High-strength branched-chain PBAT and preparation method thereof
By introducing branched structures on the PBAT molecular chain, the esterification reaction of terephthalic acid, succinic acid and adipic acid is solved, the problem of poor PBAT performance is significantly improved, and its mechanical strength and tensile strength are achieved. Optimize the performance of polyethylene.
Patent Information
- Application Number
- CN202310583743.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-23
AI Technical Summary
There is a big gap between PBAT and polyethylene in terms of performance, especially in terms of blow molding and tensile strength, it is difficult to completely replace non-degradable materials, and small molecules are lost and poor compatibility occurs during the addition of fillers or blending. question.
By introducing branched chain structures on the PBAT molecular chains through an esterification reaction, the esterification reaction of terephthalic acid, succinic acid and adipic acid are used, and the PBAT molecular chains are modified by branching agents of different chain lengths and structures. Optimize its mechanical properties.
It significantly improves the mechanical strength and tensile strength of PBAT, improves its molecular structure, and achieves better mechanical properties and degradation properties.
Smart Images

Figure CN119019654A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a high-strength branched-chain PBAT and a preparation method thereof, belonging to the technical field of polymer synthesis. Background Art
[0002] With the development of society, degradable materials are highly favored. PBAT is a thermoplastic fully biodegradable material. It is the most promising substitute for polyethylene and one of the important ways to solve polyethylene pollution. In particular, the role of PBAT in replacing polyethylene agricultural film has made the research of PBAT a focus. If PBAT is to fully replace non-degradable products such as polyethylene, PBAT currently lacks in performance. For example, the blow molding processing performance is not as good as polyethylene, and the tensile strength is also far behind polyethylene. If PBAT is to fully replace polyethylene, it is necessary to optimize the performance of PBAT.
[0003] Researchers have tried to improve the performance of PBAT by adding fillers, chain extenders or blending with other polymer materials. However, during use, small molecules have been lost, migrated or have poor compatibility with other polymer materials. Long-term studies have shown that molecular structure determines the performance of polymer materials. Modifying the molecular structure of PBAT is the most likely and effective way to improve the performance of PBAT. Grafting branched small molecules on the PBAT molecular chain in the form of chemical bonds can reconstruct and modify the PBAT molecular chain. Since different modifiers have different modification properties on polymer structures, the selection of modifiers has become a top priority. Summary of the invention
[0004] In order to solve the above problems, the object of the present invention is to provide a high-strength branched PBAT and a preparation method thereof. The high-strength branched PBAT prepared by the preparation method has high mechanical strength, excellent tensile strength and elongation at break, and the reaction is relatively complete.
[0005] In order to achieve the above object, the present invention provides a method for preparing a high-strength branched PBAT, which comprises the following steps: firstly subjecting terephthalic acid and succinic acid to an esterification reaction, and then adding adipic acid to an esterification reaction.
[0006] According to a specific embodiment of the present invention, preferably, the above preparation method comprises the following steps:
[0007] (1) First step esterification reaction: terephthalic acid and butanediol are mixed, and after the catalyst is added for the first time, the first step esterification reaction is carried out at 210-240° C. (preferably 215° C.) under a protective gas atmosphere;
[0008] (2) Second step esterification reaction: After the first step esterification reaction is completed, the temperature is lowered to below 140° C., adipic acid is added and the catalyst is added for the second time, and the second step esterification reaction is carried out at 150-190° C. (preferably 150° C.);
[0009] (3) Pre-polycondensation reaction: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C, and a catalyst is added for the third time to carry out a polycondensation reaction under the conditions of below 100 Pa and 220-260°C (preferably 230°C). After the reaction is completed, the high-strength branched PBAT is obtained;
[0010] When the boiling point of the branching agent is ≥200°C, the branching agent is added in step (1); when the boiling point of the branching agent is ≤200°C, the branching agent is added in step (2);
[0011] The branching agent includes diols and / or 1,2-epoxy compounds; more preferably, the diol includes one or a combination of two or more of 1,2-propylene glycol, 1,2-butylene glycol, 1,2-hexanediol, 7-octene-1,2-diol, butene glycol, 2,2-diisobutyl-1,3-propylene glycol, 1,2-octanediol, 1,2-decanediol, 1,2-dodecanediol, 1,2-tetradecanediol, and 2-butyl-2-ethyl-1,3-propylene glycol; the 1,2-epoxy compounds include one or a combination of two or more of 1,2-butylene oxide, 1,2-epoxyhexane, 1,2-epoxyoctane, butyl glycidyl ether, octyl glycidyl ether, tert-butyl glycidyl ether, and allyl glycidyl ether.
