High-strength foamed plastic and preparation method thereof

Through the combination of flame retardant agents and material treatment of specific proportions, the problems of flammability and strength of polyurethane foam are solved, and the preparation of foam with high flame retardancy and high strength is achieved.

CN119019634AInactive Publication Date: 2024-11-26JIESHOU FENGHUA PLASTICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411315530.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polyurethane foam is flammable and the strength decreases after the introduction of flame retardant, making it difficult to find a balance between improving flame retardancy and maintaining strength.

Method used

Using a combination of flame retardant with a specific ratio, the flame retardant is prepared by materials such as epoxy propyl alcohol, oxychloride, triethylamine and nanocarbon black, combined with dibutyltin dilaurate and additives to form a stable network structure. and flame retardant films to enhance the flame retardancy and strength of foam plastics.

Benefits of technology

The flame retardant properties and strength of foam plastics are significantly improved, the problem of decrease in strength after the introduction of flame retardant is avoided, and the balance of high flame retardancy and high strength is achieved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-strength foamed plastic, and relates to the technical field of foamed plastics, the high-strength foamed plastic comprises the following raw materials by weight: 80-100 parts of polytetrahydrofuran ether glycol, 20-30 parts of toluene diisocyanate, 1-2 parts of an auxiliary agent, 0.2-0.5 part of dibutyltin dilaurate, 10-15 parts of a flame retardant I, and 5-10 parts of a flame retardant II; wherein the flame retardant I is prepared from the following raw materials: glycidol, phosphorus oxychloride, triethylamine and methylbenzene; the flame retardant II is prepared from the following raw materials: glycidol, phosphorus oxychloride, triethylamine, methylbenzene and nano carbon black; by adding the flame retardant I, a large amount of epoxy groups with phosphate groups in the flame retardant I can be subjected to a crosslinking reaction with isocyanate groups in the prepolymer to form a stable network structure, so that the compatibility is improved, the phosphate groups on the epoxy groups exert flame retardance, the flame retardance of the foamed plastic is enhanced, and the flame retardance of the foamed plastic is improved. And the combination of the epoxy group and the isocyanate group enhances the crosslinking degree, so that the interface is more stable, and the strength of the foamed plastic can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of foam plastics, and in particular to a high-strength foam plastic and a preparation method thereof. Background Art

[0002] Foam plastics are polymer materials with plastic as the basic component and containing a large number of bubbles. Therefore, they can also be said to be composite plastics with gas as filler. Compared with pure plastics, it has many excellent properties, such as light weight, high specific strength, ability to absorb impact loads, good heat insulation and sound insulation, etc. Therefore, it has been widely used in the fields of industry, agriculture, construction, transportation, etc. Since its advent, foam plastics have been increasingly used and their varieties have been continuously enriched. Among them, the more common traditional foam plastics are mainly polyurethane (PUR), polystyrene (PS), polyvinyl chloride (PVC), polyethylene (PE), phenolic resin (PF) and other varieties.

[0003] Among them, polyurethane foam is one of the most important and largest-volume synthetic polymers since the 20th century. Due to its advantages of low density, high specific strength and outstanding thermal insulation performance, it has been widely used in aerospace sound absorption and noise reduction, railway solidified roadbed and building thermal insulation. However, polyurethane foam has a large number of hydrocarbon segments, which makes it highly flammable, and its limiting oxygen index (LOI) is only 17%-19%. After ignition, it will burn quickly and release a lot of heat, accompanied by the release of smoke and toxic gases, and the risk factor is very high.

[0004] In order to solve the flammability problem of polyurethane foam, improving flame retardancy has become an important issue that modern industry is committed to solving. In the prior art, polyurethane foam is mostly produced by the gradual polymerization reaction of polyols and isocyanates, and its flame retardancy is enhanced by introducing various flame retardants into it.

[0005] However, although the introduction of flame retardants can improve its flame retardant properties to a certain extent, it is often accompanied by a decrease in strength. This is because: first, the addition of flame retardants may change the degree of crosslinking of polyurethane foam, and the degree of crosslinking is one of the important factors affecting the strength of polyurethane foam. If the interaction between the flame retardant and the polyurethane matrix leads to a decrease in the degree of crosslinking, the strength performance of the foam may decrease; second, the compatibility between flame retardants and polyurethane is often poor, so phase separation and interface separation may occur in the foam plastic. Then, when subjected to external force, the force point of the foam plastic may become a stress concentration point, which in turn causes the foam plastic to be easily destroyed. Summary of the invention

[0006] The purpose of the present invention is to provide a high-strength foam plastic and a preparation method thereof; to solve the following technical problems:

[0007] How to prevent flame retardants from affecting the strength of foam plastics?

