Imidazolyl metal organic framework nano material as well as preparation method and application thereof
Through the preparation of imidazole-based metal organic frame nanomaterials, the high selective adsorption and enrichment of carbon dioxide is used to use its cage-shaped pore structure, which solves the problems of insufficient carbon dioxide recognition ability and complex and high cost in the prior art, and realizes the problem of low carbon dioxide recognition ability and complex enrichment methods. Efficient and economical carbon dioxide enrichment effect.
Patent Information
- Application Number
- CN202410839577.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-06-26
AI Technical Summary
It is difficult for existing metal organic frame materials to effectively identify and adsorb carbon dioxide at low concentrations, and the existing carbon dioxide enrichment methods have problems such as complex operation, high cost and low selectivity.
Using imidazole-based metal organic frame nanomaterials, nanomaterials with cage-shaped pore structures are prepared by coordination reaction between metal salts and 4,5-dicyanoimidazoles, and carbon dioxide is enriched using its high selectivity and high adsorption capacity. .
It achieves high selective adsorption and enrichment of carbon dioxide, which has the advantages of simple operation, high selectivity, large adsorption amount and good repeatability, and is suitable for the enrichment of low concentrations of carbon dioxide.
Smart Images

Figure CN119019698A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porous materials, in particular to an imidazole-based metal organic framework nano material and a preparation method and application thereof. Background Art
[0002] Carbon dioxide (CO2) is widely present in the atmosphere and strata of the earth and other planets, and plays an extremely important role in human life and the origin of life. Carbon dioxide can not only maintain the stability of the human body's internal environment and provide plants with nutrients required for photosynthesis, but also affect climate change. Carbon dioxide capture and enrichment are of great significance to maintaining life, exploring the origin of life, and protecting the natural environment. However, the low concentration of carbon dioxide in nature poses a challenge to the enrichment of carbon dioxide. At present, the main methods for separating or enriching carbon dioxide are absorption, adsorption, catalysis, and biological fixation. Among them, adsorption, as a physical method, has the advantages of high selectivity, large adsorption capacity, simple process, and low cost, and is favored by a large number of researchers.
[0003] Metal-organic frameworks (MOFs) have the characteristics of large specific surface area, adjustable pore size, and diversified structure, and have received extensive attention in the field of gas adsorption, storage, and enrichment. However, the metal-organic framework materials reported so far have insufficient recognition ability for carbon dioxide, and it is difficult to effectively and selectively adsorb carbon dioxide from mixed gases at low concentrations. By selecting new organic ligands to construct carbon dioxide-philic metal-organic frameworks, the selectivity of MOFs for carbon dioxide can be effectively improved. In addition, the development of simple synthetic methods to prepare metal-organic framework nanocrystals will be conducive to processing MOFs into enrichment devices and better play the role of MOFs in enriching carbon dioxide. Summary of the invention
[0004] The present application aims to overcome the deficiencies in the prior art and to provide an imidazole-based metal organic framework nanomaterial and a preparation method and application thereof; the preparation method and process provided by the invention are simple, and the prepared imidazole-based metal organic framework nanomaterial has high adsorption selectivity for carbon dioxide at low concentrations and excellent enrichment performance.
[0005] The above technical objectives of the present invention are achieved through the following technical solutions:
[0006] An imidazole-based metal organic framework nanomaterial comprises a metal salt and an organic ligand; the organic ligand is 4,5-dicyanoimidazole.
[0007] Preferably, the metal ions in the metal salt include zinc ions or cobalt ions.
[0008] When the metal ion is a zinc ion, the chemical structure obtained by the reaction of the metal salt with 4,5-dicyanoimidazole is as follows:
[0009]
[0010] When the metal ion is a cobalt ion, the chemical structure obtained by the reaction of the metal salt with 4,5-dicyanoimidazole is as follows:
[0011]
[0012] More preferably, the metal salt is one or more of zinc nitrate, zinc acetate, cobalt nitrate and cobalt acetate; most preferably zinc acetate or cobalt acetate.