[0012] According to a specific embodiment of the present invention, preferably, in step (1), the molar ratio of titanium in the catalyst added for the first time to the sum of the molar amounts of terephthalic acid and adipic acid is 1:500-1:10000.
[0013] According to a specific embodiment of the present invention, preferably, in step (1), the molar ratio of the terephthalic acid to the butanediol is 45:100-45:150.
[0014] According to a specific embodiment of the present invention, preferably, in step (1), the butanediol is 1,4-butanediol.
[0015] According to a specific embodiment of the present invention, preferably, the branching agent is one or a combination of two or more of 1,2-hexanediol, 1,2-octane oxide, and butyl glycidyl ether.
[0016] According to a specific embodiment of the present invention, preferably, in step (2), the molar ratio of titanium in the catalyst added for the second time to the sum of the molar amounts of terephthalic acid and adipic acid is 1:500-1:10000.
[0017] According to a specific embodiment of the present invention, preferably, in step (2), the molar ratio of the adipic acid to the terephthalic acid is 70:30-48:52.
[0018] According to a specific embodiment of the present invention, preferably, in step (3), the molar ratio of titanium in the catalyst added for the third time to the sum of the molar amounts of terephthalic acid and adipic acid is 1:500-1:10000.
[0019] According to a specific embodiment of the present invention, preferably, the catalyst added in step (1) to step (3) is a multi-nuclear catalyst, preferably including a titanium-silicon-zinc multi-nuclear catalyst and / or a titanium-silicon-aluminum multi-nuclear catalyst.
[0020] According to a specific embodiment of the present invention, preferably, the catalyst added in steps (1) to (3) is the titanium silicon composite multi-nuclear catalyst described in invention patent application 202210966547.1.
[0021] The present invention reconstructs the molecular chain of PBAT in a novel form by reacting the modified branching agent to the molecular main chain of PBAT, and prepares PBAT with different straight-chain molecular structures, thereby improving the performance of PBAT by controlling the molecular architecture of PBAT. The branching agent used in the present invention is preferably a diol and / or a 1,2-epoxy compound (i.e., a compound containing a 1,2-epoxy group). More preferably, the diol includes one or more combinations of 1,2-propylene glycol, 1,2-butylene glycol, 1,2-hexanediol, 7-octene-1,2-diol, butene glycol, and 2,2-diisobutyl-1,3-propylene glycol; 1,2-epoxy compounds include one or more combinations of 1,2-butylene oxide, 1,2-epoxyhexane, 1,2-epoxyoctane, butyl glycidyl ether, octyl glycidyl ether, tert-butyl glycidyl ether, and allyl glycidyl ether. Among them, 1,2-epoxyhexane and butyl glycidyl ether are branching agents with a boiling point below 200°C, and the other branching agents listed are branching agents with a boiling point above 200°C.
[0022] According to a specific embodiment of the present invention, preferably, the molar ratio of the branching agent to the sum of the molar amounts of terephthalic acid and adipic acid is 0.5:100-15:100.
[0023] According to a specific embodiment of the present invention, the above preparation method comprises the following specific steps:
[0024] (1) Weighing and mixing of samples: terephthalic acid and butanediol are weighed in a certain proportion and added into a three-necked flask, and a certain proportion of branching agents with different chain lengths or structures are added, and then a certain proportion of catalyst is added (if the boiling point of the branching agent is lower than 200° C., no branching agent is added in this step), and the three-necked flask is placed in an oil bath preheated to 50° C.;
[0025] (2) First step esterification reaction: nitrogen is continuously introduced into the three-necked flask in step (1), the stirring device is turned on, and after setting a suitable stirring rate, the temperature of the oil bath pot is raised to about 190°C and kept warm for a certain time, and then the temperature is raised to 210-240°C (for example, 215°C) until the first step esterification reaction is completed (the temperature is raised to 190°C and kept warm for a certain time means: keeping warm at 190°C for more than 20 minutes, and then directly raising the temperature to 210-240°C (for example, 215°C) until the first step esterification reaction is completed. When the predetermined water output is reached, it indicates that the first step