[0008] The purpose of the present invention can be achieved through the following technical solutions:

[0009] In a first aspect, the present invention discloses a high-strength foam plastic, comprising the following raw materials in parts by weight:

[0010] 80-100 parts of polytetramethylene glycol, 20-30 parts of toluene diisocyanate, 1-2 parts of auxiliary agent, 0.2-0.5 parts of dibutyltin dilaurate, 10-15 parts of flame retardant I, 5-10 parts of flame retardant II;

[0011] Preferably, polytetramethylene glycol is 85-95 parts, toluene diisocyanate is 23-28 parts, auxiliary agent is 1.2-1.8 parts, dibutyltin dilaurate is 0.3-0.5 parts, flame retardant I is 12-14 parts, and flame retardant II is 6-9 parts;

[0012] More preferably, polytetramethylene glycol is 90 parts, toluene diisocyanate is 25 parts, the auxiliary agent is 1.5 parts, dibutyltin dilaurate is 0.4 parts, flame retardant I is 13 parts, and flame retardant II is 8 parts.

[0013] The raw materials of the flame retardant I include propylene oxide, phosphorus oxychloride, triethylamine, and toluene; the raw materials of the flame retardant II include propylene oxide, phosphorus oxychloride, triethylamine, toluene, and nano carbon black.

[0014] In a further embodiment of the present invention, the preparation method of the flame retardant I is:

[0015] Step 1: Prepare 20-30 parts of glycidol, 10-20 parts of phosphorus oxychloride, 25-30 parts of triethylamine, and 115-125 parts of toluene according to weight parts;

[0016] Preferably, glycidol is 22-28 parts, phosphorus oxychloride is 12-18 parts, triethylamine is 26-28 parts, and toluene is 118-122 parts;

[0017] More preferably, the amount of glycidol is 25 parts, the amount of phosphorus oxychloride is 15 parts, the amount of triethylamine is 27 parts, and the amount of toluene is 120 parts.

[0018] Step 2: Add 80-90% toluene into the stirrer, then add propylene oxide and triethylamine, stir evenly to obtain material A, and cool material A to 0°C.

[0019] Step 3: Add the remaining toluene and phosphorus oxychloride into the container and stir evenly to obtain a phosphorus oxychloride solution, slowly drop the phosphorus oxychloride solution into material A at 0°C, stir while dropping, raise the temperature to 25-30°C after the dropwise addition and keep slowly stirring for 20-24h to obtain material B;

[0020] Preferably, the temperature is raised to 26-29°C and stirred slowly for 21-23h;

[0021] More preferably, the temperature is raised to 28°C and stirred slowly for 22 hours.

[0022] Step 4: Filter material B once to remove the generated triethylamine salt, let the obtained primary filtrate stand for 20-24 hours and then filter it again to further remove the triethylamine salt, distill the obtained secondary filtrate to remove the solvent and other products, and the solid remaining after distillation is flame retardant I.

[0023] In the formation process of flame retardant I, the epoxy group of glycidol is a strong positive center, and the amine group in triethylamine can attack the carbon atom of the epoxy group, resulting in the ring opening of the epoxy group. The nitrogen atom of triethylamine is connected to the ring-opening carbon atom of glycidol to form a series of products containing amino alcohol structures. These products react with phosphorus oxychloride having strong electrophilic properties, so that phosphorus oxychloride undergoes a series of reactions with the amino group and the hydroxyl group in the amino alcohol structure, so that the final product flame retardant I contains a large number of epoxy groups with phosphate groups and has significant flame retardant properties.

[0024] In a further embodiment of the present invention, the preparation method of the flame retardant II is:

[0025] Step 1: Prepare 20-30 parts of glycidol, 10-20 parts of phosphorus oxychloride, 25-30 parts of triethylamine, 115-125 parts of toluene, and 15-20 parts of nano carbon black according to weight parts;

[0026] Preferably, 22-28 parts of glycidol, 12-18 parts of phosphorus oxychloride, 26-28 parts of triethylamine, 118-122 parts of toluene, and 16-19 parts of nano carbon black;

[0027] More preferably, the amount of glycidol is 25 parts, phosphorus oxychloride is 15 parts, triethylamine is 27 parts, toluene is 120 parts, and nano carbon black is 18 parts.

