Flame-retardant elastic material for bridge expansion joints as well as preparation method and application of flame-retardant elastic material

By using phosphorus and nitrogen-functionalized lignin nanoparticles and prepolymers in bridge expansion joint materials, the flame retardant performance and mechanical properties of the material are improved, and the problems of insufficient flammability and flame retardant performance of traditional materials are solved. Safety and durability requirements for bridge expansion joints.

CN119019633APending Publication Date: 2024-11-26山东高速工程检测有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411117675.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional bridge expansion joint materials are prone to damage under temperature changes and loads, and the flammability and flame retardant properties of polymer elastomer materials are insufficient, making it difficult to meet the requirements of bridge safety and durability.

Method used

The lignin nanoparticles functionalized by phosphorus and nitrogen are mixed with the prepolymer, and the flame-retardant elastic material for bridge expansion joints is obtained through ultrasonic treatment and centrifugation separation, improving the flame-retardant and mechanical properties of the material.

Benefits of technology

It realizes excellent flame retardant performance of bridge expansion joint materials, solves the problem of reduced elongation and tensile strength caused by the addition of flame retardant from polymer elastic materials, and is suitable for elastomer filled seamless expansion joints in various structural forms. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019633A_ABST
    Figure CN119019633A_ABST
Patent Text Reader

Abstract

The invention provides a flame-retardant elastic material for a bridge expansion joint as well as a preparation method and application of the flame-retardant elastic material. The preparation method of the flame-retardant elastic material for the bridge expansion joint comprises the step of mixing and reacting the phosphorus and nitrogen functionalized lignin nanoparticles and a prepolymer to obtain the flame-retardant elastic material for the bridge expansion joint. The flame-retardant elastic material for the bridge expansion joint prepared by the preparation method has excellent flame retardance while meeting the use requirements of the bridge expansion joint, solves the problems that the elongation and tensile strength of a high-molecular elastic material are reduced due to the addition of a flame retardant and the fireproof grade of an elastomer filled seamless expansion joint is low, and is suitable for large-scale popularization and application. The method is suitable for elastomer filling type seamless expansion joints of various structural forms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bridge construction, and in particular to a flame retardant elastic material for bridge expansion joints, a preparation method and application thereof. Background Art

[0002] As an important transportation infrastructure, the stability and durability of bridges are crucial to traffic safety. As a key part of bridge engineering, expansion joints are responsible for adjusting the deformation of bridges caused by temperature changes, loads, etc. However, expansion joints are also the most vulnerable part of bridges, and their performance is directly related to the performance and life of the bridge.

[0003] Traditional expansion joints are usually designed with materials such as metal or rubber, but these materials have some limitations. For example, metal expansion joints are prone to noise under temperature changes and have high maintenance costs; although rubber expansion joints have a certain degree of elasticity, their weather resistance and fatigue resistance are relatively poor, and they are prone to aging at high temperatures and hardening at low temperatures, affecting the normal use of bridges.

[0004] In order to improve the performance of expansion joints, seamless expansion joint technology has been developed in recent years. This technology uses polymer elastomer materials to fill expansion joints in order to better adapt to bridge deformation and improve driving comfort. However, this polymer elastomer material generally has flammability problems. Once a fire occurs, it will seriously threaten the safety of bridge structures and driving safety.

[0005] In addition, in order to improve the flame retardant properties of elastomers, flame retardants are usually added. However, too much flame retardant will reduce the mechanical properties of the material, such as elongation and tensile strength, while insufficient addition of flame retardant will lead to poor flame retardant effect and it is difficult to achieve the expected fire protection level.

[0006] Therefore, in order to obtain an elastomeric material having both high elongation and high tensile strength and excellent flame retardant properties to meet the application requirements of seamless expansion joints of bridges and ensure their safety and reliability under various environmental conditions, the present application provides a flame retardant elastic material for bridge expansion joints, and a preparation method and application thereof. Summary of the invention

[0007] In view of the defects and deficiencies of polymer elastic materials used to fill seamless expansion joints in the prior art, the present application provides a flame-retardant elastic material for bridge expansion joints and a preparation method and application thereof. The flame-retardant elastic material prepared by the preparation method of the flame-retardant elastic material for bridge expansion joints has excellent flame retardant properties while meeting the use requirements of bridge expansion joints, solves the problems of reduced elongation and tensile strength of polymer elastic materials due to the addition of flame retardants, and low fire resistance of elastomer-filled seamless expansion joints, and is suitable for elastomer-filled seamless expansion joints of various structural forms.

[0008] One embodiment of the present application provides a method for preparing a flame retardant elastic material for a bridge expansion joint, comprising the steps of mixing phosphorus and nitrogen functionalized lignin nanoparticles with a prepolymer and reacting the mixture to obtain the flame retardant elastic material for a bridge expansion joint;

[0009] The prepolymer is obtained by adding isocyanate, polyol and catalyst into N,N-dimethylformamide solvent and reacting.