[0013] Preferably, the molar ratio of the metal ion to the organic ligand is 1:(1.5-6); more preferably 1:(1-5); most preferably 1:2.
[0014] Preferably, the nano material is a structure with a grain size of 50 to 200 nm.
[0015] In addition, to achieve the above-mentioned purpose, the present invention also provides a method for preparing an imidazole-based metal organic framework nanomaterial, which is specifically: mixing a metal salt, an organic ligand and an organic solvent under stirring at normal pressure, carrying out a coordination reaction at a certain temperature, and then successively centrifuging, washing and drying to obtain the imidazole-based metal organic framework nanomaterial.
[0016] Preferably, the organic solvent includes N,N-dimethylformamide, methanol, water, or N,N-dimethylformamide / water, N,N-dimethylformamide / methanol. More preferably, it is N,N'-dimethylformamide or N,N'-dimethylformamide / methanol; and most preferably, it is N,N'-dimethylformamide / methanol.
[0017] Preferably, the coordination reaction temperature is 25-60°C and the reaction time is 24-96h. The temperature is more preferably 40-60°C, and most preferably 50-60°C. The reaction time is more preferably 24-72h, and most preferably 48-72h.
[0018] In addition, to achieve the above-mentioned purpose, the present invention also provides an application of an imidazole-based metal organic framework nanomaterial in the selective adsorption of carbon dioxide.
[0019] Preferably, the concentration of carbon dioxide and nitrogen in static adsorption is 99.9% or 99.99%;
[0020] Preferably, the concentration of carbon dioxide in nitrogen during dynamic adsorption is 1 ppm, 10 ppm and 100 ppm.
[0021] In addition, to achieve the above purpose, the present invention also provides an application of an imidazole-based metal organic framework in a low-concentration carbon dioxide enricher, and the preparation method of the low-concentration carbon dioxide enricher is as follows:
[0022] The prepared imidazole-based metal organic framework nanomaterial is dispersed in an anhydrous organic solvent, and then the obtained dispersion is deposited on the element to form a thin film. After removing the solvent, the enricher is obtained.
[0023] The enricher is preferably used as a selective enrichment device for carbon dioxide in a carbon dioxide-nitrogen mixed system.
[0024] Preferably, the dispersion concentration is 5 to 30 mg / mL. More preferably, it is 10 to 25 mg / mL -1 , most preferably 15-25 mg mL -1 .
[0025] Preferably, the thickness of the film is ≤60 μm.
[0026] Preferably, the thin film is deposited by spin coating or drop coating.
[0027] In addition, the concentration of the low concentration carbon dioxide is ≤100ppm
[0028] Preferably, the anhydrous organic solvent includes one or more of anhydrous methanol, anhydrous acetonitrile, and anhydrous dichloromethane, more preferably anhydrous methanol and acetonitrile, and most preferably methanol.
[0029] Preferably, during the process of removing the solvent, a heating method is used, and the heating method includes vacuum heating or nitrogen flow heating.
[0030] Preferably, the heating temperature during the removal of the solvent is 80-180°C for 6-24 hours, more preferably 100-150°C, most preferably 120-150°C, and the heating time is more preferably 12-24 hours, most preferably 12-18 hours.
[0031] Preferably, the element is a silicon wafer, organic glass or aluminum wafer.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1. The imidazole-based metal organic framework nanomaterial prepared by the present invention has a cage-like pore structure, wherein the cyano group in the cage can recognize carbon dioxide, and has a high adsorption selectivity for carbon dioxide. As shown in the results of the embodiments of the present invention, the imidazole-based metal organic framework material provided by the present invention has a CO2 / N2 adsorption selectivity of up to 195 and a carbon dioxide enrichment factor of up to 1480. The framework has a cage-like structure, and the cavity of the cage can accommodate a large number of carbon dioxide molecules, thereby increasing the adsorption capacity for carbon dioxide. As shown in the results of the embodiments of the present invention, the imidazole-based metal organic framework material provided by the present invention has an adsorption capacity of 36.2 cm 3 / g, the carbon dioxide enrichment at low concentration is as high as 0.03cm 3 / g.