esterification reaction is completed); the molar ratio of the branching agent to the carboxylic acid ranges from M to 支化剂 :M 羧酸 =0.5:100-15:100, the molar ratio of catalyst to carboxylic acid is in the range of M 催化剂 :M 羧酸 =1:10000-1:500, the molar ratio of terephthalic acid to butanediol is in the range of M 对苯二甲酸 :M 丁二醇 =45:100-45:150, where M 羧酸 It is the sum of the molar amounts of terephthalic acid and adipic acid; when the content of branching agent and catalyst is too high, the color of the product will be significantly deepened, changing from the original white or light yellow to dark red or yellow-red; when it is too low, the effect of branching reaction cannot be achieved, and the performance cannot be improved compared with the unbranched product; and when the content of catalyst is too low, the reaction time will be greatly increased, the reaction cannot be completely catalyzed, the reaction is insufficient, and the performance of the material cannot be improved. When the content of terephthalic acid is too high, it will affect the degradation performance to a certain extent. When the content of terephthalic acid is too low (calculated as 100% by the sum of the molar amounts of terephthalic acid and adipic acid, it is less than 30%), the melting point of the synthesized sample is lower than 60°C, affecting its performance for summer use. Therefore, the molar ratio of the present invention is used for mixing, which can ensure that the obtained branched PBAT has excellent mechanical properties; in addition, during the reaction process, the temperature is increased from 190°C to the esterification temperature range at a rate of 5-20°C / 30min to effectively inhibit the occurrence of side reactions and the loss of components involved in the reaction;
[0026] (3) Second step esterification reaction: After the first step esterification is completed, the temperature of the oil bath is lowered to below 140°C, the catalyst is added to the three-necked flask for the second time, and a certain proportion of adipic acid is added (if the boiling point of the branching agent is ≤200°C, the branching agent is added in this step), and then the temperature of the oil bath is raised to a certain temperature until the second step esterification reaction is completed (the reaction temperature is controlled below the boiling point of the added branching agent); lowering the temperature to below 140°C can effectively prevent the hydrolysis of the catalyst and the loss of catalyst efficacy caused by the catalyst being carried away by nitrogen after atomization;
[0027] (4) Pre-polycondensation reaction: After the second step esterification reaction is completed, the temperature is lowered to below 140°C again, and the catalyst is added to the three-necked flask for the third time. After the internal pressure of the three-necked flask is pumped down to below 100 Pa, the temperature of the oil bath is raised to 220-260°C (e.g., 230°C) to carry out polycondensation reaction until the polycondensation reaction is completed.
[0028] The present invention also provides a high-strength branched PBAT prepared by the above preparation method.
[0029] According to a specific embodiment of the present invention, preferably, the branching degree of the high-strength branched PBAT is 0.5-15%, preferably 2-6%.
[0030] According to a specific embodiment of the present invention, preferably, the branch length of the high-strength branched PBAT is 2-10 carbon atoms, more preferably 2-6 carbon atoms.
[0031] The present invention uses monomers of different lengths and structures as modifiers of the PBAT straight chain to branch and entangle the straight chain structure of PBAT, construct PBAT molecular chains with different molecular structures and different branching degrees, thereby improving the performance of PBAT by controlling the PBAT molecular structure, which has the following beneficial effects:
[0032] (1) The high-strength branched PBAT prepared by using branching agents of different chain lengths or different structures described in the present invention can effectively improve the mechanical strength of PBAT through the effect of the branched chains in the PBAT molecular structure.
[0033] (2) The high-strength branched PBAT prepared by the branching agents of different chain lengths or different structures in the present invention has different effects on improving the performance of PBAT due to the different branch lengths and structures of the branching agents. The molecular structure of PBAT can be designed according to different improvement effects.
