Low-density high-resilience polyurethane material as well as preparation method and application thereof

By using a combination of highly reactive polyether polyol and symmetrical structure chain extender in polyurethane foam materials, the problems of low rebound rate and high compression permanent deformation rate are solved, and high rebound, low odor and The effect of low fatigue loss has expanded its application in the home field.

CN119019642APending Publication Date: 2024-11-26CHANGHUA CHEMICAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411142235.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing low-density polyurethane foam materials have low rebound rate, poor comfort, high compression permanent deformation rate, large fatigue loss and high odor, which limits its wide application in home furnishing fields such as mattresses.

Method used

The preparation method of low-density and high-resilience polyurethane material composed of polyether polyols, polymer polyols, modified isocyanates and other components is adopted. By introducing highly reactive polyether polyols and symmetrical structure chain extenders, combined with special processes, Increases the sponge's rebound rate and compresses permanent deformation rate and reduces odor.

Benefits of technology

It has achieved high rebound rate, low compression permanent deformation, low fatigue loss and low odor of low density and high rebound polyurethane foam, which has improved comfort and performance stability and broadened its application range in the home field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001181360000041
    Figure BDA0005001181360000041
  • Figure BDA0005001181360000042
    Figure BDA0005001181360000042
  • Figure BDA0005001181360000051
    Figure BDA0005001181360000051
Patent Text Reader

Abstract

The invention relates to a low-density and high-resilience polyurethane material as well as a preparation method and application thereof, and mainly solves the problems of low resilience rate, poor comfort, high compression permanent deformation rate, large fatigue loss and high odor of a polyurethane foam material at lower density in the prior art. According to the technical scheme, the novel low-density high-resilience polyurethane foam material is composed of a component A and a component B, and the mass ratio of the component A to the component B is 100: (40-53); the component A is prepared from the following components in parts by weight: 90 to 100 parts of polyether polyol, 5 to 10 parts of polymer polyol, 2.3 to 2.8 parts of water, 0.8 to 1.2 parts of foam stabilizer, 0.5 to 1 part of cross-linking agent, 0.1 to 0.2 part of amine catalyst and 0.1 to 0.3 part of metal catalyst; the component B comprises 30-40 parts of isocyanate, 10-15 parts of polyether polyol, 1-2.5 parts of a chain extender and 20 * 10 <-6 >-60 * 10 <-6 > parts of a storage stabilizer, the problem is well solved, and the polyurethane foam can be applied to mattresses, furniture, seats and furniture articles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a low-density high-resilience polyurethane material and a preparation method and application thereof. Background Art

[0002] Polyurethane soft sponge can be divided into four categories according to its material and performance: ordinary sponge, high rebound, slow rebound and other special sponges. At present, ordinary sponge can be widely used in the base layer of mattresses, i.e. the support layer, because of its good compression resistance. High rebound sponge is mainly used in sofa seats. Slow rebound and other special sponges are mainly used in the comfort layer of mattresses according to their special functions. With the development of society and the continuous improvement of people's material living standards, the comfort of mattresses has become more and more the focus of people's attention. Compared with ordinary sponge, high rebound sponge with higher resilience has better comfort, but the compression resistance of high rebound sponge will bring high storage and logistics costs, and will also cause quality problems such as deformation of mattresses after long-term use. This has largely limited its further use, especially in low-density cases, where this trend will become more obvious. Therefore, the development of a low-density, low-odor, high-rebound sponge foam plastic has positive significance for the entire home furnishing market.

[0003] Chinese patent 201811454502.6 discloses a 30-density high-rebound sponge and its preparation method. The prepared low-density high-rebound sponge has high rebound, and the ball rebound reaches more than 55. It has good support and suitable hardness, good stability, and is easy to transport, which reduces the production and processing cost of the high-rebound sponge. However, the sponge prepared in this patent has a low rebound rate, the highest of which is only 60.4%, and lacks a certain degree of comfort.

