Preparation method of flocculating agent for fluorine-containing wastewater treatment

The flocculant prepared by reacting acrylamide monomer with vinyl phosphate copolymer and perfluoropolyether diol via phosphoesterification solves the problems of suspended solids aggregation and poor sedimentation in fluoride-containing wastewater, achieving efficient flocculation and sedimentation while reducing the impact of fluoride ions.

CN119019697APending Publication Date: 2024-11-26HUNAN YOUSE CHENZHOU FLUORIDE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411217958.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the treatment of fluoride-containing wastewater, the poor aggregation and sedimentation of suspended solids lead to poor separation, and existing flocculants are unable to effectively solve this problem.

Method used

A copolymer is generated by copolymerizing acrylamide monomer with vinyl phosphate, and then phosphated with perfluoropolyether glycol to form a long-chain polyacrylamide with phosphate groups. This enhances the polarity of the flocculant and its adsorption performance on suspended solids. At the same time, the empty orbital effect of phosphorus is used to adsorb fluoride ions and balance the charge effect of suspended particles.

Benefits of technology

It improves the aggregation and settling properties of suspended solids, shortens the flocculation time, enhances the flocculation effect, reduces the impact of fluoride in fluoride-containing wastewater, and improves water quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019697A_ABST
    Figure CN119019697A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a flocculating agent for fluorine-containing wastewater treatment, which comprises the following steps: carrying out copolymerization reaction on an acrylamide monomer and vinyl phosphoric acid to obtain an acrylamide-vinyl phosphoric acid copolymer, and carrying out phosphorylation reaction on the acrylamide-vinyl phosphoric acid copolymer and perfluoropolyether glycol to obtain a final target product. Wherein acrylamide and vinyl phosphoric acid are subjected to a condensation reaction to form long-chain polyacrylamide with phosphate radicals, so that the polarity of the structure can be improved, the adsorption performance on suspended solid particles in water is enhanced, and the probability of forming large flocculates is further increased, thereby accelerating the sedimentation effect. Meanwhile, phosphoric acid groups are introduced into molecules, and fluorine ions in water can be adsorbed into a molecular bridge through the empty orbital effect of phosphorus, so that the influence of fluorine in fluorine-containing wastewater is reduced, the charge effect of suspended particles is balanced, and the aggregation and sedimentation performance of suspended solids are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical industry, and in particular to a method for preparing a flocculant for treating fluorine-containing wastewater. Background Art

[0002] Flocculants play an important role in the wastewater treatment process. In the wastewater treatment process, by adding flocculants, 80%-95% of suspended matter, 70%-90% of colloidal matter and COD in the water can be effectively removed; at the same time, through flocculation, more than 90% of microorganisms and pathogens in the water can be transferred into sludge, which can enhance the disinfection and sterilization effect.

[0003] The functions of flocculants mainly include the following three aspects: 1. Aggregation of suspended matter: Flocculants can adsorb on the surface of suspended matter particles to form a complex with a charge, so that the particles attract each other and cause the suspended matter to aggregate into larger agglomerates. The size and density of these agglomerates are greatly increased, making it easier for suspended matter to separate and precipitate. 2. Neutralization of charge: In water bodies, many suspended matter particles have charges on their surfaces. The presence of charges leads to mutual repulsion between particles, making it difficult for suspended matter to aggregate and precipitate. Flocculants can react with the charges in the suspended matter and neutralize their charges, thereby weakening the mutual repulsion and promoting the aggregation and precipitation of particles. 3. Improve the separation effect: The function of flocculants is not only to make suspended matter condense into agglomerates, but also to make it easier to separate the agglomerates from the suspended liquid. Generally speaking, the larger the agglomerates, the faster the sedimentation rate, and the better the separation effect. The effect of flocculants increases the size and density of agglomerates, and the separation effect is significantly improved.