[0034] 2. The absorption method is to utilize the different solubility of each component in the solvent for enrichment, but it requires a large amount of solvent. The catalytic method is to utilize a catalyst to convert the target component into other components. Not only is the reaction irreversible, but it also requires expensive catalysts. The biological fixation method utilizes organisms such as bacteria or plants to convert them into chemical substances. The reaction is generally irreversible and very time-consuming. Compared with the above methods, the present invention uses imidazole-based metal organic framework materials as selective enrichment agents for carbon dioxide, and adopts physical adsorption to enrich carbon dioxide in carbon dioxide-nitrogen mixtures. It has the advantages of simple operation, high selectivity, large adsorption capacity, and high repeatability. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The crystal structure diagram of Zn(CN-IM)2 and Co(CN-IM)2;
[0036] Figure 2 The X-ray diffraction pattern of Zn(CN-IM)2 powder prepared in Example 1;
[0037] Figure 3 This is the infrared spectrum of the Zn(CN-IM)2 powder prepared in Example 1;
[0038] Figure 4 Thermogravimetric curve of Zn(CN-IM)2 powder prepared in Example 1;
[0039] Figure 5 The scanning electron microscope photographs of the front side of the Zn(CN-IM)2 powder and the cross section of the film prepared in Example 1;
[0040] Figure 6 This is the adsorption curve of Zn(CN-IM)2 powder prepared in Example 1 to carbon dioxide and nitrogen;
[0041] Figure 7 This is a graph showing the adsorption selectivity of carbon dioxide to nitrogen for the Zn(CN-IM)2 powder prepared in Example 1;
[0042] Figure 8 X-ray diffraction pattern of Co(CN-IM)2 powder prepared in Example 2;
[0043] Fig. 9 This is the infrared spectrum of the Co(CN-IM)2 powder prepared in Example 2;
[0044] Fig.10 This is a thermogravimetric curve of Co(CN-IM)2 powder prepared in Example 2;
[0045] Fig.11 The scanning electron microscope photographs of the front side of the Co(CN-IM)2 powder and the cross section of the film prepared in Example 2;
[0046] Fig.12 This is the adsorption curve of Co(CN-IM)2 powder prepared in Example 2 to carbon dioxide and nitrogen;
[0047] Fig.13 This is a graph showing the adsorption selectivity of carbon dioxide to nitrogen for the Co(CN-IM)2 powder prepared in Example 2;
[0048] Fig.14 X-ray diffraction pattern of Zn / Co(CN-IM)2 powder prepared in Example 3;
[0049] Fig.15 This is the infrared spectrum of the Zn / Co(CN-IM)2 powder prepared in Example 3;
[0050] Fig.16 Thermogravimetric curve of Zn / Co(CN-IM)2 powder prepared in Example 3;
[0051] Fig.17 The scanning electron microscope photographs of the front side of the Zn / Co(CN-IM)2 powder and the cross section of the film prepared in Example 3;
[0052] Fig.18 This is the adsorption curve of Zn / Co(CN-IM)2 powder prepared in Example 3 to carbon dioxide and nitrogen;
[0053] Fig.19 This is a graph showing the adsorption selectivity of carbon dioxide to nitrogen for the Zn / Co(CN-IM)2 powder prepared in Example 3;
[0054] Fig. 20 It is a diagram of Zn(CN-IM)2, Co(CN-IM)2 and Zn / Co(CN-IM)2 thin film assembly;
[0055] Fig.21 Schematic diagram of the device used in the experiment of enriching carbon dioxide in carbon dioxide / nitrogen mixture. DETAILED DESCRIPTION
[0056] The preparation of the imidazolyl metal organic framework material described in the present application is further described in detail below in conjunction with specific implementation methods.
