Branched PBAT and preparation method thereof
By constructing branching points and functional sites in PBAT, the problems of poor blow molding processability and insufficient mechanical properties of films are solved, which significantly improves its mechanical properties and meets the application needs of polyethylene alternative materials.
Patent Information
- Application Number
- CN202310591542.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-23
AI Technical Summary
PBAT has poor blow molding processability and insufficient film mechanical properties, which limits its potential to replace polyethylene films in agricultural plastic films and packaging bags.
Branching is constructed by esterification of terephthalic acid and butylene glycol and adding adipic acid to conduct esterification, and branching agents with different structures or functions are grafted onto the main chain of PBAT in the form of a chemical reaction. Points and functional sites, prepare branched PBAT to improve its mechanical properties.
It effectively improves the processing performance and mechanical properties of PBAT, improves its application potential in agricultural plastic films and packaging bags, and meets the performance requirements for polyethylene alternative materials.
Smart Images

Figure CN119019655A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a branched PBAT and a preparation method thereof, belonging to the technical field of polymer synthesis. Background Art
[0002] Since the first synthesis of polyethylene, with the deepening of research, its performance has become increasingly excellent and has been applied to many aspects of life. With the development of society and the introduction of the concept of environmental friendliness, polyethylene is discarded in the environment after use due to its non-biodegradability, leading to serious environmental pollution problems. People are in urgent need of seeking a biodegradable material with performance comparable to polyethylene to meet the needs. Polybutylene adipate terephthalate (PBAT) is a fully biodegradable aliphatic-aromatic copolyester. As a fully biodegradable material, it has excellent performance and can be degraded quickly. It is the most potential and most likely environmentally friendly material to replace polyethylene. However, PBAT has some shortcomings that cannot be ignored, such as its blow molding processing performance is not as good as that of linear low-density polyethylene. In film applications, PBAT's tensile strength and modulus are also low, which to a certain extent limits its replacement of polyethylene film in the fields of agricultural mulch and packaging bags. Studies have found that the molecular structure of polymer materials has a crucial impact on their performance. Modifying or reconstructing the molecular chain structure of PBAT can effectively control the performance of PBAT. Therefore, in order to make PBAT meet the use requirements, modifiers are used to reconstruct and modify the PBAT molecular chain. The modifiers are connected to the main chain of the PBAT molecule through strong chemical bonds to functionalize the PBAT molecular chain, so as to achieve the purpose of regulating the performance of PBAT and giving it necessary functions. Summary of the invention
[0003] In order to solve the above-mentioned problems of poor blow molding processability and insufficient film mechanical properties of PBAT, the object of the present invention is to provide a branched PBAT and a preparation method thereof, which can effectively increase the branching degree of PBAT and prevent cross-linking of PBAT molecular chains. The obtained branched PBAT has good mechanical properties and the reaction is relatively complete.
[0004] In order to achieve the above object, the present invention provides a method for preparing branched PBAT, which comprises the following steps: firstly subjecting terephthalic acid and butanediol to an esterification reaction, and then adding adipic acid to carry out an esterification reaction.
[0005] According to a specific embodiment of the present invention, preferably, the above preparation method comprises the following steps:
[0006] (1) First step esterification reaction: terephthalic acid and butanediol are mixed, and after the catalyst is added for the first time, the first step esterification reaction is carried out at 200-240° C. (preferably 215° C.) under a protective gas atmosphere;
[0007] (2) Second step esterification reaction: After the first step esterification reaction is completed, the temperature is lowered to below 140° C., adipic acid is added and the catalyst is added for the second time, and the second step esterification reaction is carried out at 160-190° C. (preferably 185° C.);
[0008] (3) Pre-polycondensation reaction: After the second step esterification reaction is completed, the temperature is lowered to below 140°C, and a catalyst is added for the third time to carry out a polycondensation reaction under the conditions of below 100 Pa and 220-260°C. After the reaction is completed, the branched PBAT is obtained;
[0009] When the boiling point of the branching agent is ≥210°C, the branching agent is added in step (1); when the boiling point of the branching agent is ≤210°C, the branching agent is added in step (2);
[0010] The branching agent includes diester branching agents and / or dicarboxylic acid branching agents; more preferably, the diester branching agent includes one or a combination of two or more of diethyl n-butyl malonate, diethyl dibutyl malonate, dimethyl propyl malonate, dimethyl isobutyl-1,3-malonate, and diethyl diisobutyl malonate; the dicarboxylic acid branching agent includes one or a combination of two or more of butyl malonic acid, propyl malonic acid, propyl glutaric acid, and isobutyl malonic acid.