[0004] In short, the role of flocculants is to aggregate suspended matter, neutralize charges and improve separation effects, so that suspended matter can be condensed into larger agglomerates for subsequent treatment. Through flocculation, water quality and wastewater treatment effects can be improved, thereby protecting the environment and improving the ecology. In the process of fluoride-containing wastewater treatment, a large amount of fluoride-containing sludge is often produced. These fluoride ions will cause unstable charges in suspended particles, thereby reducing the aggregation and sedimentation of suspended matter, resulting in poor sedimentation and separation effects. Therefore, the development of focused and efficient flocculants for fluoride-containing wastewater treatment has become an important part of the field of fluoride-containing wastewater treatment. Summary of the invention

[0005] The embodiment of the present application provides a method for preparing a flocculant for treating fluorine-containing wastewater, in which acrylamide monomer and vinyl phosphoric acid are first copolymerized to obtain acrylamide-vinyl phosphoric acid copolymer, and then the final target product is obtained by phosphating with perfluoropolyether diol. Among them, acrylamide and vinyl phosphoric acid can form long-chain polyacrylamide with phosphate groups through condensation reaction, which can improve the polarity of the structure, enhance the adsorption performance of suspended solid particles in water, and further increase the probability of forming large flocculants, thereby accelerating the sedimentation effect. At the same time, the phosphate group is introduced into the molecule, and the empty orbital effect of phosphorus can adsorb fluoride ions in water into the molecular bridge, thereby reducing the influence of fluorine in fluorine-containing wastewater, balancing the charge effect of suspended particles, and thus improving the aggregation and sedimentation performance of suspended matter.

[0006] The present invention provides a method for preparing a flocculant for treating fluorine-containing wastewater, comprising:

[0007] Mixing acrylamide monomer and deionized water, and adding the mixture into a polymerization reactor; then adding vinyl phosphoric acid and an initiator into the polymerization reactor to carry out a polymerization reaction, thereby obtaining an acrylamide-vinyl phosphoric acid copolymer;

[0008] The acrylamide-vinyl phosphoric acid copolymer is dissolved in ethylene glycol or polyethylene glycol, and then perfluoropolyether glycol and an antioxidant are added; under the protection of an inert gas, a catalyst is added, and then heated to perform a phosphating reaction, and a flocculant is obtained by rotary evaporation.

[0009] In some embodiments, the mass ratio of the acrylamide monomer to deionized water is 1:3-1:5.

[0010] In some embodiments, the initiator includes at least one of hydrogen peroxide, sodium persulfate, potassium persulfate, and ammonium persulfate.

[0011] In some embodiments, the mass percentage of the initiator to the acrylamide is 0.01%-0.1%.

[0012] In some embodiments, the polymerization reaction is carried out at a pH of 6-9.

[0013] In some embodiments, the mass percentage of the perfluoropolyether diol in the copolymer of acrylamide-vinyl phosphoric acid is 0.5%-1.25%.

[0014] In some embodiments, the antioxidant includes phosphites or diphosphites.

[0015] In some embodiments, the inert gas includes nitrogen.

[0016] In some embodiments, the catalyst includes triphenyl phosphate, tri(butoxyethyl) phosphate, tributyl phosphate, or triisobutyl phosphate.

[0017] In some embodiments, the catalyst accounts for 0.01%-0.1% by weight of the acrylamide-vinyl phosphoric acid copolymer.

[0018] The present invention provides a method for preparing a flocculant for treating fluorine-containing wastewater, in which acrylamide monomer and vinyl phosphoric acid are first copolymerized to obtain acrylamide-vinyl phosphoric acid copolymer, and then the copolymer is phosphated with perfluoropolyether diol to obtain the final target product. Among them, acrylamide and vinyl phosphoric acid can form long-chain polyacrylamide with phosphate groups through condensation reaction, which can improve the polarity of the structure, enhance the adsorption performance of suspended solid particles in water, and further increase the probability of forming large flocculants, thereby accelerating the sedimentation effect. At the same time, a phosphate group is introduced into the molecule, and the empty orbital effect of phosphorus can adsorb fluoride ions in water into the molecular bridge, thereby reducing the influence of fluorine in fluorine-containing wastewater, balancing the charge effect of suspended particles, and thus improving the aggregation and sedimentation performance of suspended matter. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A flow chart of a method for preparing a flocculant for treating fluorine-containing wastewater according to some embodiments is exemplified. DETAILED DESCRIPTION

[0020] In order to better understand the above technical solution, the technical solution of the present application is described in detail below through specific implementation methods.