[0057] Example 1
[0058] (1) Under normal pressure and stirring, zinc acetate (Zn(CH3COO)2, 91.5 mg, 0.5 mmol) and 4,5-dicyanoimidazole (C5H2N4, 113.3 mg, 0.96 mmol) were added to a glass bottle, and 10 mL of N,N'-dimethylformamide / methanol mixed solvent (solvent volume ratio: 1 / 1) was added with a dropper. The solution was reacted at 50°C for 72 h. When the solution became turbid, heating was stopped. After the temperature dropped to room temperature, centrifugation was performed (speed was 10000 rpm) to obtain a solid. The obtained solid was ultrasonically washed with methanol and then centrifuged. This operation was repeated three times to obtain a washed solid.
[0059] The solvent was exchanged with methanol, with 20 mL of methanol used each time, and the exchange was carried out for 6 hours under stirring, and then centrifuged to obtain a solid; this solvent exchange step was repeated five times. The solid after methanol exchange was vacuum dried at 120°C for 12 hours to obtain an imidazole metal organic framework nanopowder material (abbreviated as Zn(CN-IM)2, with a yield of 78% and a purity of 80%).
[0060] The obtained powder material was dispersed in 5 mL of methanol to obtain a dispersion with a concentration of 20 mg / mL, and 2 drops of the dispersion (0.1 mL) were dripped onto a carrier aluminum sheet using a 5 mL dropper and air-dried at room temperature; then vacuum dried at 120° C. for 12 h to obtain an imidazole-based metal organic framework membrane element (i.e., an enricher), such as Fig. 20 By calculating the mass of the carrier and the membrane element, the mass of the imidazole-based metal organic framework material in the membrane element was calculated to be 30 mg through the mass difference.
[0061] The structure of the material was determined by X-ray diffraction. The powder X-ray diffraction pattern of Zn(CN-IM)2 prepared in this embodiment is as follows Figure 2 As shown. Figure 2 It can be seen that the material has obvious diffraction peaks at 7.3° and 12.5°. After comparison, it is found that these diffraction peaks are consistent with ZIF-8 generated by the classic reaction of 2-methylimidazole and zinc, indicating that the material is isostructural with ZIF-8. The specific structure is as follows Figure 1 shown.
[0062] Nicolet IS50 infrared spectrometer and KBr tablet were used to measure whether the reaction occurred. The infrared spectrum of Zn(CN-IM)2 prepared in this example is shown in FIG. Figure 3 As shown. Figure 3 It can be seen that the material is 420cm -1 The vibration absorption peak of Zn-N appears at , indicating that the coordination reaction between the ligand and the metal occurs smoothly.
[0063] Mettler Toledo, TGA / DSC 3+ thermogravimetric analyzer was used to determine the thermal stability of the material and verify the purity of the material. The thermogravimetric curve of Zn(CN-IM)2 prepared in this example is as follows: Figure 4 As shown. Figure 4 It can be seen that Zn(CN-IM)2 does not lose weight before 100°C, indicating that there is no residual solvent in the material; it starts to lose weight after 230°C, indicating that the Zn(CN-IM)2 prepared by the present invention has good thermal stability.
[0064] The powder and membrane element prepared in this example were characterized by scanning electron microscopy. Figure 5 As shown, the prepared Zn(CN-IM)2 particle size is 50 to 200 nm; Figure 5 As shown, there are no obvious cracks on the surface of the prepared Zn(CN-IM)2 film, indicating that the prepared membrane element has good continuity and the thickness of the film is 60μm.