[0011] According to a specific embodiment of the present invention, preferably, in step (1), the molar ratio of titanium in the catalyst added for the first time to the sum of the molar amounts of terephthalic acid and adipic acid is 1:10000-3:1000.
[0012] According to a specific embodiment of the present invention, preferably, in step (1), the molar ratio of the terephthalic acid to the butanediol is 45:100-45:150.
[0013] According to a specific embodiment of the present invention, preferably, the butanediol is 1,4-butanediol and / or 1,2-butanediol.
[0014] According to a specific embodiment of the present invention, preferably, the branching agent is one or a combination of two or more of diethyl butyl malonate, butyl malonic acid, and dimethyl isobutyl malonate.
[0015] According to a specific embodiment of the present invention, preferably, in step (2), the molar ratio of the titanium in the catalyst added for the second time to the sum of the molar amounts of the terephthalic acid and the adipic acid is 1:10000-3:1000.
[0016] According to a specific embodiment of the present invention, preferably, in step (2), the molar ratio of the adipic acid to the terephthalic acid is 70:30-48:52.
[0017] According to a specific embodiment of the present invention, preferably, in step (3), the molar ratio of the titanium in the catalyst added for the third time to the sum of the molar amounts of the terephthalic acid and the adipic acid is 1:10000-6:1000.
[0018] According to a specific embodiment of the present invention, preferably, the catalyst added in step (1) to step (3) is a multi-nuclear catalyst, more preferably includes a titanium-silicon-zinc multi-nuclear catalyst and / or a titanium-silicon-aluminum multi-nuclear catalyst.
[0019] According to a specific embodiment of the present invention, preferably, the catalyst added in steps (1) to (3) is the titanium silicon composite multi-nuclear catalyst described in invention patent application 202210966547.1.
[0020] The present invention grafts branching agents of different structures or functions onto the main chain of PBAT in the form of chemical reaction, constructs the main chain branching points and functional sites of PBAT in a novel form of connecting the branching agent to the main chain, and prepares PBAT containing branches of different structures, thereby improving the performance of PBAT by controlling the molecular architecture of PBAT. The branching agent used in the present invention is preferably a diester branching agent and / or a dicarboxylic acid branching agent; more preferably, the diester branching agent includes one or a combination of two or more of n-butyl diethyl malonate, dibutyl diethyl malonate, propyl dimethyl malonate, isobutyl-1,3-dimethyl malonate, and diisobutyl diethyl malonate; the dicarboxylic acid branching agent includes one or a combination of two or more of butyl malonic acid, propyl malonic acid, propyl glutaric acid, and isobutyl malonic acid. Among them, isobutyl-1,3-dimethyl malonate is a branching agent having a boiling point lower than 215°C, and the other branching agents listed are branching agents having a boiling point higher than 215°C.
[0021] According to a specific embodiment of the present invention, preferably, the molar ratio of the branching agent to the sum of the molar amounts of the terephthalic acid and the adipic acid is 1:100-10:100.
[0022] According to a specific embodiment of the present invention, the above preparation method comprises the following specific steps:
[0023] (1) Weighing and mixing of samples: Weigh terephthalic acid and butanediol in a certain proportion and add them into a three-necked flask, and add a certain proportion of branching agent and catalyst. If the boiling point of the branching agent is ≤210°C, then no branching agent is added in this step, and the three-necked flask is placed in an oil bath preheated to 50°C. If the boiling point of the branching agent is low, when the branching agent is added in this step, the high temperature will cause the catalyst to vaporize and be lost.