[0034] (3) In the preparation method of the present invention, the first step of the esterification reaction is to first react terephthalic acid with butanediol, and then add adipic acid to carry out the second step reaction, which can effectively improve the reaction degree of terephthalic acid. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a process flow chart of the PBAT synthesis process of the present invention;
[0036] Figure 2 The results of esterification after different addition orders are shown; Figure 2 a in the figure shows a white milky liquid obtained after 6 hours of esterification reaction in which adipic acid is added first and then terephthalic acid; Figure 2 b is a photo of a clear liquid obtained after esterification reaction for 2 hours after adding terephthalic acid first and then adipic acid;
[0037] Figure 3 The results of adding catalyst at different temperatures are shown in the figure; Figure 3 When a is 160℃, the catalyst is added and the catalyst atomizes due to hydrolysis; Figure 3 Figure b shows that when the catalyst is added at a temperature below 140°C, no atomization due to hydrolysis occurs;
[0038] Figure 4 The tensile properties of branched PBAT and pure PBAT (unbranched) in Example 1, Example 2, and Example 3 are compared;
[0039] Figure 5 The figure shows the mechanical properties of PBAT after branching with different branching degrees and different branch chain lengths; Figure 5 Figure a is a graph of mechanical properties of PBAT with different branching degrees; Figure 5 Figure b is a graph of mechanical properties of PBAT with different branch chain lengths;
[0040] Figure 6 The intrinsic viscosity and melt index result diagram of the branched PBAT and pure PBAT of Example 1, Example 2 and Example 3;
[0041] Figure 7 This is a sample photo when the catalyst and branching agent content is too high;
[0042] Figure 8 This is a diagram of the mechanical properties of multi-functional monomer branched PBAT. DETAILED DESCRIPTION
[0043] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0044] The catalysts used in the following examples and comparative examples are all titanium composite multi-nuclear catalysts recorded in the invention patent application 202210966547.1, wherein the titanium silicon zinc multi-nuclear catalyst is the product of Example 2 in the invention patent application 202210966547.1, and the titanium silicon aluminum multi-nuclear catalyst is the product of Example 9 in the invention patent application 202210966547.1. The catalyst preparation method is: first, titanate, co-catalyst and ligand 1 are added to diol, mixed to form a homogeneous solution A; then the organosilicon source is mixed with ethanol and acidic deionized water, and the organosilicon source is pre-hydrolyzed to form a solution B; then solution B is slowly dripped into solution A, and then the reaction system is removed from the low-boiling point component to obtain solution C; finally, ligand 2 is dripped into solution C and stirred evenly to obtain a liquid titanium silicon composite multi-nuclear catalyst; the molar ratio of the ligand 2 to the Ti atom in solution C is (0-3): 1. The co-catalyst is selected from at least one of triisopropyl aluminate, aluminum acetylacetonate, tribenzyl aluminate, zinc acetylacetonate, magnesium acetylacetonate and neodymium acetylacetonate; the ligand 1 and ligand 2 are independently selected from at least one of acetylacetone, 2,2'-bipyridine, acetic acid, L-lactic acid, D-lactic acid and tartaric acid.
[0045] The preparation method of the titanium-silicon-zinc multi-nuclear catalyst used below comprises the following steps:
[0046] (1) 0.05 mol of tetrabutyl titanate, 0.005 mol of zinc acetylacetonate and 0.1 mol of L-lactic acid were added dropwise to 1 mol of 1,4-butanediol and stirred thoroughly until a homogeneous solution A was formed;
[0047] (2) 0.02 mol of tetraethyl silicate, 0.15 mol of ethanol, and 0.08 mol of acidic deionized water were uniformly mixed and stirred at room temperature for 12 h to form solution B;
[0048] (3) Solution B was slowly dripped into Solution A and stirred rapidly to be uniform, and then the resulting solution was reacted at a pressure range of 150 Pa and a temperature of 80° C. for 3 h to remove low-boiling point components to obtain Solution C;
[0049] (4) 0.1 mol of acetylacetone was added dropwise to solution C and the mixture was stirred rapidly to obtain a liquid titanium-silicon composite multi-nuclear catalyst containing 2.12 wt % of titanium.
[0050] The preparation method of the titanium-silicon-aluminum multi-nuclear catalyst used below comprises the following steps:
[0051] (1) 0.05 mol of isopropyl titanate, 0.005 mol of aluminum acetylacetonate and 0.05 mol of D-lactic acid were added dropwise to 1 mol of 1,4-butanediol and stirred thoroughly until a homogeneous solution A was formed;
[0052] (2) 0.01 mol of tetraethyl silicate, 0.07 mol of ethanol, and 0.04 mol of deionized water were uniformly mixed and stirred at room temperature for 12 h to form solution B;
[0053] (3) Solution B was slowly dripped into Solution A and stirred rapidly to be uniform, and then the resulting solution was reacted at a pressure range of 120 Pa and a temperature of 80° C. for 3 h to remove low-boiling point components to obtain Solution C;
[0054] (4) Add 0.12 mol of acetylacetone and 0.005 mol of tartaric acid to solution C and stir rapidly to obtain a liquid titanium-silicon composite multi-nuclear catalyst containing 2.08 wt% of titanium.