[0021] Figure 1 The flowchart of a method for preparing a flocculant for treating fluorine-containing wastewater according to some embodiments is exemplarily shown. The embodiment of the present application provides a method for preparing a flocculant for treating fluorine-containing wastewater. The method includes S100-S200.

[0022] S100, mixing acrylamide monomer and deionized water, and adding the mixture into a polymerization reactor; then adding vinyl phosphoric acid and an initiator into the polymerization reactor to carry out a polymerization reaction, thereby obtaining an acrylamide-vinyl phosphoric acid copolymer.

[0023] S200, dissolving the acrylamide-vinyl phosphoric acid copolymer in ethylene glycol or polyethylene glycol, and then adding perfluoropolyether glycol and an antioxidant; adding a catalyst under the protection of an inert gas, and then heating to perform a phosphating reaction, and obtaining a flocculant by rotary evaporation.

[0024] In the embodiment of the present application, acrylamide monomer and vinyl phosphoric acid are first copolymerized to obtain acrylamide-vinyl phosphoric acid copolymer, and then the final target product is obtained by phosphating with perfluoropolyether diol. Among them, acrylamide and vinyl phosphoric acid can form long-chain polyacrylamide with phosphate groups through condensation reaction, which can improve the polarity of the structure, enhance the adsorption performance of suspended solid particles in water, and further increase the probability of forming large flocculants, thereby accelerating the sedimentation effect. At the same time, the phosphate group is introduced into the molecule, and the empty orbital effect of phosphorus can adsorb fluoride ions in water into the molecular bridge, thereby reducing the influence of fluorine in fluoride-containing wastewater, balancing the charge effect of suspended particles, and thus improving the aggregation and sedimentation performance of suspended matter.

[0025] In addition, the molecular structure of perfluoropolyether diol is introduced into the copolymer through phosphoesterification reaction, which can change the molecular structure from long chain to three-dimensional, further enhancing the coagulant effect. The change of molecular stereochemistry can accelerate the capture effect of suspended particles in water and enhance the aggregation effect. At the same time, the introduction of perfluoro chain can increase the attraction to fluorine in water and reduce the influence of fluorine in water. Furthermore, it also makes the substance have a certain defluorination effect. At the same time, it can enhance the hydrophobic effect of flocculants and reduce the friction resistance between liquids, thereby strengthening flocculation and improving water quality.

[0026] In addition, by introducing the perfluoropolyether structure, the stability of the flocculant can be improved, which effectively overcomes the problem of polyacrylamide becoming ineffective due to long-term storage.

[0027] In some embodiments, the mass ratio of the acrylamide monomer to deionized water is 1:3-1:5. In this embodiment, if the mass ratio of acrylamide monomer to deionized water is less than 1:5, the mixed solution will be viscous, which is not conducive to the reaction. If the mass ratio of acrylamide monomer to deionized water is greater than 1:5, the proportion of deionized water is relatively large, that is, the amount of water is large, and the loss caused by the reaction is also relatively large.

[0028] In some embodiments, the molar ratio of the vinyl phosphoric acid to acrylamide monomers is 1:1000-1:5000. In this embodiment, the polymerization reaction effect is good when the molar ratio of the vinyl phosphoric acid to acrylamide monomers is within the range of 1:1000-1:5000, and the degree of polymerization can be controlled.

[0029] In some embodiments, the molar ratio of the vinyl phosphonic acid to acrylamide monomers is 1:2000-1:3000.

[0030] In some embodiments, the initiator includes at least one of hydrogen peroxide, sodium persulfate, potassium persulfate, and ammonium persulfate.

[0031] In some embodiments, the mass percentage of the initiator to the acrylamide is 0.01%-0.1%. In this embodiment, if the mass percentage of the initiator to the acrylamide is less than 0.01%, the initiation is basically not performed. If the mass percentage of the initiator to the acrylamide is higher than 0.1%, the initiation is too fast, and the acrylamide-vinyl phosphoric acid copolymer is not obtained.