[0065] Test Case
[0066] The adsorption curves of carbon dioxide and nitrogen of the Zn(CN-IM)2 material prepared in Example 1 were tested at 298K using Autosorb iQ2 adsorptometer and Quantachrome automatic adsorption instrument. The test results are as follows: Figure 6 As shown in the figure, the solid data are carbon dioxide adsorption data, and the hollow data are nitrogen adsorption data. Figure 6 It can be seen that the adsorption capacity of Zn(CN-IM)2 material for carbon dioxide is 36.2 cm 3 / g, and the adsorption capacity of nitrogen is 1.6cm 3 / g; It shows that the Zn(CN-IM)2 prepared by the present invention has a low adsorption capacity for nitrogen and a high adsorption capacity for carbon dioxide, and can achieve the selective adsorption of carbon dioxide in a carbon dioxide-nitrogen mixed system. Figure 6 It can be seen that the adsorption selectivity of Zn(CN-IM)2 material for carbon dioxide in a carbon dioxide-nitrogen mixed system is 178, indicating that the Zn(CN-IM)2 prepared by the present invention has high selective adsorption performance for carbon dioxide in a carbon dioxide-nitrogen mixed system.
[0067] Use as Fig.21 The dynamic adsorption device shown in the figure was used to test the enrichment of carbon dioxide at low concentration on the membrane element prepared in Example 1. The test gas was composed of carbon dioxide and nitrogen, where the concentrations of carbon dioxide were 1 ppm, 10 ppm, and 100 ppm, respectively. The test results are shown in Table 2. The enrichment capacity of the prepared Zn(CN-IM)2 membrane element for carbon dioxide was 0.03 cm 3 / g; through the formula PF = C i / C f The calculated enrichment factor is 748, indicating that Zn(CN-IM)2 material has a high capacity and high selectivity enrichment effect on carbon dioxide.
[0068] Table 2
[0069]
[0070]
[0071] Example 2
[0072] Under normal pressure and stirring, cobalt acetate (Co(CH3COO)2, 88.5 mg, 0.5 mmol) and 4,5-dicyanoimidazole (C5H2N4, 113.3 mg, 0.96 mmol) were added to a glass bottle, and 10 mL of N,N'-dimethylformamide / acetonitrile mixed solvent (solvent volume ratio: 1 / 1) was added with a dropper. The solution was reacted at 50°C for 72 h, and the solution became turbid. The heating was stopped. After the temperature dropped to room temperature, the solution was centrifuged (at a speed of 10,000 rpm) to obtain an initial solid. The obtained solid was ultrasonically washed with acetonitrile and then centrifuged. This operation was repeated three times to obtain a washed solid. Acetonitrile was used for solvent exchange, with the amount of acetonitrile used each time being 20 mL. The solution was exchanged for 6 h under stirring and then centrifuged to obtain a solid. This solvent exchange step was repeated five times. The solid after acetonitrile exchange was vacuum dried at 120° C. for 12 h to obtain an imidazole-based metal organic framework nanopowder material (abbreviated as Co(CN-IM)2, with a yield of 70% and a purity of 80%).
[0073] The obtained powder material was dispersed in 5 mL of acetonitrile to obtain a dispersion with a concentration of 20 mg / mL, and 2 drops of the dispersion (0.1 mL) were spin-coated on a silicon wafer with a 5 mL dropper (rotation speed 500 rpm), and dried at room temperature; then vacuum dried at 120 ° C for 12 h to obtain an imidazole-based metal organic framework membrane element ( Fig. 20 ). By calculating the mass of the carrier silicon wafer and the membrane element, the mass of the imidazole-based metal organic framework material in the membrane element was calculated to be 40 mg through the mass difference.
[0074] The structure of the material was determined by X-ray diffraction. The powder X-ray diffraction pattern of Co(CN-IM)2 prepared in this embodiment is as follows Fig. 9 As shown. Fig. 9 It can be seen that the material has obvious diffraction peaks at 7.3° and 12.5°. After comparison, it is found that these diffraction peaks are consistent with ZIF-7 generated by the reaction of classic 2-methylimidazole and zinc, indicating that the material is isostructural with ZIF-7. The specific structure is as follows Figure 1 shown.