[0010] Preferably, the preparation of the phosphorus and nitrogen functionalized lignin nanoparticles comprises the following steps:

[0011] (1) treating acetic acid lignin powder to obtain purified lignin;

[0012] (2) dissolving the purified lignin obtained in step (1) in an alkaline solution, adding formaldehyde and polyethyleneimine, adjusting the pH value to acidic after the reaction, washing the precipitate with deionized water to neutrality, and drying to obtain nitrogen-containing lignin;

[0013] (3) adding the nitrogen-containing lignin, formaldehyde and phosphorus-based flame retardant obtained in step (2) to an N,N-dimethylformamide solvent, adjusting the pH value to acidic, and obtaining phosphorus- and nitrogen-functionalized lignin after reaction;

[0014] (4) dissolving the phosphorus- and nitrogen-functionalized lignin obtained in step (3) in an N,N-dimethylformamide solvent, slowly dripping deionized water into the solvent while performing ultrasonic treatment, and obtaining the phosphorus- and nitrogen-functionalized lignin nanoparticles after centrifugal separation.

[0015] In step (2), the purified lignin undergoes a condensation reaction with formaldehyde; the aldehyde group in the formaldehyde undergoes an addition reaction with the amino group of polyethyleneimine; and finally the polyethyleneimine is successfully grafted onto the lignin molecule.

[0016] In step (3), formaldehyde first reacts with the primary amino group and the secondary amino group of the polyethyleneimine molecule; and then reacts with the active PH group in the phosphorus-based flame retardant to obtain phosphorus- and nitrogen-functionalized lignin.

[0017] Preferably, step (1) specifically includes:

[0018] The acetic acid lignin powder is mixed with the acetic acid solution, stirred evenly, and then filtered using a sand core funnel, and the filtrate is retained;

[0019] The filtrate and deionized water are mixed and stirred evenly, and allowed to stand to collect the precipitate, wherein the temperature of the deionized water is between 60° C. and 90° C.;

[0020] The precipitate is stirred and washed with deionized water until the pH value is neutral, and then dried to obtain the purified lignin;

[0021] Wherein, the concentration of the acetic acid solution is between 80wt% and 95wt%.

[0022] In step (1), acetic acid lignin can be purchased commercially. Since acetic acid lignin powder contains some impurities and acetic acid lignin powder can be dissolved in acetic acid solution, the solid impurities contained in the acetic acid lignin powder can be removed by washing with acetic acid solution, and then the pH value is adjusted to neutral by washing with deionized water multiple times to completely remove the acetic acid solution to obtain purified lignin.

[0023] Preferably, in step (2), the alkaline solution is selected from any one of potassium hydroxide, sodium hydroxide, ammonia water, or sodium carbonate;

[0024] The concentration of the alkaline solution is between 6 wt % and 23 wt %.

[0025] Preferably, in both step (2) and step (3), an acidic solution is used to adjust the pH value to 2 to 4;

[0026] The acidic solution is selected from hydrochloric acid or sulfuric acid, and the concentration of the acidic solution is between 40wt% and 70wt%.

[0027] Preferably, in step (3), the phosphorus-based flame retardant is selected from phosphates, phosphites, organic phosphorus salts, phosphorus oxides and phosphorus-nitrogen compounds, 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide and its derivatives.

[0028] Preferably, the isocyanate is selected from any one or more of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate;

[0029] The polyol is selected from any one or more of polytetramethylene glycol, polycaprolactone polyol, polycarbonate polyol, polytetramethyl vinyl ether glycol, and castor oil; the functionality of the polyol is 2 to 3, and the average molecular weight is 400 to 6000;

[0030] The catalyst is selected from any one of triethylenediamine, dimethylethanolamine, N-methylmorpholine, N,N-dimethylcyclohexylamine, stannous octoate, stannous oleate, and dibutyltin dilaurate;

[0031] The ratio of -NCO in the isocyanate to -OH in the polyol is between 1.0 and 1.2.

[0032] According to another embodiment of the present application, a flame-retardant elastic material for bridge expansion joints prepared according to the above-mentioned preparation method of the present application is provided.

[0033] According to another embodiment of the present application, there is provided a flame-retardant elastic material for a bridge expansion joint prepared according to the above-mentioned preparation method of the present application, and application of the above-mentioned flame-retardant elastic material for a bridge expansion joint in an expansion joint structure of a bridge engineering.

[0034] Preferably, the phosphorus and nitrogen functionalized lignin nanoparticles are stirred with the prepolymer and then poured into a prefabricated mold, and then demoulded to form a prefabricated board;

[0035] The prefabricated mold comprises a mold body, a mold cavity arranged in the mold body, and a heating rod arranged in the mold body, wherein the heating rod is reciprocatingly bent and arranged in the mold body; a steel section member is arranged in the mold cavity; after the phosphorus and nitrogen functionalized lignin nanoparticles are stirred and poured into the mold cavity of the prefabricated mold with the prepolymer, the prefabricated mold is placed in a vacuum oven, the heating rod is turned on to ensure that the temperature in the vacuum oven is consistent with the temperature of the heating rod, and after curing and demoulding, the prefabricated board is obtained; the prefabricated board comprises a flame-retardant elastic material for bridge expansion joints and the steel section member.

[0036] Preferably, the steel member is pre-tensioned before pouring the phosphorus and nitrogen functionalized lignin nanoparticles and the prepolymer into the mold cavity of the prefabricated mold.