[0032] In some embodiments, the polymerization reaction temperature is 30-50° C. In this embodiment, if the polymerization reaction temperature is lower than 30° C., the reaction is very slow or no reaction occurs. If the polymerization reaction temperature is higher than 50° C., the reaction is too fast and no acrylamide-vinyl phosphoric acid copolymer is obtained.

[0033] In some embodiments, the polymerization reaction temperature is 35-45°C.

[0034] In some embodiments, the polymerization reaction is carried out at a pH of 6 to 9. In this embodiment, the polymerization reaction can be carried out smoothly in a pH range of 6 to 9.

[0035] In some embodiments, the polymerization reaction is carried out at a pH of 7-8.

[0036] In some embodiments, the polymerization reaction is carried out under a pressure of 0.01-0.03 MPa. In this embodiment, the pressure in this range can control the structure of the reactants.

[0037] In some embodiments, the polymerization reaction is carried out at a pressure of 0.01-0.15 MPa.

[0038] In some embodiments, the polymerization reaction time is 10-24 hours. In this embodiment, if the polymerization reaction time is less than 10 hours, the reaction is incomplete. If the polymerization reaction time is more than 24 hours, other structures will be generated in the polymerization reaction.

[0039] In some embodiments, the polymerization reaction time is 15-20 hours.

[0040] In some embodiments, the mass percentage of the perfluoropolyether diol in the copolymer of acrylamide-vinyl phosphoric acid is 0.5%-1.25%. In this embodiment, if the mass percentage exceeds the range of 0.5%-1.25%, the final flocculant cannot achieve the flocculation effect.

[0041] In some embodiments, the mass percentage of the perfluoropolyether diol in the copolymer of acrylamide-vinyl phosphoric acid is 0.8%-1%.

[0042] In some embodiments, the antioxidant includes phosphites or diphosphites. The antioxidant plays a stabilizing role in the reaction and can reduce the occurrence of side reactions.

[0043] In some embodiments, the antioxidant accounts for 0.05%-1% by weight of the perfluoropolyether diol.

[0044] In some embodiments, the inert gas includes nitrogen. Of course, it can also be other commonly used inert gases.

[0045] In some embodiments, the catalyst includes triphenyl phosphate, tri(butoxyethyl) phosphate, tributyl phosphate, or triisobutyl phosphate.

[0046] In some embodiments, the mass percentage of the catalyst in the copolymer of acrylamide-vinyl phosphoric acid is 0.01%-0.1%. In this embodiment, if it is less than 0.01%, the reaction is not sufficient, and if it is higher than 0.1%, the yield is reduced and the effect is not good.

[0047] In some embodiments, the reaction temperature of the phosphating reaction is 180-300° C. Temperatures exceeding this range will affect the reaction effect.

[0048] In some embodiments, the reaction temperature of the phosphoesterification reaction is 220-300°C.

[0049] In some embodiments, the reaction time of the phosphating reaction is 8-15 hours. In this embodiment, if the reaction time is short, the reaction is incomplete, and if the reaction time is long, the reaction is basically completed without significant changes, resulting in a waste of resources.

[0050] In some embodiments, the reaction time of the phosphoesterification reaction is 10-12 hours.

[0051] In some embodiments, the temperature of the rotary evaporation is 200-290°C. In this embodiment, the flocculant is obtained by vacuuming until there is no fraction. If the temperature of the rotary evaporation is lower than 200°C, basically no water can be evaporated, and the efficiency is very low. If the temperature of the rotary evaporation is higher than 290°C, the product will volatilize and even denature.

[0052] In some embodiments, the temperature of the rotary evaporation is 255-290°C.

[0053] Example 1

[0054] Step S1: 7.0g acrylamide monomer is dissolved in 35.0g deionized water, added to a polymerization reactor, stirred, and then 0.0024g (1:4454) vinyl phosphoric acid is added. The pH of the system is adjusted to 7.2 with sodium hydroxide solution, the system is heated to 35°C, and the pressure is adjusted to 0.015MPa. 0.007g hydrogen peroxide (31%) (accounting for 0.1% of the acrylamide monomer) is added, and then reacted for 20h to obtain a transparent colloid. Drying is performed to obtain 7.01g of the product.