[0055] Example 1
[0056] This embodiment provides a high-strength branched PBAT, and its preparation method includes the following steps, the process is as follows: Figure 1 As shown:
[0057] (1) Weighing and mixing of samples: 18.675 g of terephthalic acid and 26.1 g of 1,4-butanediol were weighed and added to a three-necked flask, and 1.18 g of 1,2-hexanediol was added. Then, 30 μL of titanium silicon zinc multinuclear catalyst was added and the three-necked flask was placed in an oil bath preheated to 50° C.;
[0058] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 260 r / min, the temperature of the oil bath was raised to 190° C. and kept at that temperature for 20 min, then the temperature of the oil bath was gradually raised to 215° C. at a rate of 5° C. every 20 min, and kept at 215° C. until the first step esterification reaction was completed;
[0059] (3) Second step esterification reaction: After the first step esterification is completed, the temperature of the oil bath is lowered to below 140°C, and 20 μL of titanium-silicon-zinc multinuclear catalyst is added to the three-necked flask for the second time. At this time, the catalyst does not atomize (such as Figure 3 b), and after adding 20.06 g of adipic acid, the bath temperature was raised to 185°C and reacted for 2 hours. The second step of esterification was completed and the melt was clear and transparent, as shown in FIG. Figure 2 As shown in b;
[0060] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, and 36 μL of titanium-silicon-zinc multi-nuclear catalyst is added to the three-necked flask for the third time. After the pressure in the three-necked flask is pumped down to below 100 Pa, the temperature of the oil bath is raised to 230°C for polycondensation reaction until the polycondensation reaction is completed to obtain branched PBAT;
[0061] (5) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain branched PBAT.
[0062] Example 2
[0063] This embodiment provides a high-strength branched PBAT, and the preparation method thereof comprises the following steps:
[0064] (1) Weighing and mixing of samples: 18.675 g of terephthalic acid and 26.1 g of 1,4-butanediol were weighed and added into a three-necked flask, and 30 μL of titanium silicon zinc multi-nuclear catalyst was added, and the three-necked flask was placed in an oil bath preheated to 50°C;
[0065] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 260 r / min, the temperature of the oil bath was raised to 190° C. and kept at that temperature for 20 min, then the temperature of the oil bath was gradually raised to 215° C. at a rate of 5° C. every 20 min, and kept at 215° C. until the first step esterification reaction was completed;
[0066] (3) Second step esterification reaction: After the first step esterification reaction is completed, the temperature of the oil bath is lowered to below 140°C, and 20 μL of titanium silicon zinc multi-nuclear catalyst is added to the three-necked flask for the second time. At this time, the catalyst does not atomize, and after adding 1.3 g of butyl glycidyl ether, 19.27 g of adipic acid is added, and the temperature of the bath is raised to 185°C until the second step esterification reaction is completed, and the melt is clear and transparent;
[0067] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, and 36 μL of titanium-silicon-zinc multi-nuclear catalyst is added to the three-necked flask for the third time. After the pressure in the three-necked flask is pumped down to below 100 Pa, the temperature of the oil bath is raised to 230°C for polycondensation reaction until the polycondensation reaction is completed to obtain branched PBAT;
[0068] (5) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain branched PBAT.
[0069] Example 3
[0070] This embodiment provides a high-strength branched PBAT, and the preparation method thereof comprises the following steps:
[0071] (1) Weighing and mixing of samples: 18.675 g of terephthalic acid and 26.1 g of 1,4-butanediol were weighed and added into a three-necked flask, and 30 μL of titanium-silicon-aluminum multi-nuclear catalyst was added, and the three-necked flask was placed in an oil bath preheated to 50°C;
[0072] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 260 r / min, the temperature of the oil bath was raised to 190° C. and kept at that temperature for 20 min, then the temperature of the oil bath was gradually raised to 215° C. at a rate of 5° C. every 20 min, and kept at 215° C. until the first step esterification reaction was completed;
[0073] (3) Second step esterification reaction: After the first step esterification is completed, the temperature of the oil bath is lowered to below 140°C, and 20 μL of titanium-silicon-aluminum multi-nuclear catalyst is added to the three-necked flask for the second time. At this time, the catalyst does not atomize, and 1.28 g of 1,2-epoxyoctane is added. Subsequently, 20.06 g of adipic acid is added, and the temperature of the bath is raised to 185°C until the second step esterification reaction is completed, and the melt is clear and transparent;
[0074] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, and 36 μL of titanium-silicon-aluminum multi-nuclear catalyst is added to the three-necked flask for the third time. After the pressure in the three-necked flask is pumped down to below 100 Pa, the temperature of the oil bath is raised to 230°C for polycondensation reaction until the polycondensation reaction is completed to obtain branched PBAT;
[0075] (5) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain branched PBAT.