[0024] (2) First step esterification reaction: nitrogen is continuously introduced into the three-necked flask in step (1), a stirring device is turned on, and after setting a suitable stirring rate, the temperature is rapidly raised to 190° C., and the esterification reaction is carried out at 190° C. for 20 min, and the temperature of the oil bath is gradually raised from 190° C. to between 200° C. and 240° C. (e.g., 215° C.) until the first step esterification reaction is completed (gradually raised to between 200° C. and 240° C. means: raising the temperature at a heating rate of 5-20° C. / 30 min-60 min, and keeping the temperature for more than 20 min after reaching the set temperature of 190° C., and then raising the temperature to between 200° C. and 240° C., and the temperature is kept within the range of 200° C. and 240° C. until the first step esterification reaction is completed, and when the predetermined water output is reached, it indicates that the first step esterification reaction is completed); the molar ratio of the branching agent to the carboxylic acid is in the range of M 支化剂 :M 羧酸 =1:100-10:100, the molar ratio of catalyst to carboxylic acid is in the range of M 催化剂 :M 羧酸 =1:10000-3:1000, the molar ratio of terephthalic acid to butanediol is in the range of M 对苯二甲酸 :M 丁二醇 =45:100-45:150, where M 羧酸 It is the sum of the molar amounts of terephthalic acid and adipic acid; terephthalic acid is added preferentially, which can make the reaction of terephthalic acid sufficient and the solution clear and transparent; and when the branching agent content is too high, the melt strength will be greatly reduced; if the catalyst content is too high, the melt will have a serious color reaction, and if it is too low, the esterification and polycondensation time will be greatly extended, and the performance of the material cannot be improved; when the terephthalic acid content is too high, it will have a certain degree of impact on the degradation performance. Taking the sum of the molar amounts of terephthalic acid and adipic acid as 100%, when the terephthalic acid content is less than 30%, the crystal structure of PBAT will change from PBT to PBA. At this time, BT as a defect hinders the integrity of the BT crystal, thereby reducing the crystallization rate and crystallinity of PBAT, and the mechanical properties also decrease to a certain extent, and the melting point is reduced to below 50°C, which has a serious impact on the safety of use. Thus, the molar ratio of the present invention is used for mixing, which can ensure that the obtained branched PBAT has excellent mechanical properties; in addition, gradually increasing the temperature can effectively inhibit the occurrence of side reactions and the loss of components involved in the reaction;
[0025] (3) Second step esterification reaction: After the first step esterification reaction is completed, the temperature of the oil bath is lowered to below 140°C, the catalyst is added to the three-necked flask for the second time, and a certain proportion of adipic acid is added (if the boiling point of the branching agent is ≤210°C, the branching agent is added in this step), and then the temperature of the oil bath is raised to a certain temperature (the reaction temperature is controlled below the boiling point of the added branching agent) until the second step esterification reaction is completed; lowering the temperature to below 140°C can effectively prevent the hydrolysis of the catalyst and the loss of catalyst efficacy caused by the catalyst being carried away by nitrogen after atomization;
[0026] (4) Pre-polycondensation reaction: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, and the catalyst is added to the three-necked flask for the third time. After the internal pressure of the three-necked flask is pumped down to below 100 Pa, the temperature of the oil bath is raised to between 220-260°C for polycondensation reaction until the polycondensation reaction is completed.
[0027] The present invention also provides a branched PBAT prepared by the above preparation method.
[0028] According to a specific embodiment of the present invention, preferably, the branching degree of the branched PBAT is 1%-10% (%, molar percentage), preferably 2%-6%.
[0029] According to a specific embodiment of the present invention, preferably, the branch chain length of the branched PBAT is 2-10 carbon atoms, more preferably 2-6 carbon atoms.
[0030] The preparation method of the present invention is to use branched monomers with different functional groups as branching agents to modify the straight chain of PBAT during the synthesis process of PBAT, construct the main chain branching points of PBAT in a novel form, and prepare PBAT with different branching degrees, which can effectively improve the branching degree of PBAT and prevent the cross-linking of PBAT molecular chains, thereby improving the performance of PBAT by controlling the PBAT molecular chain structure. The present invention has the following beneficial effects:
[0031] (1) The branched PBAT prepared by the branching agents with different functional group structures described in the present invention can effectively improve the processing performance of PBAT through the effect of the branch chain in the PBAT molecular structure;
[0032] (2) The branched PBAT prepared by the branching agents with different branched chains described in the present invention has different effects on improving the performance of PBAT due to the different branched chain structures of the branching agents. The molecular structure of PBAT can be designed according to different improvement effects and for different purposes;
[0033] (3) In the preparation method of the present invention, the first step of the esterification reaction is to first react terephthalic acid with butanediol, and then add adipic acid to carry out the second step reaction, which can effectively improve the reaction degree of terephthalic acid. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The PBAT synthesis flow chart of the present invention;
[0035] Figure 2 This is a new PBAT structure diagram constructed after the PBAT main chain is modified by the branching agent used in Example 1;
[0036] Figure 3 This is a comparison chart of the tensile properties of branched PBAT and pure PBAT (unbranched) in Example 1;
[0037] Figure 4 The intrinsic viscosity and melt index results of the branched PBAT of Examples 1-3 and the unbranched PBAT under the same conditions are shown in FIG.