[0028] Step 2: Add glycidol and nano carbon black into a mixer and stir evenly to obtain modified nano carbon black with glycidol coated on the surface;

[0029] Step 3: Add 80-90% toluene, modified nano carbon black and triethylamine into the stirrer, stir evenly to obtain material M, and cool material M to 0°C;

[0030] Step 3: Add the remaining toluene and phosphorus oxychloride into the container and stir evenly to obtain a phosphorus oxychloride solution, slowly drop the phosphorus oxychloride solution into the material M at 0°C, stirring while dropping, and after the dropwise addition, heat to 25-30°C and keep stirring slowly for 20-24h to obtain material N;

[0031] Preferably, the temperature is raised to 26-29°C and stirred slowly for 21-23h;

[0032] More preferably, the temperature is raised to 28°C and stirred slowly for 22 hours.

[0033] Step 4: Filter material N once, let the first filtrate stand for 20-24 hours and then filter it again, distill the second filtrate, and the solid remaining after distillation is flame retardant II.

[0034] The preparation methods of flame retardant II and flame retardant I are similar, and the only difference is that before reacting glycidol with triethylamine, glycidol and nano-carbon black are first mixed, and high-speed stirring is adopted during mixing. The epoxy group in the glycidol molecule is a highly active functional group. On the surface of nano-carbon black, the epoxy group reacts with the hydroxyl group on the surface of carbon black to form an ether bond, and reacts with the carboxyl group to form an ester bond, so that the glycidol molecule is firmly wrapped on the surface of nano-carbon black. Nano-carbon black has a high specific surface area and strength. It is wrapped in glycidol, which can greatly improve the strength performance of glycidol; therefore, the flame retardant II finally obtained has flame retardant properties, and its strength performance is also greatly improved.

[0035] In a further embodiment of the present invention: in the second step, the material A is cooled to 0°C by a salt bath method.

[0036] In a further embodiment of the present invention, the auxiliary agent is one or both of liquid paraffin and dimethyl silicone oil, preferably a mixture of the two.

[0037] In a second aspect, the present invention further discloses a method for preparing the high-strength foam plastic as described above, comprising the following preparation steps:

[0038] S1: Under a nitrogen atmosphere, 40-60% of polytetramethylene glycol is added into a stirrer, and then toluene diisocyanate is added, and stirred at 75-85° C. for 2-3 hours to obtain a prepolymer;

[0039] S2: adding the remaining polytetramethylene glycol and the additive to the prepolymer, stirring at 75-80° C. for 0.5-1 h, then adding dibutyltin dilaurate, and continuing stirring for 1.5-2 h to obtain a mixed solution;

[0040] S3: After adding flame retardant I to the mixed liquid, the mixture is immediately stirred rapidly until foaming occurs, and then allowed to stand for free foaming until the foam surface no longer rises, and the mixture is immediately transferred to a drying device, and heated at 80-100° C. for 4-5 hours to obtain a semi-cured foamed plastic preform;

[0041] S4: dissolving flame retardant II in water to form a flame retardant solution, injecting the flame retardant solution into an impregnation box, transferring the foamed plastic preform into the impregnation box, ensuring that the flame retardant solution covers the foamed plastic preform, then sealing the impregnation box, adjusting the pressure of the impregnation box to -(0.1-0.2)MPa, and maintaining the pressure at the pressure for 10-15min, and after the end, taking out the foamed plastic preform and drying it until no droplets fall;

[0042] S5: Put the foamed plastic preform back into the drying equipment again, and heat it at 80-100° C. for 3-4 hours to obtain a high-strength foamed plastic.

[0043] First, during the preparation process, by adding flame retardant I, a large number of epoxy groups with phosphoric acid groups in flame retardant I can undergo cross-linking reaction with isocyanate groups in prepolymers to form a stable network structure, thereby improving compatibility. The phosphoric acid groups on the epoxy groups play a flame retardant role and enhance the flame retardancy of the foam plastics. The combination of epoxy groups and isocyanate groups enhances the cross-linking degree and makes the interface more stable, thereby improving the strength of the foam plastics.