[0004] Chinese Patent 201910335853.3 discloses a high-rebound sponge and a preparation method to solve the problems of poor quality, short service life and easy tearing of high-rebound sponges in related technologies. In this invention patent, the formula system can be attributed to a polyether-polyester-high polymer polyol system. Usually, the introduction of polyester and polymer polyols will lead to a decrease in the resilience of the foam, but in this patent, the foam resilience reaches 72%. This technical route lacks certain theoretical support, and in terms of performance presentation, there are only rebound and hardness, and the test standards used are not clarified, so it is of little reference value. There is a certain degree of similarity between the invention patent and the problem to be solved by this patent, and both are committed to solving the technical difficulties in the industry, but this invention has not found a suitable solution. Summary of the invention

[0005] One of the technical problems to be solved by the present invention is that the existing polyurethane foam materials have low rebound rate, poor comfort, high compression permanent deformation rate, large fatigue loss and high odor at relatively low density. A new low-density high-rebound polyurethane material is provided, which has the advantages of high rebound rate, good comfort, low compression permanent deformation, small fatigue loss and low odor.

[0006] The second technical problem to be solved by the present invention is to provide a method for preparing a low-density high-resilience polyurethane material corresponding to the first technical problem to be solved.

[0007] The third technical problem to be solved by the present invention is to provide an application of a low-density high-resilience polyurethane material corresponding to solving the first technical problem.

[0008] In order to solve one of the above technical problems, the technical solution adopted by the present invention is as follows: composed of component A and component B, the mass ratio of component A to component B is 100:40-53; in parts by weight, component A includes: polyether polyol: 90-100 parts, polymer polyol: 5-10 parts, water: 2.3-2.8 parts, foam stabilizer: 0.8-1.2 parts, cross-linking agent: 0.5-1 part, amine catalyst: 0.1-0.2 parts, metal catalyst: 0.1-0.3 parts; component B includes isocyanate 30-40 parts, polyether polyol A: 10-15 parts, chain extender: 1-2.5 parts, storage stabilizer; 20×10- 6 ~60×10- 6份 The polyether polyol is a polyether polyol of ethylene oxide-propylene oxide copolymer with at least one of glycerol, trimethylolpropane and ethanolamine as an initiator, a molecular weight of 4000-8000, a primary hydroxyl content of ≥70%, an unsaturation of 0.01-0.2 mmol / g, and a functionality of 3; the polymer polyol is a polymer polyol with at least one of glycerol, pentaerythritol, xylitol, sorbitol or sucrose as an initiator, a molecular weight of 6000-8000, a functionality of 2-4, and a solid content of 25- 45%; the foam stabilizer is a polysiloxane-olefin oxide block or graft copolymer; the crosslinking agent is a small molecule polyol and a polyamine compound containing two or more functional groups; the amine catalyst is a tertiary amine catalyst containing a hydroxyl group; the metal catalyst is one or more of an alkyl compound and a carboxylate such as organic tin, zinc, bismuth, etc.; the isocyanate is selected from at least one of toluene diisocyanate, crude MDI or carbodiimide modified isocyanate; the chain extender is a difunctional aromatic small molecule alcohol with a symmetrical structure.

[0009] In the above technical solution, preferably, the polyether polyol is selected from CHE-2901L; and the polymer polyol is selected from at least one of CHP-H30 and CHP-H45.

[0010] In the above technical scheme, preferably, the foam stabilizer is selected from at least one of B8681, B8716 or L5333; the cross-linking agent is selected from at least one of triethanolamine, diethanolamine, glycerol or trimethylolpropane; the amine catalyst is selected from at least one of a foaming tertiary amine catalyst, a gel tertiary amine catalyst or a balanced tertiary amine catalyst; the metal catalyst is selected from at least one of dibutyltin dilaurate, stannous octoate, and dibutyltin diacetate; the isocyanate is selected from one of BASF-T80, PM-200 or MDI-LL.