[0038] Figure 5 The DSC diagram of the branched PBAT and the unbranched PBAT in Example 1 is shown in FIG. Figure 5 a in the middle is the crystallization curve, Figure 5 b in the middle is the melting curve;
[0039] Figure 6 This is the melting curve when the terephthalic acid content is 20%. DETAILED DESCRIPTION
[0040] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0041] The catalysts used in the following examples and comparative examples are all from the titanium composite multi-nuclear catalysts recorded in the invention patent application 202210966547.1, wherein the titanium silicon zinc multi-nuclear catalyst is the product of Example 2 in the invention patent application 202210966547.1, and the titanium silicon aluminum multi-nuclear catalyst is the product of Example 9 in the invention patent application 202210966547.1. The preparation method of the catalyst is: first, titanate, co-catalyst and ligand 1 are added to the diol, and mixed to form a homogeneous solution A; then the organosilicon source is mixed with ethanol and acidic deionized water, and the organosilicon source is pre-hydrolyzed to form a solution B; then solution B is slowly dripped into solution A, and then the reaction system is removed from the low-boiling point component to obtain solution C; finally, ligand 2 is dripped into solution C and stirred evenly to obtain a liquid titanium silicon composite multi-nuclear catalyst; the molar ratio of the ligand 2 to the Ti atom in solution C is (0-3): 1. The co-catalyst is selected from at least one of triisopropyl aluminate, aluminum acetylacetonate, tribenzyl aluminate, zinc acetylacetonate, magnesium acetylacetonate and neodymium acetylacetonate; the ligand 1 and ligand 2 are independently selected from at least one of acetylacetone, 2,2'-bipyridine, acetic acid, L-lactic acid, D-lactic acid and tartaric acid.
[0042] The preparation method of the titanium-silicon-zinc multi-nuclear catalyst used below comprises the following steps:
[0043] (1) 0.05 mol of tetrabutyl titanate, 0.005 mol of zinc acetylacetonate and 0.1 mol of L-lactic acid were added dropwise to 1 mol of 1,4-butanediol and stirred thoroughly until a homogeneous solution A was formed;
[0044] (2) 0.02 mol of tetraethyl silicate, 0.15 mol of ethanol, and 0.08 mol of acidic deionized water were uniformly mixed and stirred at room temperature for 12 h to form solution B;
[0045] (3) Solution B was slowly dripped into Solution A and stirred rapidly to be uniform, and then the resulting solution was reacted at a pressure range of 150 Pa and a temperature of 80° C. for 3 h to remove low-boiling point components to obtain Solution C;
[0046] (4) 0.1 mol of acetylacetone was added dropwise to solution C and the mixture was stirred rapidly to obtain a liquid titanium-silicon composite multi-nuclear catalyst containing 2.12 wt % of titanium.
[0047] The preparation method of the titanium-silicon-aluminum multi-nuclear catalyst used below comprises the following steps:
[0048] (1) 0.05 mol of isopropyl titanate, 0.005 mol of aluminum acetylacetonate and 0.05 mol of D-lactic acid were added dropwise to 1 mol of 1,4-butanediol and stirred thoroughly until a homogeneous solution A was formed;
[0049] (2) 0.01 mol of tetraethyl silicate, 0.07 mol of ethanol, and 0.04 mol of deionized water were uniformly mixed and stirred at room temperature for 12 h to form solution B;
[0050] (3) Solution B was slowly dripped into Solution A and stirred rapidly to be uniform, and then the resulting solution was reacted at a pressure range of 120 Pa and a temperature of 80° C. for 3 h to remove low-boiling point components to obtain Solution C;
[0051] (4) 0.12 mol of acetylacetone and 0.005 mol of tartaric acid were added dropwise to solution C and stirred rapidly to obtain a liquid titanium-silicon composite multi-nuclear catalyst containing 2.08 wt% of titanium.