[0044] Secondly, the foamed plastic preform is taken out when it is heated to a state where it is not completely solidified, that is, it is taken out when it is in a semi-solidified state. At this time, the foamed plastic preform has completed foaming, and a number of openings are formed inside it. At this time, it is placed in an impregnation box containing a flame retardant solution, and the flame retardant solution is introduced into the openings by drawing negative pressure. The flame retardant II in the flame retardant solution combines with part of the isocyanate groups in the foam plastic in the openings, thereby forming a flame retardant film formed by flame retardant II inside the openings, which can not only further enhance the flame retardancy of the foam plastic, but also the nano carbon black inside it supports the inner wall of the opening, thereby improving the strength performance of the foam plastic.

[0045] In a further embodiment of the present invention: in step S2, the dibutyltin dilaurate is added dropwise with stirring, and the time interval between each two drops is 3-5 minutes.

[0046] In a further embodiment of the present invention: in step S4, the mass fraction of the flame retardant solution is 25-35%, preferably 30%.

[0047] In a further embodiment of the present invention, after completion, the foamed plastic preform is taken out and placed above an impregnation box to dry, so that the liquid droplets fall into the impregnation box.

[0048] Beneficial effects of the present invention:

[0049] (1) In the foam plastic of the present invention, by adding flame retardant I, a large number of epoxy groups with phosphoric acid groups in flame retardant I can undergo cross-linking reaction with isocyanate groups in prepolymer to form a stable network structure, thereby improving its compatibility. The phosphoric acid groups on the epoxy groups play a flame retardant role and enhance the flame retardancy of the foam plastic. The combination of epoxy groups and isocyanate groups enhances the cross-linking degree and makes the interface more stable, thereby improving the strength of the foam plastic.

[0050] (2) In the preparation process of the foam plastic of the present invention, the foam plastic preform is taken out after being heated to a state where it is not completely solidified, i.e., it is taken out in a semi-solidified state. At this time, the foam plastic preform has completed foaming and a plurality of openings are formed inside it. At this time, it is placed in an impregnation box containing a flame retardant solution. The flame retardant solution is introduced into the openings by drawing negative pressure. The flame retardant II in the flame retardant solution combines with part of the isocyanate groups in the foam plastic in the openings, thereby forming a flame retardant film formed by the flame retardant II inside the openings. This can not only further enhance the flame retardancy of the foam plastic, but also the nano carbon black inside it can support the inner wall of the opening, thereby improving the strength performance of the foam plastic. DETAILED DESCRIPTION

[0051] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.

[0052] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.

[0053] Example 1

[0054] Preparation of flame retardant Ⅰ:

[0055] Add 1020g of toluene to a stirring tank, then add 250g of propylene oxide and 270g of triethylamine, stir evenly to obtain material A, and cool material A to 0°C in a salt bath; add 180g of toluene and 150g of phosphorus oxychloride to a beaker and stir evenly to obtain a phosphorus oxychloride solution, slowly drop the phosphorus oxychloride solution into material A at 0°C, stirring while dropping, and after the dropwise addition, heat to 28°C and keep stirring slowly for 22h to obtain material B; filter material B once to remove the generated triethylamine salt, and filter the obtained primary filtrate again after standing for 24h to further remove the triethylamine salt, and distill the obtained secondary filtrate to remove the solvent and other products. The solid remaining after distillation is flame retardant I, which weighs 216g.

[0056] Example 2

[0057] Preparation of flame retardant II:

[0058] 250g of propylene oxide and 180g of nano carbon black were added to a mixer, and stirred at 1000rpm for 15min to obtain modified nano carbon black with propylene oxide coated on the surface; 1020g of toluene was added to a stirring tank, and then the modified nano carbon black and 270g of triethylamine were added, and the mixture was stirred evenly to obtain material M, and the material M was cooled to 0°C in a salt bath; 180g of toluene and 150g of phosphorus oxychloride were added to a beaker and stirred evenly to obtain a phosphorus oxychloride solution, and the phosphorus oxychloride solution was slowly dripped into the material M at 0°C, and stirred while dripping. After the dripping was completed, the temperature was raised to 28°C and the mixture was stirred slowly for 22h to obtain material N; material N was filtered once, and the obtained primary filtrate was filtered again after standing for 24h, and the obtained secondary filtrate was distilled, and the solid remaining after distillation was flame retardant II, which weighed 376g.