[0011] In the above technical solution, preferably, the foaming tertiary amine catalyst is selected from at least one of LED103, LE-15 or ZF-10; the gel tertiary amine catalyst is selected from at least one of ZR-50, DPA, LED-204.

[0012] In the above technical solution, preferably, the chain extender is a difunctional aromatic small molecule alcohol with a symmetrical structure, selected from at least one of hydroquinone dihydroxyethyl ether (HQEE) and resorcinol bishydroxyethyl ether (HER), and the storage stabilizer is benzoyl chloride.

[0013] To solve the second of the above technical problems, the technical solution adopted by the present invention is as follows:

[0014] A method for preparing the aforementioned low-density high-resilience polyurethane foam material comprises the following steps:

[0015] (1) Preparation of component A: Weigh 90-100 parts of polyether polyol, 5-10 parts of polymer polyol, 2.3-2.8 parts of water, 0.8-1.2 parts of foam stabilizer, 0.5-1 part of cross-linking agent, 0.1-0.2 parts of amine catalyst, and 0.1-0.3 parts of metal catalyst in parts by weight; add them into a container in sequence, stir and mix thoroughly to obtain component A, and control the temperature at 23-25° C.;

[0016] (2) Preparation of component B

[0017] In parts by weight, weigh 10-15 parts of polyether polyol and 1-2.5 parts of chain extender, add them into the reaction kettle, stir and heat to 90-100°C, dehydrate and degas under vacuum for 2-3 hours, cool to 60°C, add 30-40 parts of isocyanate, and 20×10- 6 ~60×10- 6Component B is obtained when the NCO content is 32% to 33%;

[0018] (3) Preparation of low-density high-resilience polyurethane foam

[0019] The prepared component A and component B are mixed in a mass ratio of 100:40-53, fully stirred for 3-5 seconds at a rotation speed of 2000-5000 rpm, and then quickly injected into a mold and naturally matured for 24-48 hours to obtain a low-density and high-resilience polyurethane foam.

[0020] To solve the third of the above technical problems, the technical solution adopted by the present invention is as follows:

[0021] The aforementioned low-density high-resilience polyurethane foam material can be widely used in mattresses, furniture, seats, and furniture products.

[0022] The present invention provides a new low-density high-resilience polyurethane foam material, a composition of polyether polyol, polymer polyol and modified isocyanate B component, foaming to form a polyurethane foam material with high rebound rate, low compression permanent deformation, small fatigue loss and low odor, wherein the high-activity polyether polyol A synthesized by introducing a special structure and a special process, a higher equivalent value, and secondly, a symmetrical chain extender with a benzene ring structure is selected, and an effective combination is performed, which can well improve the ball rebound rate and compression permanent deformation rate of the sponge, and the extremely low odor can greatly reduce the odor and VOC value of the sponge. At the same time, the foaming difficulty of the high / pure polyether system in the industry is high, which is very easy to cause the foam closed cell shrinkage or collapse, so the technicians in this industry will use the method of increasing the amount of polymer polyol and adding powder to improve the open cell and stability of the foam, and this method will bring about the decline of rebound and compression permanent deformation performance. The prepolymerization process can well avoid the occurrence of excessive reaction heat, sponge closed cell shrinkage or collapse in the one-step foaming process, thereby preparing a polyurethane foam material with higher performance. DETAILED DESCRIPTION

[0023] Table 1 List of raw materials - additives

[0024]

[0025] Table 2 List of raw materials - main raw materials

[0026]

[0027] [Example 1]

[0028] (1) Preparation of component A

[0029] 90 parts of CHE-2901L, 10 parts of CHE-507LF, 2.4 parts of water, 0.03 parts of ZF-10, 0.1 parts of ZR-50, 0.9 parts of L-5333, 0.5 parts of DEOA and 0.15 parts of T900 were weighed in parts by weight, and added into a container in sequence, and stirred and mixed thoroughly to obtain component A;