[0052] Example 1
[0053] This embodiment provides a branched PBAT, and the preparation method thereof comprises the following steps, as shown in the process Figure 1 As shown:
[0054] (1) Weighing and mixing of samples: 17.93 g of terephthalic acid and 27 g of 1,4-butanediol were weighed and added into a three-necked flask, and 2.16 g of diethyl butylmalonate branching agent and 30 μL of titanium silicon zinc multi-nuclear catalyst were added, and the three-necked flask was placed in an oil bath preheated to 50° C.;
[0055] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 260 r / min, the oil bath was heated to 190° C. and kept at this temperature for 20 min, then the temperature of the oil bath was gradually increased to 215° C. at a rate of 10° C. every 20 min, and the esterification was carried out at 215° C. for 60 min. When the water output reached a predetermined value, the first step esterification reaction was completed;
[0056] (3) Second step esterification reaction: After the first step esterification is completed, the temperature of the oil bath is lowered to below 140°C, 20 μL of titanium silicon zinc multi-nuclear catalyst is added to the three-necked flask for the second time, and 19.27 g of adipic acid is added. The temperature of the bath is then raised to 185°C for esterification for 120 min. When the water output reaches the predetermined value, the second step esterification reaction is completed;
[0057] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, and 35 μL of titanium-silicon-zinc multi-nuclear catalyst is added to the three-necked flask for the third time. After the pressure in the three-necked flask is reduced to below 100 Pa, the temperature of the oil bath is raised to 230°C for polycondensation reaction for 1.5 hours to obtain branched PBAT;
[0058] (5) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain a branched PBAT having a structure as shown in Figure 2 shown.
[0059] Example 2
[0060] This embodiment provides a branched PBAT, and the preparation method thereof comprises the following steps:
[0061] (1) Weighing and mixing of samples: 17.93 g of terephthalic acid and 27 g of 1,4-butanediol were weighed and added into a three-necked flask, and 1.6 g of butylmalonic acid branching agent and 30 μL of titanium silicon zinc multi-nuclear catalyst were added, and the three-necked flask was placed in an oil bath preheated to 50° C.;
[0062] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 260 r / min, the oil bath was heated to 190° C. and kept at this temperature for 20 min, then the temperature of the oil bath was gradually increased to 215° C. at a rate of 15° C. every 20 min, and esterification was carried out at 215° C. for 60 min. When the water output reached a predetermined value, the first step esterification reaction was completed;
[0063] (3) Second step esterification reaction: After the first step esterification is completed, the temperature of the oil bath is lowered to below 140°C, 20 μL of titanium silicon zinc multi-nuclear catalyst is added to the three-necked flask for the second time, and 19.27 g of adipic acid is added. The temperature of the bath is then raised to 185°C for esterification for 120 min. When the water output reaches the predetermined value, the second step esterification reaction is completed;
[0064] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, and 30 μL of titanium-silicon-zinc multi-nuclear catalyst is added to the three-necked flask for the third time. After the pressure in the three-necked flask is pumped below 100 Pa, the temperature of the oil bath is raised to 230°C for polycondensation reaction for 1.5 hours to obtain branched PBAT;
[0065] (5) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain branched PBAT.