[0059] Example 3

[0060] Preparation of high-strength foam plastics:

[0061] Under nitrogen atmosphere, 40 g of polytetramethylene glycol was added to a stirrer, and then 20 g of toluene diisocyanate was added, and the mixture was stirred at 75° C. for 3 h to obtain a prepolymer; 40 g of polytetramethylene glycol, 0.5 g of liquid paraffin and 0.5 g of dimethyl silicone oil were added to the prepolymer, and the mixture was stirred at 75° C. for 1 h, and then 0.3 g of dibutyltin dilaurate was added, and the mixture was stirred for 2 h to obtain a mixed solution; 10 g of flame retardant I was added to the mixed solution, and the mixture was immediately stirred quickly until foaming, and then the mixture was allowed to stand and wait for free foaming until the foam surface no longer rose, and the mixture was immediately transferred to a drying device, and heated at 80° C. for 5 h to obtain a semi-cured foamed plastic preform, and a sample with a length, width and height of 3 cm was cut out;

[0062] Add 50g of flame retardant II into a beaker, then add 200g of water, stir evenly to obtain a flame retardant solution with a mass fraction of 25%, inject the flame retardant solution into a glass impregnation cylinder with a diameter of 6cm, transfer the foamed plastic preform sample to the glass impregnation cylinder, observe that the flame retardant solution overflows the foamed plastic preform, then seal the impregnation box, adjust the pressure of the impregnation box to -0.2MPa, and maintain the pressure for 10min. After the end, take out the foamed plastic preform sample and dry it on the glass impregnation cylinder until no droplets fall. During this process, the dripping droplets flow into the glass impregnation cylinder; it is calculated that 43g of flame retardant II remains in the glass impregnation cylinder; then put the foamed plastic preform back into the drying equipment again, and heat it at 80℃ for 4h to obtain a high-strength foamed plastic.

[0063] Example 4

[0064] Under nitrogen atmosphere, 40 g of polytetramethylene glycol was added to a stirrer, and then 23 g of toluene diisocyanate was added, and the mixture was stirred at 80° C. for 2.5 h to obtain a prepolymer; 45 g of polytetramethylene glycol, 0.5 g of liquid paraffin and 0.7 g of dimethyl silicone oil were added to the prepolymer, and the mixture was stirred at 78° C. for 0.8 h, and then 0.4 g of dibutyltin dilaurate was added, and the mixture was stirred for 1.8 h to obtain a mixed solution; 12 g of flame retardant I was added to the mixed solution, and the mixture was immediately stirred quickly until foaming, and then allowed to stand for free foaming until the foam surface no longer rose, and the mixture was immediately transferred to a drying device, and heated at 90° C. for 4.5 h to obtain a semi-cured foamed plastic preform, and a sample with a length, width and height of 3 cm was cut out;

[0065] Add 60g of flame retardant II into a beaker, then add 200g of water, stir evenly to obtain a flame retardant solution with a mass fraction of 30%, inject the flame retardant solution into a glass impregnation cylinder with a diameter of 6cm, transfer the foamed plastic preform sample to the glass impregnation cylinder, observe that the flame retardant solution overflows the foamed plastic preform, then seal the impregnation box, adjust the pressure of the impregnation box to -0.15MPa, and maintain the pressure at this pressure for 12.5min. After the end, take out the foamed plastic preform sample and dry it above the glass impregnation cylinder until no droplets fall. In this process, the falling droplets are transferred into the glass impregnation cylinder; it is calculated that 55g of flame retardant II remains in the glass impregnation cylinder; then put the foamed plastic preform back into the drying equipment again, and heat it at 90℃ for 3.5h to obtain a high-strength foamed plastic.