[0030] (2) Preparation of component B

[0031] In terms of weight, weigh 10 parts of CHE-2901L and 2 parts of HQEE, add them into the reactor, stir and heat to 90-100°C, dehydrate and degas under vacuum for 2-3 hours, cool, add 37 parts of T80, 20×10- 6 The mixture was heated to 80-85°C for 2-3 hours, and the NCO content was detected to be 32.4%, thereby obtaining component B;

[0032] (3) Preparation of low-density and high-resilience polyurethane foam materials

[0033] The prepared component B and component A were mixed in a mass ratio of 100:44, fully stirred for 4 seconds at a rotation speed of 3000 rpm, and then quickly injected into an open mold and naturally matured for 24 hours to obtain a low-density and high-resilience polyurethane foam material.

[0034] [Examples 2 to 6 and Comparative Examples 1 to 3]

[0035] Examples 2 to 6 are carried out according to the steps of Example 1, with the only difference being the type of reaction raw materials, the type of catalyst, the raw material ratio, the reaction time and the temperature, as shown in Table 3. The conventional physical property test data of the prepared low-density and high-resilience polyurethane foam material are shown in Table 4.

[0036] Comparative Examples 1 to 2 were carried out according to the steps of Example 1. In addition to the differences in the types of reaction raw materials, catalyst types, raw material ratios, reaction time and temperature, there was also a difference in component B. No prepolymerization was required, and the isocyanate was directly weighed. See Table 3 for details.

[0037] Comparative Example 3 is a reproduction of Example 7 in accordance with Chinese Patent 201910335853.3, which discloses a high-resilience sponge and a preparation method. Because the patent disclosure is not sufficient, some raw materials cannot be obtained from existing channels, so substitutes with similar indicators and similar structures are selected. However, it does not violate the technical route and core ideas disclosed in the patent, as shown in Table 3, and the conventional performance data of the prepared polyurethane foam are shown in Table 4.

[0038] Table 3 Weight percentage of raw materials of each component in Examples 1 to 6 and Comparative Examples 1 to 3

[0039]

[0040]

[0041] Table 4 Performance test data of low-density high-resilience polyurethane materials prepared in Examples 1 to 6 and Comparative Examples 1 to 3

[0042]

[0043] Comparative Example 1 is a conventional density of 33kg / m 3 The formula route of the high-resilience sponge is shown in Figure 2. Comparative Example 2 uses conventional high-resilience polyether (pure polyether) on the market for foaming. The foam has severe closed-cell shrinkage and must be artificially broken. Comparative Example 3 reproduces Example 7 in Chinese Patent 201910335853.3, which discloses a high-resilience sponge and a preparation method. Examples 1 to 6 are adjusted on the basis of conventional high-resilience sponge formulas to improve the rebound rate and compression permanent deformation performance. It was found that by selecting suitable raw materials and reasonable ratios, the problems of low foam rebound rate and high compression permanent deformation rate at low density can be greatly improved. At the same time, the comfort and fatigue loss of the high-resilience sponge can be greatly improved, and the application field of the high-resilience sponge can be broadened.

[0044] The above content introduces in detail a method for preparing a low-density high-resilience polyurethane foam provided by the present invention. The embodiments herein illustrate the principle and implementation mode of the present invention. The introduction of the above embodiments is only for understanding the core idea of ​​the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the art shall make any modification to the present invention within the protection scope of the claims without departing from the principle of the present invention.