[0037] Preferably, when the steel member is pre-tensioned, corresponding to different types of expansion joints, the corresponding relationship between the tensioning force and the tensioning amount of the steel member is as follows:

[0038] F x =ω·b x

[0039] Among them, F x is the tensile force applied to the steel member, in KN; b x is the tension amount, in cm; ω is the tension parameter;

[0040] Corresponding to different expansion joint models, the value of ω is as follows:

[0041] For the 60-type expansion joint, ω is 1.173;

[0042] For the 80 model expansion joint, ω is 0.980;

[0043] For the 100 model expansion joint, ω is 0.856;

[0044] For the 120 model expansion joint, ω is 0.702;

[0045] For the 160 model expansion joint, ω is 0.484.

[0046] Preferably, the heating rod is arranged in an "S" shape in the mold body.

[0047] Preferably, the prefabricated panels are installed at the bridge connection, and the installation method comprises the following steps:

[0048] Cleaning bridge expansion joint notches;

[0049] pouring anchor concrete;

[0050] Install precast panels;

[0051] Pour the sealing layer.

[0052] Preferably, before installing the prefabricated panels, the prefabricated panels are pre-tensioned according to the installation temperature and the length of the bridge. For expansion joints of different types, the corresponding relationship between the tensioning force and the tensioning amount of the prefabricated panels is as follows:

[0053]

[0054] Among them, F y is the tensile force applied to the precast panel, in KN; b y is the tension amount, in cm; λ and A are tension parameters;

[0055] Corresponding to different expansion joint models, the values ​​of λ and A are as follows:

[0056] For the 60 model expansion joint, λ is 14.5 and A is 3;

[0057] For the 80 model expansion joint, λ is 12 and A is 5.5;

[0058] For the 100 type expansion joint, λ is 10 and A is 13;

[0059] For the 120 model expansion joint, λ is 8.5 and A is 14.5;

[0060] For the 160 model expansion joint, λ is 7 and A is 17.

[0061] As described above, the flame-retardant elastic material for bridge expansion joints of the present application and its preparation method and application have the following beneficial effects:

[0062] The flame-retardant elastic material for bridge expansion joints prepared by the preparation method provided in the present application has excellent flame retardant properties while meeting the use requirements of bridge expansion joints, solves the problems of reduced elongation and tensile strength of polymer elastic materials due to the addition of flame retardants, and low fire resistance level of elastomer-filled seamless expansion joints, and is suitable for elastomer-filled seamless expansion joints of various structural forms. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1Shown is a tensile stress-strain curve of the flame-retardant elastic material for bridge expansion joints provided in Example 2 of the present application.

[0064] Figure 2 Shown is a schematic cross-sectional structure diagram of the prefabricated mold provided in Example 3 of the present application.

[0065] Figure 3 Shown is a schematic diagram of the top view of the prefabricated mold provided in Example 3 of the present application.

[0066] Figure 4 Shown is a structural schematic diagram of the cleaning of the expansion joint groove in the application method of the precast panel at the bridge connection provided in Example 3 of the present application.

[0067] Figure 5 Shown is a structural schematic diagram of pouring anchoring concrete in the application method of the precast panels provided in Example 3 of the present application at the bridge connection.

[0068] Figure 6 Shown is a structural schematic diagram of installing prefabricated panels in the application method of prefabricated panels at bridge connections provided in Example 3 of the present application.

[0069] Figure 7 Shown is a structural schematic diagram of pouring a sealing layer in the application method of the precast panels provided in Example 3 of the present application at the bridge connection.

[0070] Component number description

[0071] 10, mold body; 20, mold cavity; 30, heating rod; 40, steel structure. DETAILED DESCRIPTION

[0072] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0073] The raw materials, reagents, solvents, etc. used in the examples are all commercially available.

[0074] In bridge engineering, expansion joints are important structures that connect various sections of a bridge. Their performance is directly related to the overall safety and service life of the bridge. With the continuous increase in traffic volume and the increasing weight of vehicle loads, bridge expansion joints are facing more severe challenges. Although traditional expansion joint structures, such as seamless expansion joints, can adapt to the deformation requirements of bridges to a certain extent, their installation and maintenance are complicated, and problems such as poor driving comfort and high noise are gradually becoming prominent.

[0075] What is particularly critical is that during long-term use, bridge expansion joints not only need to withstand repeated impact loads from vehicles and the isotropic deformation of the bridge itself due to temperature changes, but also need to have good waterproof, weather-resistant and fatigue-resistant properties. These requirements make the selection of expansion joint materials particularly important. However, the currently commonly used polymer elastomer filling materials, although they have certain flexibility and weather resistance, their flammability has become a bottleneck restricting their widespread application.

[0076] The flammability of polymer elastomer materials not only threatens the safe use of bridges, but also may spread rapidly when a fire occurs, increasing the difficulty of rescue and property losses. Therefore, improving the flame retardant properties of elastic materials used in bridge expansion joints has become a technical problem that needs to be solved urgently.

[0077] However, there is a significant contradiction in the process of adding flame retardants: adding more flame retardants will significantly reduce the elongation and tensile strength of the elastomer, affecting the deformation absorption capacity and overall stability of the expansion joint; while adding less flame retardants may cause the flame retardant to be unevenly dispersed in the elastomer, unable to effectively play a flame retardant role, which greatly reduces the flame retardant effect.