[0066] Example 5

[0067] Under nitrogen atmosphere, 45 g of polytetramethylene glycol was added to a stirrer, and then 25 g of toluene diisocyanate was added, and the mixture was stirred at 80° C. for 2.5 h to obtain a prepolymer; 45 g of polytetramethylene glycol, 0.8 g of liquid paraffin and 0.7 g of dimethyl silicone oil were added to the prepolymer, and the mixture was stirred at 78° C. for 0.8 h, and then 0.4 g of dibutyltin dilaurate was added, and the mixture was stirred for 1.8 h to obtain a mixed solution; 13 g of flame retardant I was added to the mixed solution, and the mixture was immediately stirred quickly until foaming, and then the mixture was allowed to stand and wait for free foaming until the foam surface no longer rose, and the mixture was immediately transferred to a drying device, and heated at 90° C. for 4.5 h to obtain a semi-cured foamed plastic preform, and a sample with a length, width and height of 3 cm was cut out;

[0068] Add 60g of flame retardant II into a beaker, then add 200g of water, stir evenly to obtain a flame retardant solution with a mass fraction of 30%, inject the flame retardant solution into a glass impregnation cylinder with a diameter of 6cm, transfer the foamed plastic preform sample to the glass impregnation cylinder, observe that the flame retardant solution overflows the foamed plastic preform, then seal the impregnation box, adjust the pressure of the impregnation box to -0.15MPa, and maintain the pressure at this pressure for 12.5min. After the end, take out the foamed plastic preform sample and dry it above the glass impregnation cylinder until no droplets fall. In this process, the dripping droplets are transferred into the glass impregnation cylinder; it is calculated that 52g of flame retardant II remains in the glass impregnation cylinder; then put the foamed plastic preform back into the drying equipment again, and heat it at 90℃ for 3.5h to obtain a high-strength foamed plastic.

[0069] Example 6

[0070] Under nitrogen atmosphere, 50 g of polytetramethylene glycol was added to a stirrer, and then 28 g of toluene diisocyanate was added, and the mixture was stirred at 80° C. for 2.5 h to obtain a prepolymer; 45 g of polytetramethylene glycol, 0.8 g of liquid paraffin and 1 g of dimethyl silicone oil were added to the prepolymer, and the mixture was stirred at 78° C. for 0.8 h, and then 0.5 g of dibutyltin dilaurate was added, and the mixture was stirred for 1.8 h to obtain a mixed solution; 14 g of flame retardant I was added to the mixed solution, and the mixture was immediately stirred quickly until foaming, and then the mixture was allowed to stand and wait for free foaming until the foam surface no longer rose, and the mixture was immediately transferred to a drying device, and heated at 90° C. for 4.5 h to obtain a semi-cured foamed plastic preform, and a sample with a length, width and height of 3 cm was cut out;

[0071] Add 60g of flame retardant II into a beaker, then add 200g of water, stir evenly to obtain a flame retardant solution with a mass fraction of 30%, inject the flame retardant solution into a glass impregnation cylinder with a diameter of 6cm, transfer the foamed plastic preform sample to the glass impregnation cylinder, observe that the flame retardant solution overflows the foamed plastic preform, then seal the impregnation box, adjust the pressure of the impregnation box to -0.15MPa, and maintain the pressure at this pressure for 12.5min. After the end, take out the foamed plastic preform sample and dry it above the glass impregnation cylinder until no droplets fall. In this process, the dripping droplets are transferred into the glass impregnation cylinder; it is calculated that 52g of flame retardant II remains in the glass impregnation cylinder; then put the foamed plastic preform back into the drying equipment again, and heat it at 90℃ for 3.5h to obtain a high-strength foamed plastic.

[0072] Example 7

[0073] Under nitrogen atmosphere, 60g of polytetramethylene glycol was added to a stirrer, and then 30g of toluene diisocyanate was added, and the mixture was stirred at 85°C for 2h to obtain a prepolymer; 40g of polytetramethylene glycol, 1g of liquid paraffin and 1g of dimethyl silicone oil were added to the prepolymer, and the mixture was stirred at 80°C for 0.5h, and then 0.5g of dibutyltin dilaurate was added, and the mixture was stirred for 1.5h to obtain a mixed solution; 15g of flame retardant I was added to the mixed solution, and the mixture was immediately stirred quickly until foaming, and then the mixture was allowed to stand and wait for free foaming until the foam surface no longer rose, and the mixture was immediately transferred to a drying device, and heated at 100°C for 4h to obtain a semi-cured foamed plastic preform, and a sample with a length, width and height of 3cm was cut out;

[0074] Add 70g of flame retardant II into a beaker, then add 200g of water, stir evenly to obtain a flame retardant solution with a mass fraction of 35%, inject the flame retardant solution into a glass impregnation cylinder with a diameter of 6cm, transfer the foamed plastic preform sample to the glass impregnation cylinder, observe that the flame retardant solution overflows the foamed plastic preform, then seal the impregnation box, adjust the pressure of the impregnation box to -0.1MPa, and maintain the pressure for 15min. After the end, take out the foamed plastic preform sample and dry it above the glass impregnation cylinder until no droplets fall. In this process, the dripping droplets are transferred into the glass impregnation cylinder; it is calculated that 50g of flame retardant II remains in the glass impregnation cylinder; then put the foamed plastic preform back into the drying equipment again, and heat it at 100℃ for 3h to obtain a high-strength foamed plastic.