[0066] Example 3
[0067] This embodiment provides a branched PBAT, and the preparation method thereof comprises the following steps:
[0068] (1) Weighing and mixing of samples: 17.93 g of terephthalic acid and 27 g of 1,4-butanediol were weighed and added into a three-necked flask, and 30 μL of titanium-silicon-aluminum multi-nuclear catalyst was added, and the three-necked flask was placed in an oil bath preheated to 50° C.;
[0069] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 260 r / min, the oil bath was heated to 190° C. and kept at this temperature for 20 min, then the temperature of the oil bath was gradually increased to 215° C. at a rate of 20° C. every 30 min, and the esterification was carried out at 215° C. for 60 min. When the water output reached a predetermined value, the first step esterification reaction was completed;
[0070] (3) Second step esterification reaction: After the first step esterification is completed, the temperature of the oil bath is lowered to below 140°C, 20 μL of titanium-silicon-aluminum multi-nuclear catalyst is added to the three-necked flask for the second time, and 1.88 g of dimethyl isobutylmalonate and 19.27 g of adipic acid are added, and the temperature of the bath is raised to 185°C for esterification for 120 min. When the water output reaches the predetermined value, the second step esterification reaction is completed;
[0071] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, 40 μL of titanium-silicon-aluminum multi-nuclear catalyst is added to the three-necked flask for the third time, and the pressure in the three-necked flask is pumped below 100 Pa, and the temperature of the oil bath is raised to 230°C for polycondensation reaction for 1.5 hours to obtain branched PBAT;
[0072] (5) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain branched PBAT.
[0073] Comparative Example 1
[0074] This comparative example provides a branched PBAT, and its preparation method comprises the following steps:
[0075] (1) Weighing and mixing of samples: 19.27 g of adipic acid and 27 g of 1,4-butanediol were weighed and added into a three-necked flask, and 50 μL of titanium silicon zinc multinuclear catalyst, 1.88 g of dimethyl isobutyl malonate and 17.93 g of terephthalic acid were added, and then the three-necked flask was placed in an oil bath preheated to 50° C.;
[0076] (2) Esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 260 r / min, the oil bath was heated to 170° C. and kept warm for 20 min, then the temperature of the oil bath was gradually increased to 215° C. at a rate of 5° C. every 20 min, and the esterification reaction was carried out at 215° C. for 8 hours, but no clear and transparent melt was obtained;
[0077] (3) Low-compression polycondensation: After the esterification reaction is completed, the temperature is lowered to below 140°C again, and 40 μL of titanium-silicon-zinc multi-nuclear catalyst is added to the three-necked flask for the third time. After the pressure in the three-necked flask is reduced to below 100 Pa, the temperature of the oil bath is raised to 230°C for polycondensation reaction for 2 hours to obtain branched PBAT;
[0078] (4) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain branched PBAT.
[0079] Comparative Example 2
[0080] This comparative example provides an unbranched PBAT, and its preparation method comprises the following steps:
[0081] (1) Weighing and mixing of samples: 17.93 g of terephthalic acid and 27 g of 1,4-butanediol were weighed and added into a three-necked flask, and 30 μL of titanium silicon zinc multi-nuclear catalyst was added, and the three-necked flask was placed in an oil bath preheated to 50°C;
[0082] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 250 r / min, the oil bath was heated to 190° C. and kept at this temperature for 20 min, then the temperature of the oil bath was gradually increased to 215° C. at a rate of 20° C. every 30 min, and esterification was carried out at 215° C. for 60 min. When the water output reached a predetermined value, the first step esterification reaction was completed;
[0083] (3) Second step esterification reaction: After the first step esterification is completed, the temperature of the oil bath is lowered to below 140°C, 20 μL of titanium silicon zinc multi-nuclear catalyst is added to the three-necked flask for the second time, and 19.27 g of adipic acid is added, and the temperature of the bath is raised to 185°C for esterification for 120 min. When the water output reaches the predetermined value, the second step esterification reaction is completed;
[0084] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, and 36 μL of titanium-silicon-zinc multi-nuclear catalyst is added to the three-necked flask for the third time. After the pressure in the three-necked flask is reduced to below 100 Pa, the temperature of the oil bath is raised to 230°C for polycondensation reaction for 1.5 hours to obtain branched PBAT;
[0085] (5) Finally, the obtained PBAT is removed from the three-necked flask and the water is dried to obtain unbranched PBAT.