[0076] Comparative Example 1
[0077] This comparative example provides a branched PBAT, and its preparation method comprises the following steps:
[0078] (1) Weighing and mixing of samples: 19.27 g of adipic acid and 26.1 g of 1,4-butanediol were weighed and added into a three-necked flask, and 60 μL of titanium-silicon-aluminum multi-nuclear catalyst was added, and the three-necked flask was placed in an oil bath preheated to 50° C.;
[0079] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 260 r / min, the oil bath was heated to 160° C. and kept warm for 20 min, then the temperature of the oil bath was gradually increased to 185° C. at a rate of 5° C. every 20 min, and the first step esterification reaction was completed at 185° C. The esterification time was 2 h, and a clear transparent liquid was obtained;
[0080] (3) Second step esterification reaction: After the first step esterification was completed, the temperature of the oil bath was lowered to below 140°C, and 35 μL of titanium-silicon-aluminum multi-nuclear catalyst was added to the three-necked flask for the second time. At this time, the catalyst did not atomize, and 1.3 g of butyl glycidyl ether was added. After adding 18.675 g of terephthalic acid, the temperature of the bath was raised to 215°C, and the esterification reaction was carried out for more than 6 hours. No clear and transparent melt was obtained. Figure 2 As shown in a;
[0081] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, and 72 μL of titanium-silicon-aluminum multi-nuclear catalyst is added to the three-necked flask for the third time. After the pressure in the three-necked flask is pumped down to below 100 Pa, the temperature of the oil bath is raised to 230°C for polycondensation reaction until the polycondensation reaction is completed to obtain branched PBAT;
[0082] (5) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain branched PBAT.
[0083] Comparative Example 2
[0084] This comparative example provides a branched PBAT, and its preparation method comprises the following steps:
[0085] (1) Weighing and mixing of samples: 18.675 g of terephthalic acid and 26.1 g of 1,4-butanediol were weighed and added into a three-necked flask, and 50 μL of titanium silicon zinc multi-nuclear catalyst was added, and the three-necked flask was placed in an oil bath preheated to 50°C;
[0086] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 260 r / min, the temperature of the oil bath was raised to 190° C. and kept at that temperature for 20 min, then the temperature of the oil bath was gradually raised to 215° C. at a rate of 5° C. every 20 min, and kept at 215° C. until the first step esterification reaction was completed;
[0087] (3) Second step esterification reaction: After the first step esterification was completed, the temperature of the oil bath was lowered to 160°C, and 30 μL of titanium-silicon-zinc multinuclear catalyst was added to the three-necked flask for the second time. At this time, the catalyst was atomized due to the high temperature (such as Figure 3 As shown in a), part of the catalyst was lost due to mist or deactivated by hydrolysis; then 1.3 g of butyl glycidyl ether was added, and then 19.27 g of adipic acid was added, and the bath temperature was raised to 185°C until the second step esterification reaction was completed;
[0088] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, 60 μL of titanium-silicon-zinc multi-nuclear catalyst is added to the three-necked flask for the third time, and the pressure in the three-necked flask is pumped below 100 Pa, and the temperature of the oil bath is raised to 230°C for polycondensation reaction until the polycondensation reaction is completed to obtain branched PBAT;
[0089] (5) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain branched PBAT.
[0090] Comparative Example 3
[0091] This comparative example provides a branched PBAT, and its preparation method comprises the following steps:
[0092] (1) Weighing and mixing of samples: 18.675 g of terephthalic acid and 26.1 g of 1,4-butanediol were weighed and added into a three-necked flask, and 150 μL of titanium silicon zinc multi-nuclear catalyst was added, and the three-necked flask was placed in an oil bath preheated to 50°C;
[0093] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 260 r / min, the temperature of the oil bath was raised to 190° C. and kept at that temperature for 20 min, then the temperature of the oil bath was gradually raised to 215° C. at a rate of 5° C. every 20 min, and kept at 215° C. until the first step esterification reaction was completed;
[0094] (3) Second step esterification reaction: After the first step esterification is completed, the temperature of the oil bath is lowered to below 140°C, and 100 μL of titanium silicon zinc multi-nuclear catalyst is added to the three-necked flask for the second time. At this time, the catalyst does not atomize, and 4.425 g of 1,2-hexanediol is added, followed by 20.06 g of adipic acid. The temperature of the bath is raised to 185°C until the second step esterification reaction is completed, and the melt is clear and transparent;
[0095] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, and 100 μL of titanium-silicon-zinc multi-nuclear catalyst is added to the three-necked flask for the third time. After the pressure in the three-necked flask is pumped below 100 Pa, the temperature of the oil bath is raised to 230°C for polycondensation reaction. During the polycondensation process, the melt turns yellow-red until the polycondensation reaction is completed, and the branched PBAT is obtained;
[0096] (5) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain a yellow-red branched PBAT, such as Figure 7 shown.