[0075] Comparative Example 1

[0076] Under nitrogen atmosphere, 45 g of polytetramethylene glycol was added into a stirrer, and then 25 g of toluene diisocyanate was added, and the mixture was stirred at 80°C for 2.5 h to obtain a prepolymer; 45 g of polytetramethylene glycol, 0.8 g of liquid paraffin and 0.7 g of dimethyl silicone oil were added into the prepolymer, and the mixture was stirred at 78°C for 0.8 h, and then 0.4 g of dibutyltin dilaurate was added, and the mixture was stirred for 1.8 h to obtain a mixed solution; 13 g of flame retardant I was added into the mixed solution, and the mixture was immediately stirred rapidly until foaming occurred, and then the mixture was allowed to stand and wait for free foaming until the foam surface no longer rose, and the mixture was immediately transferred into a drying device and heated at 90°C for 7 h to obtain a high-strength foamed plastic, and a sample with a length, width and height of 3 cm was cut out.

[0077] Comparative Example 2

[0078] Under nitrogen atmosphere, 45 g of polytetramethylene glycol was added into a stirrer, and then 25 g of toluene diisocyanate was added, and the mixture was stirred at 80°C for 2.5 h to obtain a prepolymer; 45 g of polytetramethylene glycol, 0.8 g of liquid paraffin and 0.7 g of dimethyl silicone oil were added into the prepolymer, and the mixture was stirred at 78°C for 0.8 h, and then 0.4 g of dibutyltin dilaurate was added, and the mixture was stirred for 1.8 h to obtain a mixed solution; 21 g of flame retardant I was added into the mixed solution, and the mixture was immediately stirred rapidly until foaming, and then the mixture was allowed to stand and wait for free foaming until the foam surface no longer rose, and the mixture was immediately transferred into a drying device and heated at 90°C for 7 h to obtain a high-strength foamed plastic, and a sample with a length, width and height of 3 cm was cut out.

[0079] Comparative Example 3

[0080] Compared with Example 5, the only difference is that flame retardant II is replaced by flame retardant I.

[0081] The foamed plastics obtained in Examples 3-7 and Comparative Examples 1-3 were subjected to performance tests, including flame retardancy test, tensile strength test and impact strength test. The test methods were based on the following standards:

[0082] Flame retardant properties: GB / T2406.1-2008

[0083] Tensile strength: GB / T9641-1988

[0084] Impact strength: GJB1585-93

[0085] The test results are listed in Table 1. Table 1 is as follows:

[0086] Table 1

[0087] Contact angle (°) Tensile strength(Mpa) <![CDATA[Impact strength (KJ / m 2 )]]> Example 3 153 15 4.1 Example 4 154 16 4.5 Example 5 161 18 4.8 Example 6 160 18 4.6 Example 6 155 17 4.2 Comparative Example 1 100 3 1.2 Comparative Example 2 115 5 2.2 Comparative Example 3 132 4 2.1

[0088] By analyzing the data in Table 1, it can be seen that the contact angles of the foam plastics prepared in Examples 3-7 are significantly greater than those of the foam plastics prepared in Comparative Examples 1-3, indicating that they have stronger flame retardant properties; at the same time, the tensile strength and impact strength of the foam plastics prepared in Examples 3-7 are significantly better than those of the foam plastics prepared in Comparative Examples 1-3. Therefore, the foam plastics prepared by the method of the present invention have greatly improved strength while having high flame retardancy.

[0089] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A high-strength foam plastic, characterized in that: The invention comprises the following raw materials in parts by weight: 80-100 parts of polytetramethylene glycol, 20-30 parts of toluene diisocyanate, 1-2 parts of auxiliary agent, 0.2-0.5 parts of dibutyltin dilaurate, 10-15 parts of flame retardant I, 5-10 parts of flame retardant II; The raw materials of the flame retardant I include propylene oxide, phosphorus oxychloride, triethylamine, and toluene; the raw materials of the flame retardant II include propylene oxide, phosphorus oxychloride, triethylamine, toluene, and nano carbon black.