[0055] Step S2: Dissolve 5.0 g of the copolymer obtained in S1 in ethylene glycol, then add 0.05 g of perfluoropolyether diol (1% of the mass of the copolymer) and 0.0005 g of dimethyl phosphite. Under nitrogen protection, add 0.005 g of triphenyl phosphate (0.1% of the mass of the copolymer), stir for 1 hour, then heat to 200°C and stir to react for 12 hours. After the reaction is completed, transfer all the reaction products to a rotary evaporation flask, set the rotary evaporation temperature to 265°C, turn on the vacuum, and distill until no liquid is distilled to stop the reaction. The remaining product is rinsed with a small amount of acetone to remove impurities. Dry to obtain 4.97 g of product.

[0056] Embodiment 2:

[0057] Step S1:

[0058] Dissolve 70.0g of acrylamide monomer in 210.0g of deionized water, add to the polymerization reactor, start stirring, and then add 0.05g (1:2143) of vinyl phosphoric acid. Use sodium hydroxide solution to adjust the pH of the system to 8.0, raise the temperature of the system to 50°C, and adjust the pressure to 0.012MPa. Add 0.07g of sodium persulfate, and then react for 18h to obtain a transparent colloid. Dry to obtain 70.1g of product.

[0059] Step S2: Dissolve 60.0g of the copolymer obtained in S1 in ethylene glycol, then add 0.5g of perfluoropolyether diol (0.8% of the mass of the copolymer) and 0.0003g of dioctadecyl pentaerythritol diphosphite. Under nitrogen protection, add 0.02g of tributyl phosphate (0.03% of the mass of the copolymer), stir for 1h, then heat to 240°C and stir for 10h. After the reaction is completed, transfer all the reaction products to a rotary evaporation flask, set the rotary evaporation temperature to 285°C, turn on the vacuum, and distill until no liquid is distilled to stop the reaction. The remaining product is rinsed with a small amount of acetone to remove impurities. Dry to obtain 57.1g of product.

[0060] Example 3

[0061] Step S1:

[0062] Dissolve 70.0g of acrylamide monomer in 210.0g of deionized water, add to the polymerization reactor, start stirring, and then add 0.05g (1:2143) of vinyl phosphoric acid. Use sodium hydroxide solution to adjust the pH of the system to 6.2, raise the temperature of the system to 50°C, and adjust the pressure to 0.012MPa. Add 0.07g of sodium persulfate, and then react for 18h to obtain a transparent colloid. Dry to obtain 69.98g of product.

[0063] Step S2: Dissolve 60.0g of the copolymer obtained in S1 in ethylene glycol, then add 0.55g of perfluoropolyether diol and 0.0004g of dioctadecyl pentaerythritol diphosphite. Under nitrogen protection, add 0.02g of tributyl phosphate, stir for 1h, then heat to 240°C and stir for 10h. After the reaction is completed, transfer all the reaction products to a rotary evaporation flask, set the rotary evaporation temperature to 285°C, turn on the vacuum, and distill until no liquid is distilled to stop the reaction. The remaining product is rinsed with a small amount of acetone to remove impurities. Dry to obtain 58.2g of product.

[0064] Example 4

[0065] Step S1:

[0066] Dissolve 71.0g of acrylamide monomer in 220.0g of deionized water, add to the polymerization reactor, start stirring, and then add 0.108g (1:1000) of vinyl phosphoric acid. Use sodium hydroxide solution to adjust the pH of the system to 6.8, raise the temperature of the system to 50°C, and adjust the pressure to 0.012MPa. Add 0.07g of sodium persulfate, and then react for 18h to obtain a transparent colloid. Dry to obtain 69.9g of product.

[0067] Step S2: Dissolve 60.0g of the copolymer obtained in S1 in ethylene glycol, then add 0.55g of perfluoropolyether diol and 0.0004g of dioctadecyl pentaerythritol diphosphite. Under nitrogen protection, add 0.02g of tributyl phosphate, stir for 1h, then heat to 240°C and stir for 10h. After the reaction is completed, transfer all the reaction products to a rotary evaporation flask, set the rotary evaporation temperature to 285°C, turn on the vacuum, and distill until no liquid is distilled to stop the reaction. The remaining product is rinsed with a small amount of acetone to remove impurities. Dry to obtain 58.2g of product.