[0097] Comparative Example 4
[0098] This comparative example provides a branched PBAT, the preparation method of which is the same as that of Example 1, but the amount of terephthalic acid added is 30%, that is, the molar ratio of terephthalic acid: adipic acid = 3:7. The melting temperature of the obtained branched PBAT is 52°C, which is lower than 60°C, affecting its performance in summer use.
[0099] evaluate:
[0100] 1. The mechanical tensile properties, melt index and intrinsic viscosity of the branched structure modified PBAT prepared in Examples 1, 2 and 3 were evaluated. The PBAT used in the following tests, unless otherwise specified, was prepared according to the preparation process of Example 1, except that no branching agent was added during preparation, the amount of branching agent added was different, and branching agents with different carbon atom numbers were added.
[0101] 2. Test methods and conclusions:
[0102] (1) Tensile performance test
[0103] The obtained branched PBAT was dried in an oven at 60°C and molded at 160°C. It was pressed into standard specimens according to GB / T1040.2-2006 and the tensile strength was tested at room temperature with a tensile speed of 50 mm / min using a universal testing machine Instron 5500R. The tensile results are shown in Figure 4 , Figure 5 ;in, Figure 4 In the figure, based on the vertical part on the right, the curves from left to right are PBAT (i.e., unbranched PBAT), Example 1, Example 3, and Example 2; Figure 5 3, 4, 5, 6, and 7 represent branching agents of 3%, 4%, 5%, 6%, and 7% of the total molar amount of the added acid, respectively; PBAT represents unbranched PBAT; 2C-10C represent branching agents of the same structure whose carbon chain lengths that do not participate in the reaction are 2 carbon atoms to 10 carbon atoms, respectively (the branching agents are 1,2-butanediol, 1,2-hexanediol, 1,2-octanediol, 1,2-decanediol, and 1,2-dodecanediol, respectively); wherein, Figure 5 The vertical part on the right is used as the reference for a. From left to right, the curves are 7, PBAT, 4, 3, 5, and 6. Figure 5 The vertical part on the right is taken as the standard in middle b, and the curves from left to right are 4C, 2C, 8C, 10C, and 6C. It can be seen from the figure that under the same conditions, the tensile strength and elongation at break of branched PBAT are significantly improved compared with unbranched PBAT.
[0104] (2) Melt index test
[0105] The obtained branched PBAT was dried in an oven at 60°C and cut into small particles. The melt index test was performed at 190°C and 2.16 kg. The results are as follows: Figure 6 As can be seen from the figure, under the same conditions, compared with the unbranched PBAT (the preparation process is the same as that of Example 1, and the PBAT obtained without adding any branching agent), the melt index of the branched PBAT is significantly reduced, and the melt index of different branched structures under the same conditions is quite different.
[0106] (3) Intrinsic viscosity performance test
[0107] The obtained branched PBAT was dried in an oven at 60°C, dissolved in a solvent mixed with phenol and 1,1,2,2-tetrachloroethane, wherein the mass ratio of phenol to 1,1,2,2-tetrachloroethane was 1:1, dissolved into a solution with a mass fraction of 0.5%, tested using an Ubbelohde viscometer, and finally calculated to obtain the intrinsic viscosity. The results are shown in Figure 6 As can be seen from the figure, under the same conditions, compared with the unbranched PBAT, the intrinsic viscosity of the branched PBAT is improved, the result is consistent with the melt index, and different branched structures have different intrinsic viscosities under the same conditions.
[0108] 3. According to GB / T1040.2-2006, PBAT branched with different branching agents was pressed into standard specimens, and mechanical properties were tested according to the test method in GB / T1040.2-2006. The preparation method of the PBAT involved below is the same as that of Example 1, except that different branching agents were added and the amount of branching agents added was different;
[0109] Results Figure 8 , Figure 8 In the a, 2-OH to 6-OH represent PBAT prepared from branched monomers with dihydroxy functional groups to hexahydroxy functional groups (the branched monomers represented by 2-OH to 6-OH are 2-butyl-1,3-propanediol, trimethylolpropane, pentaerythritol, and dipentaerythritol, respectively), 0.5%, 0.1%, 1%, and 0.2% represent that the branching agent is 0.5%, 0.1%, 1%, and 0.2% of the total molar amount of the added acid, Figure 8 In the middle a, the vertical part on the right is taken as the standard. From left to right, the curves are 4-OH-0.2%, 3-OH-1%, 3-OH-0.5%, 4-OH-0.1%, 6-OH, and 2-OH.