2. The high-strength foam plastic according to claim 1, characterized in that: The preparation method of the flame retardant I is: Step 1: Prepare 20-30 parts of glycidol, 10-20 parts of phosphorus oxychloride, 25-30 parts of triethylamine, and 115-125 parts of toluene according to weight parts; Step 2: Add 80-90% toluene into the stirrer, then add propylene oxide and triethylamine, stir evenly to obtain material A, and cool material A to 0°C; Step 3: Add the remaining toluene and phosphorus oxychloride into the container and stir evenly to obtain a phosphorus oxychloride solution, slowly drop the phosphorus oxychloride solution into material A at 0°C, stir while dropping, raise the temperature to 25-30°C after the dropwise addition and keep slowly stirring for 20-24h to obtain material B; Step 4: Filter material B once, let the first filtrate stand for 20-24 hours and then filter it again, distill the second filtrate, and the solid remaining after distillation is flame retardant I.

3. The high-strength foam plastic according to claim 1, characterized in that: The preparation method of the flame retardant II is: Step 1: Prepare 20-30 parts of glycidol, 10-20 parts of phosphorus oxychloride, 25-30 parts of triethylamine, 115-125 parts of toluene, and 15-20 parts of nano carbon black according to weight parts; Step 2: Add glycidol and nano carbon black into a mixer and stir evenly to obtain modified nano carbon black with glycidol coated on the surface; Step 3: Add 80-90% toluene, modified nano carbon black and triethylamine into the stirrer, stir evenly to obtain material M, and cool material M to 0°C; Step 3: Add the remaining toluene and phosphorus oxychloride into the container and stir evenly to obtain a phosphorus oxychloride solution, slowly drop the phosphorus oxychloride solution into the material M at 0°C, stirring while dropping, and after the dropwise addition, heat to 25-30°C and keep stirring slowly for 20-24h to obtain material N; Step 4: Filter material N once, let the first filtrate stand for 20-24 hours and then filter it again, distill the second filtrate, and the solid remaining after distillation is flame retardant II.

4. The high-strength foam plastic according to claim 2 or 3, characterized in that: In the second step, the material A was cooled to 0°C by a salt bath method.

5. The high-strength foam plastic according to claim 1, characterized in that: The auxiliary agent is one or both of liquid paraffin and dimethyl silicone oil.

6. A method for preparing a high-strength foam plastic according to any one of claims 1 to 5, characterized in that: The method comprises the following preparation steps: S1: Under a nitrogen atmosphere, 40-60% of polytetramethylene glycol is added into a stirrer, and then toluene diisocyanate is added, and stirred at 75-85° C. for 2-3 hours to obtain a prepolymer; S2: adding the remaining polytetramethylene glycol and the additive to the prepolymer, stirring at 75-80° C. for 0.5-1 h, then adding dibutyltin dilaurate, and continuing stirring for 1.5-2 h to obtain a mixed solution; S3: After adding flame retardant I to the mixed liquid, the mixture is immediately stirred rapidly until foaming occurs, and then allowed to stand for free foaming until the foam surface no longer rises, and the mixture is immediately transferred to a drying device, and heated at 80-100° C. for 4-5 hours to obtain a semi-cured foamed plastic preform; S4: dissolving flame retardant II in water to form a flame retardant solution, injecting the flame retardant solution into an impregnation box, transferring the foamed plastic preform into the impregnation box, ensuring that the flame retardant solution covers the foamed plastic preform, then sealing the impregnation box, adjusting the pressure of the impregnation box to -(0.1-0.2)MPa, and maintaining the pressure at the pressure for 10-15min, and after the end, taking out the foamed plastic preform and drying it until no droplets fall; S5: Put the foamed plastic preform back into the drying equipment again, and heat it at 80-100° C. for 3-4 hours to obtain a high-strength foamed plastic.

7. The method for preparing high-strength foam plastic according to claim 6, characterized in that: In step S2, the dibutyltin dilaurate is added dropwise with stirring, and the time interval between each two drops is 3-5 minutes.

8. The method for preparing high-strength foam plastic according to claim 6, characterized in that: In step S4, the mass fraction of the flame retardant solution is 25-35%.