[0078] In view of the above defects, the present application provides a flame retardant elastic material for bridge expansion joints and a preparation method and application thereof, which are now described in detail through the following embodiments.

[0079] Embodiment 1

[0080] This embodiment provides a method for preparing a flame retardant elastic material for a bridge expansion joint, comprising the following steps:

[0081] S1. Mix acetic acid lignin powder with acetic acid solution, stir evenly, and filter the solution with a sand core funnel to remove solid impurities; stir the filtered filtrate and deionized water evenly, and let it stand for more than 6 hours to collect the precipitate; repeatedly use deionized water to stir and wash the precipitate until the pH value is neutral; dry the washed precipitate to obtain purified lignin.

[0082] S2, dissolving the purified lignin obtained in step S1 into an alkaline solution, adding formaldehyde and polyethyleneimine, heating to 50°C, and reacting for a period of time; adjusting the pH value of the solution after the reaction to acidic with an acidic solution; washing the precipitate with deionized water to neutrality; and obtaining nitrogen-containing lignin after drying.

[0083] S3. Add the nitrogen-containing lignin, formaldehyde and phosphorus-based flame retardant obtained in step S2 to N,N-dimethylformamide (DMF) solvent, adjust the pH value of the mixed solution to acidic with an acidic solution, and stir at 80° C. for 5 hours; remove the DMF solvent and repeatedly wash with deionized water; and obtain phosphorus- and nitrogen-functionalized lignin (PNL) after drying.

[0084] S4, dissolving the phosphorus and nitrogen functionalized lignin (PNL) obtained in step S3 in N,N-dimethylformamide (DMF) solvent; slowly dripping deionized water while ultrasonically treating; and obtaining phosphorus and nitrogen functionalized lignin nanoparticles (Nano-PNL) by centrifugal separation.

[0085] S5. Add isocyanate, polyol and catalyst into N,N-dimethylformamide (DMF) solvent, and react at 80° C. for 5 hours to obtain a prepolymer; dissolve the phosphorus and nitrogen functionalized lignin nanoparticles (Nano-PNL) obtained in step S4 and add them to the prepolymer, and after reaction, obtain a flame retardant elastic material for bridge expansion joints.

[0086] In step S2, lignin undergoes a condensation reaction with formaldehyde, and then the aldehyde group in the formaldehyde undergoes an addition reaction with the amino group of polyethyleneimine, and finally the polyethyleneimine is successfully grafted onto the lignin molecule.

[0087] In step S3, formaldehyde first reacts with the primary amino group and the secondary amino group of the polyethyleneimine molecule, and then reacts with the PH group in the phosphorus-based flame retardant to finally obtain phosphorus- and nitrogen-functionalized lignin.

[0088] In step S4, phosphorus and nitrogen functionalized lignin nanoparticles are obtained through solvent exchange reaction and ultrasonic reaction treatment. The phosphorus and nitrogen functionalized lignin nanoparticles have good solubility and promote more hydrogen bond formation and chemical cross-linking. These intermolecular interactions help to improve the tensile strength and elongation of the flame retardant elastic material, and further enhance the dispersibility and compatibility of the flame retardant in the flame retardant elastic material matrix, overcoming the weakening effect of traditional flame retardant addition on the mechanical properties of the flame retardant elastic material.

[0089] In an optional embodiment, in step S1, the concentration of the acetic acid solution is between 80wt% and 95wt%. Specifically, the concentration of the acetic acid solution can be, for example, 80wt%, 81wt%, 82wt%, 83wt%, 84wt%, 85wt%, 86wt%, 87wt%, 88wt%, 89wt%, 90wt%, 91wt%, 92wt%, 93wt%, 94wt%, 95wt%, etc. Acetic acid lignin has the same chemical structure as lignin and can be purchased directly. Because there are still some impurities in the acetic acid lignin powder, and the acetic acid lignin powder can be dissolved in the acetic acid solution, the solid impurities are removed by washing with the acetic acid solution. The precipitate is then washed with deionized water for multiple times, and the pH value is adjusted to neutral, the acetic acid solution is completely removed, and the purified lignin is obtained.

[0090] In an optional embodiment, the temperature of the deionized water in step S1 is 60° C. to 90° C. Specifically, the temperature of the deionized water may be, for example, 60° C., 65° C., 70° C., 75° C., 80° C., 85° C., 90° C., etc.

[0091] In an optional embodiment, the alkaline solution in step S2 is selected from any one of potassium hydroxide, sodium hydroxide, ammonia water and sodium carbonate. Optionally, the concentration of the alkaline solution is between 6wt% and 23wt%. Specifically, the concentration of the alkaline solution can be, for example, 6wt%, 8wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, 22wt%, 23wt%, etc.

[0092] In an optional embodiment, the acidic solution in step S2 and step S3 is selected from hydrochloric acid or sulfuric acid. Optionally, the concentration of the sulfuric acid solution is between 40wt% and 70wt%. Specifically, the concentration of the sulfuric acid solution can be, for example, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, etc. Optionally, the pH value is adjusted to 2 to 4 with the acidic solution. Specifically, the pH value can be, for example, 2, 3, 4, etc.

[0093] In an optional embodiment, the phosphorus-based flame retardant in step S3 is selected from any one of phosphates, phosphites, organic phospholipids, phosphorus oxides and phosphorus-nitrogen compounds, 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide and its derivatives.