[0068] Example 5

[0069] Step S1:

[0070] Dissolve 35g of acrylamide monomer in 140g of deionized water, add to the polymerization reactor, start stirring, and then add 0.03g of vinyl phosphoric acid. Use sodium hydroxide solution to adjust the pH of the system to 7.1, heat the system to 45°C, and adjust the pressure to 0.01MPa. Add 0.02g of ammonium persulfate, and then react for 15h to obtain a transparent colloid. Dry to obtain 35.04g of product.

[0071] Step S2: Dissolve 30.0 g of the copolymer obtained in S1 in ethylene glycol, then add 0.27 g of perfluoropolyether diol (0.9% of the mass of the copolymer) and 0.0002 g of diethyl phosphite. Under nitrogen protection, add 0.03 g of tributyl phosphate (0.1% of the mass of the copolymer), stir for 1 hour, then heat to 260°C and stir for 12 hours. After the reaction is completed, transfer all the reaction products to a rotary evaporation flask, set the rotary evaporation temperature to 275°C, turn on the vacuum, and distill until no liquid is distilled to stop the reaction. The remaining product is rinsed with a small amount of acetone to remove impurities. Dry to obtain 29.6 g of product.

[0072] Example 6

[0073] Step S1:

[0074] Dissolve 35g of acrylamide monomer in 140g of deionized water, add to the polymerization reactor, start stirring, and then add 0.03g of vinyl phosphoric acid. Use sodium hydroxide solution to adjust the pH of the system to 7.1, heat the system to 45°C, and adjust the pressure to 0.01MPa. Add 0.02g of ammonium persulfate, and then react for 15h to obtain a transparent colloid. Dry to obtain 35.04g of product.

[0075] Step S2:

[0076] Dissolve 30.0 g of the copolymer obtained in S1 in ethylene glycol, then add 0.15 g of perfluoropolyether diol (0.5% of the mass of the copolymer) and 0.0002 g of diethyl phosphite. Under nitrogen protection, add 0.03 g of tributyl phosphate, stir for 1 h, then heat to 260 ° C, and stir for 12 h. After the reaction is completed, transfer all the reaction products to a rotary evaporation flask, set the rotary evaporation temperature to 275 ° C, turn on the vacuum, and distill until no liquid is distilled to stop the reaction. The remaining product is rinsed with a small amount of acetone to remove impurities. Dry to obtain 29.8 g of product.

[0077] Example 7

[0078] Step S1:

[0079] Dissolve 52.5g of acrylamide monomer in 210g of deionized water, add to the polymerization reactor, start stirring, and then add 0.027g of vinyl phosphoric acid. Use sodium hydroxide solution to adjust the pH of the system to 7.5, raise the temperature of the system to 50°C, and adjust the pressure to 0.011MPa. Add 0.045g of potassium persulfate, and then react for 17h to obtain a transparent colloid. Dry to obtain 52.53g of product.

[0080] Step S2: Dissolve 50.0g of the copolymer obtained in S1 in polyethylene glycol, then add 0.45g of perfluoropolyether diol (0.9% of the mass of the copolymer) and 0.0004g of tetraphenyl dipropylene glycol diphosphite. Under nitrogen protection, add 0.035g of tris(butoxyethyl) phosphate (0.07% of the mass of the copolymer), stir for 1h, then heat to 260°C and stir for 11h. After the reaction is completed, transfer all the reaction products to a rotary evaporation flask, set the rotary evaporation temperature to 280°C, turn on the vacuum, and distill until no liquid is distilled to stop the reaction. The remaining product is rinsed with a small amount of acetone to remove impurities. Dry to obtain 48.79g of product.

[0081] Example 8

[0082] Step S1:

[0083] Dissolve 35g of acrylamide monomer in 140g of deionized water, add to the polymerization reactor, start stirring, and then add 0.03g of vinyl phosphoric acid. Use sodium hydroxide solution to adjust the pH of the system to 7.1, heat the system to 45°C, and adjust the pressure to 0.01MPa. Add 0.02g of ammonium persulfate, and then react for 15h to obtain a transparent colloid. Dry to obtain 35.04g of product.