[0110] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0111] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a high-strength branched PBAT, comprising the following steps: First, terephthalic acid and succinic acid are subjected to esterification reaction, and then adipic acid is added to carry out esterification reaction.
2. The preparation method according to claim 1, wherein The preparation method comprises the following steps: (1) First step esterification reaction: terephthalic acid and butanediol are mixed, and after the catalyst is added for the first time, the first step esterification reaction is carried out at 210-240° C. under a protective gas atmosphere; (2) Second step esterification reaction: After the first step esterification reaction is completed, the temperature is lowered to below 140° C., adipic acid is added and the catalyst is added for the second time, and the second step esterification reaction is carried out at 150-190° C.; (3) Pre-polycondensation reaction: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C, and a catalyst is added for the third time to carry out a polycondensation reaction under the conditions of below 100 Pa and 220-260°C. After the reaction is completed, the high-strength branched PBAT is obtained; When the boiling point of the branching agent is ≥200°C, the branching agent is added in step (1); when the boiling point of the branching agent is ≤200°C, the branching agent is added in step (2); The branching agent includes diols and / or 1,2-epoxy compounds; Preferably, the diol includes one or a combination of two or more of 1,2-propylene glycol, 1,2-butylene glycol, 1,2-hexanediol, 7-octene-1,2-diol, butene glycol, 2,2-diisobutyl-1,3-propylene glycol, 1,2-octanediol, 1,2-decanediol, 1,2-dodecanediol, 1,2-tetradecanediol, and 2-butyl-2-ethyl-1,3-propylene glycol; Preferably, the 1,2-epoxy compound includes one or a combination of two or more of 1,2-butylene oxide, 1,2-hexylene oxide, 1,2-octane oxide, butyl glycidyl ether, octyl glycidyl ether, tert-butyl glycidyl ether, and allyl glycidyl ether.
3. The preparation method according to claim 2, wherein In step (1), the molar ratio of titanium in the catalyst added for the first time to the sum of the molar amounts of terephthalic acid and adipic acid is 1:500-1:10000; Preferably, in step (1), the molar ratio of the terephthalic acid to the butanediol is 45:100-45:
150.
4. The preparation method according to claim 2, wherein In step (2), the molar ratio of titanium in the catalyst added for the second time to the sum of the molar amounts of terephthalic acid and adipic acid is 1:500-1:10000; Preferably, in step (2), the molar ratio of the adipic acid to the terephthalic acid is 70:30-48:
52.
5. The preparation method according to claim 2, wherein: In step (3), the molar ratio of titanium in the catalyst added for the third time to the sum of the molar amounts of terephthalic acid and adipic acid is 1:500-1:10000.
6. The preparation method according to claim 2, wherein: The catalyst added in step (1) to step (3) is a multi-nuclear catalyst, preferably comprising a titanium-silicon-zinc multi-nuclear catalyst and / or a titanium-silicon-aluminum multi-nuclear catalyst; Preferably, the catalyst added in steps (1) to (3) is the titanium-silicon composite multi-nuclear catalyst described in invention patent application 202210966547.
1.
7. The preparation method according to claim 2, wherein: The molar ratio of the branching agent to the sum of the molar amounts of terephthalic acid and adipic acid is 0.5:100-15:
100.
8. A high-strength branched PBAT prepared by the preparation method according to any one of claims 1 to 7.
9. The high-strength branched PBAT according to claim 8, wherein: The branching degree of the high-strength branched PBAT is 0.5-15%, preferably 2-6%.
10. The high-strength branched PBAT according to claim 8, wherein: The branch length of the high-strength branched PBAT is 2-10 carbon atoms, more preferably 2-6 carbon atoms.
Citation Information
Patent Citations
Cladodified fat-aromatic copolyester and synthesis method thereof
CN104356372A
Copolymerized high-fluidity polyester master batch matrix material and preparation method thereof
CN109180918A
Process and apparatus for preparing biodegradable polyesters
CN110869413A
Biodegradable copolyester and preparation method thereof
CN111892701A
Branched hydrophobic biodegradable polyester as well as preparation method and application thereof
CN114716653A