[0094] In an optional embodiment, the power of the ultrasound in step S4 is above 200W.

[0095] In an optional embodiment, the particle size of the phosphorus and nitrogen functionalized lignin nanoparticles (Nano-PNL) obtained in step S4 is between 200 nm and 600 nm.

[0096] In an optional embodiment, the isocyanate in step S5 is selected from any one of toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), and hexamethylene diisocyanate (HDI).

[0097] In an optional embodiment, the polyol in step S5 is selected from any one or more of polytetramethylene glycol (PTMG), polycaprolactone polyol (PCL), polycarbonate polyol (PCDL), polytetramethyl vinyl ether glycol (PTMEG), and castor oil.

[0098] In an optional embodiment, the functionality of the polyol in step S5 is 2 to 3, and the average molecular weight is between 400 and 6000. Specifically, the functionality of the polyol can be, for example, 2, 3, etc., and the average molecular weight can be, for example, 400, 800, 1000, 1500, 2000, 2500, 3000, 3500, 4000, 4500, 5000, 5500, 6000, etc.

[0099] In an optional embodiment, the ratio of -NCO groups in isocyanate to -OH groups in polyol in step S5 is 1.0 to 1.2. Specifically, the ratio of -NCO groups in isocyanate to -OH groups in polyol can be 1.0, 1.1, 1.2, etc.

[0100] In an optional embodiment, the catalyst in step S5 is selected from any one of triethylenediamine, dimethylethanolamine, N-methylmorpholine, N,N-dimethylcyclohexylamine, stannous octoate, stannous oleate, and dibutyltin dilaurate.

[0101] Embodiment 2

[0102] This embodiment provides a flame retardant elastic material for a bridge expansion joint. The flame retardant elastic material for a bridge expansion joint is prepared by the method provided in Embodiment 1. The preparation method comprises the following steps:

[0103] (1) 50 g of acetic acid lignin powder was mixed with 350 mL of 95 wt% acetic acid solution, and the solution was filtered with a G4 sand core funnel to remove solid impurities after stirring for 2 h; the filtered filtrate was evenly stirred with 80°C deionized water, and the precipitate was collected after standing for 8 h; the precipitate was repeatedly stirred and washed with deionized water until the pH value of the precipitate was neutral; the precipitate was placed in a vacuum oven and dried at 80°C for 12 h to obtain purified lignin.

[0104] (2) Add 20 g of the purified lignin obtained in step (1) to 500 mL of a 22 wt% NaOH solution and stir until completely dissolved; add 4.5 g of formaldehyde and 4 g of polyethyleneimine, heat to 50° C. and keep warm for 6 h after dissolution; adjust the pH value of the solution to 2 with hydrochloric acid after the reaction; then wash the precipitate with deionized water until it is neutral; and dry it in a vacuum at 70° C. for 48 h to obtain nitrogen-containing lignin.

[0105] (3) The nitrogen-containing lignin obtained in step (2), 0.384 mL of formaldehyde and 2 g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) were added to 300 mL of DMF solvent, the pH value was adjusted to 3 with hydrochloric acid, and the mixture was stirred at 80° C. for 5 h; the DMF solvent was removed by a rotary evaporator, and the obtained product was repeatedly washed with deionized water; and the mixture was dried at 70° C. in a vacuum oven for 48 h to obtain phosphorus- and nitrogen-functionalized lignin (PNL).

[0106] The reaction equation of step (3) is as follows:

[0107]

[0108] (4) The lignin (PNL) obtained in step (3) was dissolved in 200 mL of DMF solvent, and 200 mL of deionized water was slowly added dropwise during ultrasonic treatment, and phosphorus- and nitrogen-functionalized lignin nanoparticles (Nano-PNL) were obtained by centrifugal separation.

[0109] (5) Add 21.4 g of hexamethylene diisocyanate (HDI), 100 g of polytetramethylvinyl ether glycol (PTMEG), and 0.25 g of dibutyltin dilaurate (DBTDL) to 300 mL of DMF solvent, and react at 80°C for 5 h to obtain a prepolymer; add 6.39 g of phosphorus and nitrogen functionalized lignin nanoparticles (Nano-PNL) obtained in step (4) to 100 mL of DMF solvent, dissolve, and then add to the prepolymer, react at 85°C for 0.5 h, and then pour into a prefabricated mold; place the prefabricated mold in a vacuum oven, store at 80°C for 24 h, and then demold for testing or use.

[0110] The amount of the phosphorus- and nitrogen-functionalized lignin nanoparticles (Nano-PNL) added is 6% to 18% of the total mass of the polytetramethylethylene ether glycol (PTMEG) and the phosphorus- and nitrogen-functionalized lignin nanoparticles (Nano-PNL). Different flame-retardant elastic materials for bridge expansion joints can be obtained by changing the amount of the phosphorus- and nitrogen-functionalized lignin nanoparticles (Nano-PNL) added.

[0111] According to the preparation method of the above embodiment, a series of flame-retardant elastic materials for bridge expansion joints were prepared, as shown in Table 1.