[0075] Nicolet IS50 infrared spectrometer and KBr tablet were used to measure whether the reaction occurred. The infrared spectrum of Co(CN-IM)2 prepared in this example is shown in FIG. Fig.10 As shown. Fig.10 It can be seen that the material is 414cm -1 The vibration absorption peak of Co-N appears at , indicating that the coordination reaction between the ligand and the metal occurs smoothly.
[0076] The Mettler Toledo, TGA / DSC 3+ thermogravimetric analyzer was used to determine the thermal stability of the material and verify the purity of the material. The thermogravimetric curve of Co(CN-IM)2 prepared in this example is shown in FIG. Fig.11 As shown. Fig.11 It can be seen that the Co(CN-IM)2 material did not lose weight before 100°C, indicating that there was no residual solvent in the material; it began to lose weight after 245°C, indicating that the Co(CN-IM)2 prepared by the present invention has good thermal stability.
[0077] The powder and membrane element prepared in this example were characterized by scanning electron microscopy. Fig.12 As shown, the prepared powder particle size is 50 to 200 nm; Fig.12 As shown, there are no obvious cracks on the surface of the prepared Co(CN-IM)2 membrane, indicating that the prepared membrane element has good continuity and the thickness of the film is 80 μm.
[0078] Test Case
[0079] The adsorption curves of carbon dioxide and nitrogen of the Co(CN-IM)2 material prepared in Example 1 were tested at 298K using Autosorb iQ2 adsorptometer and Quantachrome automatic adsorption instrument. The test results are as follows: Fig.13 As shown in the figure, the solid points are carbon dioxide adsorption points, and the hollow points are nitrogen adsorption points. Fig.13 It can be seen that the adsorption capacity of carbon dioxide by Co(CN-IM)2 material is 29.2 cm 3 / g, and the adsorption capacity of nitrogen is 1.1cm 3 / g; It shows that the Co(CN-IM)2 prepared by the present invention has a low adsorption capacity for nitrogen and a high adsorption capacity for carbon dioxide, and can achieve selective adsorption of carbon dioxide in a carbon dioxide-nitrogen mixed system. Fig.13It can be seen that the adsorption selectivity of Co(CN-IM)2 material for carbon dioxide in a carbon dioxide-nitrogen mixed system is 195, indicating that the Co(CN-IM)2 prepared by the present invention has high selective adsorption performance for carbon dioxide in a carbon dioxide-nitrogen mixed system.
[0080] Use as Fig.21 The dynamic adsorption device shown in the figure was used to test the enrichment of carbon dioxide at low concentration on the membrane element prepared in Example 2. The test gas was composed of carbon dioxide and nitrogen, where the concentrations of carbon dioxide were 1 ppm, 10 ppm, and 100 ppm, respectively. The test results are shown in Table 3. The enrichment capacity of the prepared Co(CN-IM)2 membrane element for carbon dioxide was 0.028 cm 3 / g; through the formula PF = C i / C f The calculated enrichment factor is 1480, indicating that Co(CN-IM)2 material has a high capacity and high selectivity enrichment effect on carbon dioxide.
