecule is When the binder has the largest bonding force, the lithium-ion battery using the binder has the best cycle stability.

[0220] In the technical solution of the embodiment of the present application, by grafting at least one functional side group with a fluorescent effect on the main chain of the butadiene repeating unit, the distribution of the negative electrode binder in the negative electrode plate can be directly characterized in situ by a fluorescent microscope, whether the negative electrode binder floats, and other phenomena, and then the secondary battery failure analysis can be performed. Moreover, the functional side group of the binder in the embodiment of the present application includes a large π bond, which can produce a π-π conjugation effect with negative electrode materials such as graphite negative electrode and silicon-based negative electrode, increase the interaction between the negative electrode binder and the negative electrode material, and improve the bonding force of the negative electrode binder; and it can also improve the dispersion performance of negative electrode materials such as graphite negative electrode and silicon-based negative electrode, so that the dispersion of negative electrode materials in the negative electrode plate is more uniform, thereby improving the cycle stability of lithium-ion batteries.

[0221] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A binder, It is characterized in that The invention comprises modified polybutadiene and / or modified polystyrene butadiene copolymer, wherein the main chain of the modified polybutadiene comprises butadiene repeating units and modified butadiene repeating units; the main chain of the modified polystyrene butadiene copolymer comprises styrene repeating units, butadiene repeating units and modified butadiene repeating units, wherein at least one functional side group is grafted on the main chain of butadiene, and the functional side group has a fluorescent effect.

2. The adhesive according to claim 1, It is characterized in that The functional side groups include large π bonds.

3. The adhesive according to claim 1 or 2, It is characterized in that The functional side groups include at least one of condensed ring aromatic hydrocarbon free radicals, condensed ring aromatic hydrocarbon derivative free radicals, naphthalene diimide free radicals, naphthalene diimide derivative free radicals, triphenylamine free radicals, or triphenylamine derivative free radicals.

4. The adhesive according to any one of claims 1 to 3, It is characterized in that The functional side groups include At least one of the free radicals.

5. The adhesive according to any one of claims 1 to 4, It is characterized in that The functional side groups are formed by functional molecules, which include thiol groups, the sulfur atoms in which are connected to the carbon atoms in the modified butadiene repeating units, and the hydrogen atoms in which are replaced.

6. The adhesive according to claim 5, It is characterized in that The general formula of the functional side group is: R includes at least one of alkyl groups, and R' includes at least one of condensed aromatic hydrocarbon radicals, condensed aromatic hydrocarbon derivative radicals, naphthalene dicarboximide radicals, naphthalene dicarboximide derivative radicals, triphenylamine radicals, or triphenylamine derivative radicals.

7. The adhesive according to claim 6, It is characterized in that The R includes x is greater than or equal to 1 and less than or equal to 9.

8. The adhesive according to claim 6 or 7, It is characterized in that The R' includes At least one of the free radicals.

9. The binder according to any one of claims 1 to 8, It is characterized in that The modified polystyrene butadiene copolymer is a block copolymer or a random copolymer.

10. The binder according to any one of claims 1 to 9, It is characterized in that The number average molecular weight of the modified polybutadiene is 10,000-1,000,000, and the number average molecular weight of the modified polystyrene butadiene copolymer is 10,000-1,000,000.

11. The binder according to any one of claims 1 to 10, It is characterized in that The modified polybutadiene includes modified cis-1,4-polybutadiene.

12. A method for preparing the binder according to any one of claims 1 to 11, It is characterized in that include: Mixing a functional molecule with polybutadiene and / or polystyrene butadiene copolymer, wherein the functional molecule reacts with the polybutadiene and / or the polystyrene butadiene copolymer, and the functional molecule is grafted onto the main chain of the butadiene repeating unit in the polybutadiene and / or the polystyrene butadiene copolymer to form the functional side group; The reaction product of the above reaction is extracted to obtain the binder.

13. The method for preparing the adhesive according to claim 12, It is characterized in that include: Adding the functional molecule and the polybutadiene and / or the polystyrene butadiene copolymer into a solvent and mixing them to obtain a mixed solution; Performing photoinitiation or thermal initiation on the mixed solution so that the functional molecule reacts with the polybutadiene and / or the polystyrene butadiene copolymer; A precipitant is added to extract the reaction product of the above reaction to obtain a binder.

14. A method for preparing the adhesive according to claim 12 or 13, It is characterized in that The functional molecule includes a thiol group, and the thiol group undergoes a click reaction with the polybutadiene and / or the polystyrene butadiene copolymer.

15. A method for preparing a binder according to any one of claims 12 to 14, It is characterized in that The molar ratio of the polybutadiene and / or the polystyrene butadiene copolymer to the functional molecule is greater than or equal to 2:1 and less than or equal to 3:

1.

16. A method for preparing the binder according to any one of claims 13 to 15, It is characterized in that The solvent includes at least one of chloroform, cyclohexane and benzene.

17. A method for preparing a binder according to any one of claims 13 to 16, It is characterized in that The precipitant includes at least one of methanol, water and acetone.

18. A method for preparing the adhesive according to any one of claims 12 to 17, It is characterized in that After the reaction product of the above reaction is extracted, the extracted reaction product is further freeze-dried.

19. A negative electrode sheet, It is characterized in that The invention comprises an adhesive as described in any one of claims 1 to 11 or an adhesive prepared by the method for preparing the adhesive as described in any one of claims 12 to 18.

20. A secondary battery, It is characterized in that Comprising the negative electrode sheet as described in claim 19.

21. An electrical device, It is characterized in that Comprising the secondary battery as claimed in claim 20.

Citation Information

Patent Citations

  • Method for modifying styrene-butadiene-styrene (SBS) block copolymer

    CN102391424A

  • Silicon-containing polythioether fluorescent probe and application thereof

    CN110527090A

  • Binder with high ionic conductivity and lithium ion battery containing binder

    CN111900393A

  • Double-molecular-weight-distribution binder for negative electrode and preparation method and application thereof

    CN112375179A

  • Fluorescent functional monomer, pressure-sensitive adhesive enabling timely detection of coating defects and preparation method of pressure-sensitive adhesive

    CN113735772A