[0112] Table 1

[0113]

[0114] In Table 1:

[0115] CPU: No flame retardant added;

[0116] PU / 6%L: 6wt% lignin added;

[0117] PU / 6%-PNL: lignin functionalized with 6 wt% phosphorus and nitrogen;

[0118] PU / 6%-Nano-PNL: lignin nanoparticles functionalized with 6 wt% phosphorus and nitrogen;

[0119] PU / 12%-Nano-PNL: lignin nanoparticles functionalized with 12 wt% phosphorus and nitrogen;

[0120] PU / 18%-Nano-PNL: lignin nanoparticles functionalized with 18 wt% phosphorus and nitrogen;

[0121] PU / 6%-DOPO-HQ: 6wt% reactive non-halogen flame retardant DOPO-HQ was added.

[0122] The samples in Table 1 were tested according to GBT528 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber". Type I specimens were selected for the samples and the tensile testing machine was used for the test. The tensile stress-strain curves were as follows: Figure 1 As shown. Figure 1 It can be clearly seen that after adding lignin, phosphorus-nitrogen functionalized lignin, and flame retardant DOPO-HQ, the tensile strength and elongation of the flame retardant elastic material are reduced to varying degrees. This is due to the poor compatibility and weak binding force of lignin molecules and DOPO-HQ in the CPU matrix. The 6wt% addition of phosphorus-nitrogen functionalized lignin nanoparticles (Nano-PNL) avoids the problems of poor uniformity, poor dispersibility and easy agglomeration of lignin. The good compatibility of Nano-PNL with the prepolymer is more conducive to the formation of more hydrogen bonds, enhanced cross-linking network effect, and obvious strain-induced crystallization, thereby improving the tensile properties of polyurethane elastic materials. When the addition amount of Nano-PNL is increased to 18wt%, the tensile strength and elongation of the polyurethane elastomer are significantly reduced. This is because excessive nanoparticles are prone to agglomeration, which increases the structural defects of the CPU matrix, thereby generating stress concentration areas, which have a negative impact on the tensile properties of the material.

[0123] The samples in Table 1 were tested for flame retardancy and tensile mechanical properties, wherein tensile strength and elongation were tested using GBT528 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber"; total heat release, total smoke production, and ignition time were tested according to ISO 5660, using cone calorimetry, and measured using a cone calorimeter; limiting oxygen index was measured using ASTM D2863, using an automatic limited oxygen index tester. The above test results are shown in Table 2.

[0124] Table 2 Flame retardant properties and tensile mechanical properties.

[0125]

[0126] It can be seen from Table 2 that the limiting oxygen index of CPU without any flame retardant material is 19.3%, which is a flammable material; the limiting oxygen index does not change significantly after adding lignin; after adding 12wt% Nano-PNL, the limiting oxygen index increases to 30.2%, and it extinguishes itself after removing the fire source, and the flame retardancy is significantly improved.

[0127] Cone calorimetry showed that the ignition time increased by 12 s after the addition of lignin, and the total heat release and smoke production decreased slightly.

[0128] When Nano-PNL was added, the ignition time was extended by 28s, and the total heat release and smoke production were greatly reduced. Its flame retardant performance is better than that of polyurethane elastic materials directly added with flame retardant DOPO-HQ. The high flame retardant performance of Nano-PNL is mainly due to the synergistic mechanism of phosphorus and nitrogen functional groups, which enhances the formation of thicker carbon layers while reducing thermal conductivity. The dense carbon layer can further prevent the generation and release of smoke and play a role in fire prevention. In addition, Nano-PNL releases ammonia while forming a dense carbon layer, and exerts a flame retardant effect through both condensed phase and gas phase.

[0129] Embodiment 3

[0130] This embodiment provides an application of a flame-retardant elastic material for bridge expansion joints in the expansion joint structure of a bridge project. The phosphorus- and nitrogen-functionalized lignin nanoparticles and prepolymer obtained in Embodiment 1 or Embodiment 2 are stirred and poured into a prefabricated mold, and a prefabricated board is formed after demolding.

[0131] like Figure 2 As shown in FIG. 1 , the prefabricated mold includes a mold body 10, a mold cavity 20 and a heating rod 30. The mold cavity 20 is disposed in the mold body 10. Figure 3 As shown, the heating rod 30 is arranged in the mold body 10, and the heating rod 30 is arranged in a reciprocating bending shape on a certain plane of the mold body 10, for example, in an "S" shape; a certain plane of the mold body 10 is located at the plane with the largest contact surface for realizing the heat transfer from the heating rod 30 to the mold cavity 20. A steel member 40 is arranged in the mold cavity 20. The steel member 40 is placed in the mold cavity 20. After the flame-retardant elastic material for bridge expansion joints is poured into the mold cavity 20, it is demolded together with the steel member 40 to form a prefabricated board. Therefore, the prefabricated board includes the flame-retardant elastic material for bridge expansion joints and the steel member 40. Figure 2 As shown, the cross-section of the steel member 40 is a plurality of trapezoidal structures or a plurality of corrugated structures arranged at intervals. Due to the different thermal conductivity rates of the castable and the steel member 40, there is a certain temperature difference between the inside and outside during the curing process of the material, and there will be a certain shrinkage deformation after curing, which will cause the material to peel off from the steel member 40; after the heating rod 30 is set, the uniformity of the internal and external temperatures is effectively ensured, and the shrinkage deformation of the material after curing is greatly reduced while the reaction rate is increased, ensuring that the flame-retardant elastic material and the steel member 40 can be firmly combined, thereby improving the preparation quality of the prefabricated board. By presetting the heating rod 30 in the prefabricated mold, the curing time of the castable is effectively reduced, and the problem of tearing and peeling from the steel member 40 caused by the curing shrinkage of the material is greatly reduced, thereby improving the quality of the prefabricated board.