Claims

1. A low-density high-resilience polyurethane material, consisting of component A and component B, wherein the mass ratio of component A to component B is 100:40-53; in parts by weight, component A comprises: Polyether polyol: 90-100 parts, polymer polyol: 5-10 parts, water: 2.3-2.8 parts, foam stabilizer: 0.8-1.2 parts, crosslinking agent: 0.5-1 parts, amine catalyst: 0.1-0.2 parts, metal catalyst: 0.1-0.3 parts; component B includes isocyanate 30-40 parts, polyether polyol: 10-15 parts, chain extender: 1-2.5 parts, storage stabilizer; 20×10 -6 ~60×10 -6 The polyether polyol is a polyether polyol of ethylene oxide-propylene oxide copolymer with at least one of glycerol, trimethylolpropane and ethanolamine as an initiator, a molecular weight of 4000-8000, a primary hydroxyl content of ≥70%, an unsaturation of 0.01-0.2 mmol / g, and a functionality of 3; the polymer polyol is a polymer polyol with at least one of glycerol, pentaerythritol, xylitol, sorbitol or sucrose as an initiator, a molecular weight of 6000-8000, a functionality of 2-4, and a solid content of 25 ~45%; the foam stabilizer is a polysiloxane-olefin oxide block or graft copolymer; the crosslinking agent is a small molecule polyol and a polyamine compound containing two or more functional groups; the amine catalyst is a tertiary amine catalyst containing a hydroxyl group; the metal catalyst is one or more of an alkyl compound and a carboxylate such as organic tin, zinc, bismuth, etc.; the isocyanate is selected from at least one of toluene diisocyanate, crude MDI or carbodiimide modified isocyanate; the chain extender is a difunctional aromatic small molecule alcohol with a symmetrical structure.

2. The low-density high-resilience polyurethane material according to claim 1, characterized in that: The polyether polyol is selected from CHE-2901L; the polymer polyol B is selected from at least one of CHP-H30 and CHP-H45.

3. The low-density high-resilience polyurethane material according to claim 1, characterized in that: The foam stabilizer is selected from at least one of B8681, B8716 or L5333; the cross-linking agent is selected from at least one of triethanolamine, diethanolamine, glycerol or trimethylolpropane; the amine catalyst is selected from at least one of a foaming tertiary amine catalyst, a gel tertiary amine catalyst or a balanced tertiary amine catalyst; the metal catalyst is selected from at least one of dibutyltin dilaurate, stannous octoate and dibutyltin diacetate; the isocyanate is selected from one of BASF-T80, PM-200 or MDI-LL.

4. The low-density high-resilience polyurethane material according to claim 1, characterized in that: The foaming tertiary amine catalyst is selected from at least one of LED103, LE-15 or ZF-10; the gel tertiary amine catalyst is selected from at least one of ZR-50, DPA and LED-204.

5. The low-density high-resilience polyurethane material according to claim 1, characterized in that: The chain extender is a difunctional aromatic small molecule alcohol with a symmetrical structure, selected from at least one of hydroquinone dihydroxyethyl ether (HQEE) and resorcinol bishydroxyethyl ether (HER), and the storage stabilizer is benzoyl chloride.

6. A method for preparing the low-density high-resilience polyurethane foam material according to claim 1, comprising the following steps: (1) Preparation of component A: Weigh 90-100 parts of polyether polyol, 5-10 parts of polymer polyol, 2.3-2.8 parts of water, 0.8-1.2 parts of foam stabilizer, 0.5-1 part of cross-linking agent, 0.1-0.2 parts of amine catalyst, and 0.1-0.3 parts of metal catalyst in parts by weight; add them into a container in sequence, stir and mix thoroughly to obtain component A, and control the temperature at 23-25° C.; (2) Preparation of component B In parts by weight, weigh 10-15 parts of polyether polyol A and 1-2.5 parts of chain extender, add them into a reaction kettle, stir and heat to 90-100° C., dehydrate and degas under vacuum for 2-3 hours, cool to 60° C., add 30-40 parts of isocyanate and 20×10-6-60×10-6 parts of storage stabilizer, stir and heat to 80-85° C. for reaction for 2-3 hours, and obtain component B when the NCO content is 32%-33%; (3) Preparation of low-density high-resilience polyurethane foam The prepared component A and component B are mixed in a mass ratio of 100:40-53, fully stirred for 3-6 seconds at a rotation speed of 2000-5000 rpm, and then quickly injected into a mold and naturally matured for 24-48 hours to obtain a low-density and high-resilience polyurethane foam.

7. The low-density high-resilience polyurethane foam material according to claim 1 is used in mattresses, furniture, chairs and home furnishings.