[0086] Comparative Example 3
[0087] This comparative example provides a branched PBAT with an inconspicuous pole climbing phenomenon, and the preparation method thereof comprises the following steps:
[0088] (1) Weighing and mixing of samples: 17.93 g of terephthalic acid and 27 g of 1,4-butanediol were weighed and added into a three-necked flask, and 30 μL of titanium silicon zinc multinuclear catalyst and 8.4 g of butylmalonic acid were added, and the three-necked flask was placed in an oil bath preheated to 50°C;
[0089] (2) First step esterification reaction: nitrogen was continuously introduced into the three-necked flask in step (1), the stirring device was turned on, the stirring rate was set to 250 r / min, the oil bath was heated to 190° C. and kept at this temperature for 20 min, then the temperature of the oil bath was gradually increased to 215° C. at a rate of 20° C. every 30 min, and esterification was carried out at 215° C. for 60 min. When the water output reached a predetermined value, the first step esterification reaction was completed;
[0090] (3) Second step esterification reaction: After the first step esterification is completed, the temperature of the oil bath is lowered to below 140°C, 20 μL of titanium silicon zinc multi-nuclear catalyst is added to the three-necked flask for the second time, and 19.27 g of adipic acid is added, and the temperature of the bath is raised to 185°C for esterification for 120 min. When the water output reaches the predetermined value, the second step esterification reaction is completed;
[0091] (4) Low-compression polycondensation: After the second step of esterification reaction is completed, the temperature is lowered to below 140°C again, and 36 μL of titanium silicon zinc multi-nuclear catalyst is added to the three-necked flask for the third time. After the pressure in the three-necked flask is pumped below 100 Pa, the temperature of the oil bath pot is raised to 230°C for polycondensation reaction for 4 hours. At this time, the PBAT melt climbing phenomenon is not obvious, and the melt viscosity is very low;
[0092] (5) Finally, the obtained PBAT is removed from the three-necked flask and dried to obtain branched PBAT with very low melt viscosity.
[0093] evaluate:
[0094] 1. The mechanical tensile properties, melt index, intrinsic viscosity and DSC of the PBAT prepared by branching the ester-based branched structure obtained in Example 1 were evaluated.
[0095] 2. Test methods and conclusions:
[0096] (1) Tensile properties test of PBAT prepared by ester-based branched chain structure
[0097] The prepared butylmalonate branched PBAT (Example 1) was dried in an oven at 60°C and molded at 160°C. It was pressed into standard specimens according to GB / T1040.2-2006 and the tensile strength was tested at room temperature at a tensile speed of 50 mm / min using a universal testing machine Instron 5500R. The tensile results are shown in Figure 3 ,from Figure 3It can be seen that under the same conditions, compared with the unbranched PBAT (Comparative Example 2, represented as PBAT in the figure), the tensile strength and elongation at break of the branched PBAT are significantly improved;
[0098] (2) Melt index test of PBAT prepared by structural branching such as ester branching
[0099] The prepared butylmalonate branched PBAT (Example 1) was dried in an oven at 60°C and cut into small particles. The melt index test was performed at 190°C and 2.16 kg. The results are as follows: Figure 4 ,from Figure 4 It can be seen that under the same conditions, compared with the unbranched PBAT (Comparative Example 2), the melt index of the branched PBAT is significantly reduced, and the melt index of different branched structures under the same conditions is quite different;
[0100] (3) Test of intrinsic viscosity performance of PBAT prepared by structural branching such as ester branching
[0101] The prepared butylmalonate branched PBAT (Example 1) was dried in an oven at 60°C, dissolved in a solvent mixed with phenol and 1,1,2,2-tetrachloroethane, wherein the mass ratio of phenol to 1,1,2,2-tetrachloroethane was 1:1, dissolved into a solution with a mass fraction of 0.5%, tested using an Ubbelohde viscometer, and finally calculated to obtain the intrinsic viscosity. The results are shown in Figure 4 ,from Figure 4 It can be seen that under the same conditions, compared with the unbranched PBAT, the intrinsic viscosity of the branched PBAT is improved, and the result is consistent with the melt index, and the intrinsic viscosity of different branched structures under the same conditions is different;
[0102] (4) DSC performance test of PBAT prepared with structural branching such as ester group branching
[0103] The prepared butylmalonate branched PBAT (Example 1) was dried in an oven at 60°C and tested in a DSC tester. The test conditions were: first, the temperature was lowered from 160°C to -50°C at a rate of 10°C / min, and then the temperature was raised to 160°C at a rate of 10°C / min after 1 minute of heat preservation. The results are shown in Figure 5 After branching, the crystallization temperature of PBAT decreases (e.g. Figure 5 ), but its melting temperature increases (as shown in a Figure 5 (as shown in b). Figure 6Calculated based on the sum of the molar amounts of terephthalic acid and adipic acid as 100%, the PBAT synthesized when the terephthalic acid content is less than 30% (the terephthalic acid content is 20%, that is, the molar ratio of terephthalic acid: adipic acid = 2:8, the preparation method is the same as that of Comparative Example 2, only the molar ratio of terephthalic acid to adipic acid is adjusted), the melting temperature is lower than 50°C, the melting temperature is too low, and its food safety is seriously affected when used in summer.