[0132] In an optional embodiment, the specific steps of forming the prefabricated panel include:

[0133] The steel member 40 is arranged in advance in the mold cavity 20;

[0134] The phosphorus and nitrogen functionalized lignin nanoparticles are dispersed in N,N-dimethylformamide (DMF), the prepolymer is added, and the mixture is reacted at 85°C for 0.5h before being poured into the mold cavity 20;

[0135] The prefabricated mold is placed in a vacuum oven, and the heating rod 30 is turned on at the same time to ensure that the temperature in the vacuum oven and the temperature of the heating rod are both maintained at 80° C. The prefabricated plate is obtained after curing for more than 10 hours and demoulding.

[0136] In an optional embodiment, before pouring the phosphorus and nitrogen functionalized lignin nanoparticles and prepolymer into the mold cavity 20, the steel member 40 is pre-stressed to ensure that the steel member 40 is in a slightly compressed state after casting, to ensure that the steel member 40 and the flame-retardant elastic material for the bridge expansion joint can be effectively combined, to ensure that the precast panel is cast densely, and to improve the quality of the precast panel.

[0137] In the optional embodiment, corresponding to different types of expansion joints, the corresponding relationship between the tensioning force and the tensioning amount of the steel member 40 is as follows:

[0138] F x =ω·b x

[0139] Among them, F x is the tensile force applied to the steel member, in KN; b x is the tension amount, in cm; ω is the tension parameter;

[0140] For different expansion joint models, the corresponding table of ω values ​​is shown in Table 3.

[0141] Table 3

[0142] Expansion joint model Type 60 Type 80 Type 100 Type 120 Type 160 ω 1.173 0.980 0.856 0.702 0.484

[0143] This embodiment also provides a method for installing a prefabricated panel at a bridge connection, comprising the following steps:

[0144] S100. Cleaning of expansion joint notches.

[0145] like Figure 4 As shown, the bridge includes a first beam and a second beam, and a portion of the upper surfaces of the first beam and the second beam are provided with a bridge deck pavement structure; an expansion joint is provided between the first beam and the second beam; and an expansion joint notch is formed between the upper surfaces of the first beam and the second beam that are not covered by the bridge deck pavement structure. The original expansion joint notch of the bridge is cleaned, and if it is a bridge to be repaired, the existing expansion device components and parts need to be removed; the cleaning depth of the expansion joint notch is generally not less than 15 cm, and the width is not less than 40 cm. Embedded steel bars are provided on the upper surfaces of the portions of the first beam and the second beam that are not provided with the bridge deck pavement structure, and the embedded steel bars penetrate into the first beam and the second beam.

[0146] S200, pour anchoring concrete.

[0147] like Figure 5 As shown, anchor bolts are embedded in the expansion joint groove after cleaning, and anchor concrete is poured to the control elevation. Parts of the embedded anchor bolts extend out of the upper surface of the anchor concrete, and the embedded steel bars are completely embedded in the anchor concrete. The anchor bolt model is M16, and its installation spacing along the transverse direction of the bridge is 15cm.

[0148] S300, install prefabricated panels.

[0149] like Figure 6 As shown, the surface of the anchoring concrete is leveled, and the height difference after surface leveling should be less than ±1mm; the precast slab is tensioned according to the calculation of the expansion and contraction of the bridge, and the precast slab is anchored by pre-embedded anchor bolts.

[0150] Before installation, precast panels should be pre-tensioned according to the installation temperature and bridge length to ensure that the precast panels are always in a tensioned state during operation and effectively prevent arching of expansion joints.

[0151] When constructing expansion joints of different types, the corresponding relationship between the tension force and tension amount of the precast panels is as follows:

[0152]

[0153] Among them, F y is the tensile force applied to the precast panel, in KN; b y is the tension amount, in cm; λ and A are tension parameters;

[0154] For different expansion joint models, the corresponding table of λ and A values ​​is shown in Table 4.

[0155] Expansion joint model Type 60 Type 80 Type 100 Type 120 Type 160 λ 14.5 12 10 8.5 7 A 3 5.5 13 14.5 17

[0156] S400, pouring elastic sealing layer.

[0157] Cast the notches between the two sides of the precast slab and the bridge deck pavement to form an elastic sealing layer. The upper surface of the elastic sealing layer is flush with the upper surface of the precast slab and the upper surface of the bridge deck pavement structure, and the height difference is controlled within ±1mm. The elastic sealing layer can be made of concrete or asphalt. If concrete is used, its strength should not be less than C50, and the steel fiber content should not be less than 150kg / m 3 .

[0158] The prefabricated panels are installed at bridge connections, wherein the bridge is an existing bridge that needs to have its expansion device repaired or a newly constructed bridge that needs to have its expansion device constructed, and the constructed expansion devices are all located at expansion joint notches reserved on the existing bridge to be repaired or the main beam of the newly constructed bridge.