[0084] Step S2:

[0085] Dissolve 30.0 g of the copolymer obtained from S1 in ethylene glycol, then add 0.15 g of perfluoropolyether diol and 0.0002 g of diethyl phosphite. Under nitrogen protection, add 0.03 g of tributyl phosphate, stir for 1 h, then heat to 260 ° C and stir for 12 h. After the reaction is completed, transfer all the reaction products to a rotary evaporation flask, set the rotary evaporation temperature to 200 ° C, turn on the vacuum, and distill until no liquid is distilled to stop the reaction. The remaining product is rinsed with a small amount of acetone to remove impurities. Dry to obtain 28.8 g of product.

[0086] The same concentration of the product obtained in this example was prepared with flocculants and polyacrylamide, and the fluorine-containing wastewater suspension was added to a 1000 ml measuring cylinder for application testing. The time from adding the flocculant to the complete separation of the flocs was taken as the object of investigation. The experimental results are shown in Table 1.

[0087] Table 1 Experimental comparison results

[0088]

[0089]

[0090] By comparing the above experimental results, it can be seen that the flocculant prepared in the embodiment of the present application has a short flocculation time, and has a flocculation effect with large particles and a clear separation interface, thereby improving the aggregation and sedimentation function of the suspended matter.

[0091] In summary, the present invention provides a method for preparing a flocculant for treating fluorine-containing wastewater, in which acrylamide monomer and vinyl phosphoric acid are first copolymerized to obtain acrylamide-vinyl phosphoric acid copolymer, and then the final target product is obtained by phosphating with perfluoropolyether diol. Among them, acrylamide and vinyl phosphoric acid can form long-chain polyacrylamide with phosphate groups through condensation reaction, which can improve the polarity of the structure, enhance the adsorption performance of suspended solid particles in water, and further increase the probability of forming large flocculants, thereby accelerating the sedimentation effect. At the same time, the phosphate group is introduced into the molecule, and the empty orbital effect of phosphorus can adsorb fluoride ions in water into the molecular bridge, thereby reducing the influence of fluorine in fluorine-containing wastewater, balancing the charge effect of suspended particles, and thus improving the aggregation and sedimentation performance of suspended matter.

[0092] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed. The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application. The above are only preferred implementation methods of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.

Claims

1. A method for preparing a flocculant for treating fluorine-containing wastewater, It is characterized in that include: Mixing acrylamide monomer and deionized water, and adding the mixture into a polymerization reactor; then adding vinyl phosphoric acid and an initiator into the polymerization reactor to carry out a polymerization reaction, thereby obtaining an acrylamide-vinyl phosphoric acid copolymer; The acrylamide-vinyl phosphoric acid copolymer is dissolved in ethylene glycol or polyethylene glycol, and then perfluoropolyether glycol and an antioxidant are added; under the protection of an inert gas, a catalyst is added, and then heated to perform a phosphating reaction, and a flocculant is obtained by rotary evaporation.

2. The method according to claim 1, It is characterized in that The mass ratio of the acrylamide monomer to deionized water is 1:3-1:

5.

3. The method according to claim 1, It is characterized in that The initiator includes at least one of hydrogen peroxide, sodium persulfate, potassium persulfate and ammonium persulfate.

4. The method according to claim 1, It is characterized in that The mass percentage of the initiator to the acrylamide is 0.01%-0.1%.

5. The method according to claim 1, It is characterized in that The polymerization reaction is carried out at a pH of 6-9.

6. The method according to claim 1, It is characterized in that The mass percentage of the perfluoropolyether diol in the copolymer of acrylamide-vinyl phosphoric acid is 0.5%-1.25%.

7. The method according to claim 1, It is characterized in that The antioxidant includes phosphites or diphosphites.

8. The method according to claim 1, It is characterized in that The inert gas includes nitrogen.

9. The method according to claim 1, It is characterized in that The catalyst includes triphenyl phosphate, tri(butoxyethyl) phosphate, tributyl phosphate or triisobutyl phosphate.