[0104] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0105] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing branched PBAT, wherein The following steps are involved: First, terephthalic acid and butanediol are subjected to esterification reaction, and then adipic acid is added to carry out esterification reaction.
2. The preparation method according to claim 1, in, The preparation method comprises the following steps: (1) First step esterification reaction: terephthalic acid and butanediol are mixed, and after the catalyst is added for the first time, the first step esterification reaction is carried out at 200-240° C. under a protective gas atmosphere; (2) Second step esterification reaction: After the first step esterification reaction is completed, the temperature is lowered to below 140° C., adipic acid is added and the catalyst is added for the second time, and the second step esterification reaction is carried out at 160-190° C.; (3) Pre-polycondensation reaction: After the second step esterification reaction is completed, the temperature is lowered to below 140°C, and a catalyst is added for the third time to carry out a polycondensation reaction under the conditions of below 100 Pa and 220-260°C. After the reaction is completed, the branched PBAT is obtained; When the boiling point of the branching agent is ≥210°C, the branching agent is added in step (1); when the boiling point of the branching agent is ≤210°C, the branching agent is added in step (2); The branching agent includes diester branching agents and / or dicarboxylic acid branching agents; Preferably, the diester branching agent includes one or a combination of two or more of diethyl n-butyl malonate, diethyl dibutyl malonate, dimethyl propyl malonate, dimethyl isobutyl-1,3-malonate, and diethyl diisobutyl malonate; Preferably, the dicarboxylic acid branching agent includes one or a combination of two or more of butylmalonic acid, propylmalonic acid, propylglutaric acid and isobutylmalonic acid.
3. The preparation method according to claim 2, in, In step (1), the molar ratio of titanium in the catalyst added for the first time to the sum of the molar amounts of terephthalic acid and adipic acid is 1:10000-3:1000; Preferably, in step (1), the molar ratio of the terephthalic acid to the butanediol is 45:100-45:
150.
4. The preparation method according to claim 2, in, In step (2), the molar ratio of titanium in the catalyst added for the second time to the sum of the molar amounts of terephthalic acid and adipic acid is 1:10000-3:1000; Preferably, in step (2), the molar ratio of the adipic acid to the terephthalic acid is 70:30-48:
52.
5. The preparation method according to claim 2, in, In step (3), the molar ratio of the titanium in the catalyst added for the third time to the sum of the molar amounts of the terephthalic acid and the adipic acid is 1:10000-6:1000.
6. The preparation method according to claim 2, in, The catalyst added in step (1) to step (3) is a multi-nuclear catalyst, preferably comprising a titanium-silicon-zinc multi-nuclear catalyst and / or a titanium-silicon-aluminum multi-nuclear catalyst; Preferably, the catalyst added in steps (1) to (3) is the titanium-silicon composite multi-nuclear catalyst described in invention patent application 202210966547.
1.
7. The preparation method according to claim 2, in, The molar ratio of the branching agent to the sum of the molar amounts of the terephthalic acid and the adipic acid is 1:100-10:
100.
8. A branched PBAT prepared by the preparation method according to any one of claims 1 to 7.
9. The branched PBAT according to claim 8, in, The branching degree of the branched PBAT is 1%-10%, preferably 2%-6%.
10. The branched PBAT according to claim 8, in, The branch chain length of the branched PBAT is 2-10 carbon atoms, more preferably 2-6 carbon atoms.
Citation Information
Patent Citations
Process and apparatus for preparing biodegradable polyesters
CN110869413A
Branched hydrophobic biodegradable polyester as well as preparation method and application thereof
CN114716653A
PBAT resin and preparation method thereof
CN114853999A
Copolyesters with enhanced tear strength
US20110207859A1
Aliphatic-aromatic copolyetheresters
US20130158168A1