[0159] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for preparing a flame-retardant elastic material for a bridge expansion joint, characterized in that: The method comprises the steps of mixing phosphorus and nitrogen functionalized lignin nanoparticles with prepolymer and reacting the mixture to obtain a flame retardant elastic material for bridge expansion joints; The prepolymer is prepared by adding isocyanate, polyol and catalyst into N,N-dimethylformamide solvent. Obtained after reaction.

2. The preparation method according to claim 1, characterized in that: The preparation of the phosphorus and nitrogen functionalized lignin nanoparticles comprises the following steps: (1) treating acetic acid lignin powder to obtain purified lignin; (2) dissolving the purified lignin obtained in step (1) in an alkaline solution, adding formaldehyde and polyethyleneimine, adjusting the pH value to acidic after the reaction, washing the precipitate with deionized water to neutrality, and drying to obtain nitrogen-containing lignin; (3) adding the nitrogen-containing lignin, formaldehyde and phosphorus-based flame retardant obtained in step (2) to an N,N-dimethylformamide solvent, adjusting the pH value to acidic, and obtaining phosphorus- and nitrogen-functionalized lignin after reaction; (4) dissolving the phosphorus- and nitrogen-functionalized lignin obtained in step (3) in an N,N-dimethylformamide solvent, slowly dripping deionized water into the solvent while performing ultrasonic treatment, and obtaining the phosphorus- and nitrogen-functionalized lignin nanoparticles after centrifugal separation.

3. The preparation method according to claim 2, characterized in that: Step (1) specifically includes: The acetic acid lignin powder is mixed with the acetic acid solution, stirred evenly, and then filtered using a sand core funnel, and the filtrate is retained; The filtrate and deionized water are mixed and stirred evenly, and the mixture is allowed to stand to collect the precipitate, wherein the temperature of the deionized water is between 60° C. and 90° C.; The precipitate is stirred and washed with deionized water until the pH value is neutral, and then dried to obtain the purified lignin; Wherein, the concentration of the acetic acid solution is between 80wt% and 95wt%.

4. The preparation method according to claim 2, characterized in that: In step (2), the alkaline solution is selected from any one of potassium hydroxide, sodium hydroxide, ammonia water, or sodium carbonate; The concentration of the alkaline solution is between 6 wt % and 23 wt %.

5. The preparation method according to claim 2, characterized in that: In both step (2) and step (3), an acidic solution is used to adjust the pH value to 2 to 4; The acidic solution is selected from hydrochloric acid or sulfuric acid, and the concentration of the acidic solution is between 40wt% and 70wt%.

6. The preparation method according to claim 2, characterized in that: In step (3), the phosphorus-based flame retardant is selected from phosphates, phosphites, organic phosphorus salts, phosphorus oxides and phosphorus-nitrogen compounds, 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide and its derivatives.

7. The preparation method according to claim 1, characterized in that: The isocyanate is selected from any one or more of toluene diisocyanate, diphenylmethane diisocyanate, isophorone diisocyanate, and hexamethylene diisocyanate; the polyol is selected from any one or more of polytetramethylene glycol, polycaprolactone polyol, polycarbonate polyol, polytetramethyl vinyl ether glycol, and castor oil; the functionality of the polyol is 2 to 3, and the average molecular weight is 400 to 6000; The catalyst is selected from any one of triethylenediamine, dimethylethanolamine, N-methylmorpholine, N,N-dimethylcyclohexylamine, stannous octoate, stannous oleate, and dibutyltin dilaurate; The ratio of -NCO in the isocyanate to -OH in the polyol is between 1.0 and 1.

2.

8. A flame retardant elastic material for bridge expansion joints prepared according to the preparation method according to any one of claims 1 to 7.

9. Use of the flame-retardant elastic material for bridge expansion joints prepared by the preparation method according to any one of claims 1 to 7, and the flame-retardant elastic material for bridge expansion joints according to claim 8 in the expansion joint structure of bridge engineering.

10. The use according to claim 9, characterized in that: The phosphorus and nitrogen functionalized lignin nanoparticles are mixed with the prepolymer and poured into a prefabricated mold, and a prefabricated board is formed after demoulding; The prefabricated mold comprises a mold body, a mold cavity arranged in the mold body, and a heating rod arranged in the mold body, wherein the heating rod is reciprocatingly bent and arranged in the mold body; a steel member is arranged in the mold cavity; After the phosphorus and nitrogen functionalized lignin nanoparticles are stirred with the prepolymer and poured into the mold cavity of the prefabricated mold, the prefabricated mold is placed in a vacuum oven, the heating rod is turned on, and the temperature in the vacuum oven is ensured to be consistent with the temperature of the heating rod. After curing and demoulding, the prefabricated board is obtained; Preferably, before pouring the phosphorus and nitrogen functionalized lignin nanoparticles and the prepolymer into the mold cavity of the prefabricated mold, the steel member is pre-tensioned; Preferably, the prefabricated panels are installed at the bridge connection, and the installation method comprises the following steps: Cleaning bridge expansion joint notches; pouring anchor concrete; Install precast panels; Pouring sealing layer; Preferably, before installing the prefabricated panels, the prefabricated panels are pre-tensioned according to the installation temperature and the length of the bridge.