[0081] Table 3
[0082] <![CDATA[Initial CO2 concentration]]> <![CDATA[Concentration of desorbed CO2 after enrichment]]> Enrichment Factor (PF) 1ppm 1480.6ppm 1480.6 10ppm 1827.2ppm 182.7 100ppm 1646.3ppm 16.5
[0083] Example 3
[0084] (1) Under normal pressure and stirring, zinc acetate (Zn(CH3COO)2, 45.8 mg, 0.25 mmol), cobalt acetate (Co(CH3COO)2, 44.3 mg, 0.25 mmol), and 4,5-dicyanoimidazole (C5H2N4, 113.3 mg, 0.96 mmol) were added to a glass bottle, and 10 mL of N,N'-dimethylformamide / methanol mixed solvent (solvent volume ratio: 1 / 1) was added with a dropper. The solution was reacted at 50°C for 72 h. The solution became turbid and the heating was stopped. After the temperature dropped to room temperature, the solution was centrifuged (speed was 10000 rpm) to obtain a solid. The obtained solid was ultrasonically washed with methanol and then centrifuged. This operation was repeated three times to obtain a washed solid. The solvent was exchanged with methanol, and the amount of methanol used each time was 20 mL. The exchange was carried out under stirring for 6 h, and then centrifuged to obtain a solid. This solvent exchange step was repeated five times. The solid after methanol exchange was vacuum dried at 120° C. for 12 h to obtain an imidazole-based metal organic framework nanopowder material (abbreviated as Zn / Co(CN-IM)2, with a yield of 75% and a purity of 80%).
[0085] The obtained powder material was dispersed in 5 mL of methanol to obtain a dispersion with a concentration of 20 mg / mL, and 2 drops of the dispersion (0.1 mL) were dripped onto a plexiglass sheet using a 5 mL dropper and air-dried at room temperature; then vacuum dried at 120°C for 12 hours to obtain an imidazole metal organic framework membrane element. By calculating the mass of the carrier silicon wafer and the membrane element, the mass of the imidazole metal organic framework material in the membrane element was calculated to be 15 mg by the mass difference.
[0086] The structure of the material was determined by X-ray diffraction. The powder X-ray diffraction pattern of Zn / Co(CN-IM)2 prepared in this embodiment is shown in FIG. Fig.14 As shown. Fig.14 It can be seen that the material shows obvious diffraction peaks at 7.3° and 12.5°. After comparison, it is found that these diffraction peaks are consistent with the crystals generated by the reaction of 4,5-dicyanoimidazole and zinc, indicating that the material is isostructural with Zn(CN-IM)2.
[0087] Nicolet IS50 infrared spectrometer and KBr tablet were used to measure whether the reaction occurred. The infrared spectrum of Zn / Co(CN-IM)2 prepared in this example is shown in FIG. Fig.15 As shown. Fig.15 It can be seen that the material is 421cm -1 、412cm -1 The vibration absorption peaks of Zn-N and Co-N appear at the positions respectively, indicating that the coordination reaction between the ligand and the metal occurs smoothly.
[0088] Mettler Toledo, TGA / DSC 3+ thermogravimetric analyzer was used to determine the thermal stability of the material and verify the purity of the material. The thermogravimetric curve of Zn / Co(CN-IM)2 prepared in this example is shown in Figure 2. Fig.16 As shown. Fig.16 It can be seen that Zn / Co(CN-IM)2 does not lose weight before 100°C, indicating that there is no residual solvent in the material; it starts to lose weight after 240°C, indicating that the Zn / Co(CN-IM)2 prepared by the present invention has good thermal stability.
[0089] The powder and membrane element prepared in this example were characterized by scanning electron microscopy. Fig.17 As shown, the particle size of the prepared powder is 50 to 200 nm; Fig.17 As shown, there are no obvious cracks on the surface of the prepared Zn / Co(CN-IM)2 film, indicating that the prepared membrane element has good continuity and the thickness of the film is 30 μm.
[0090] Test Case
[0091] The adsorption curves of carbon dioxide and nitrogen of the Zn / Co(CN-IM)2 material prepared in Example 3 were tested at 298K using Autosorb iQ2 adsorptometer and Quantachrome automatic adsorption instrument. The test results are as follows: Fig.18 As shown in the figure, the solid points are carbon dioxide adsorption points, and the hollow points are nitrogen adsorption points. Fig.18 It can be seen that the adsorption capacity of Zn / Co(CN-IM)2 material for carbon dioxide is 35.8 cm 3 / g, and the adsorption capacity of nitrogen is 1.3cm 3 / g; It shows that the Zn / Co(CN-IM)2 prepared by the present invention has a low adsorption capacity for nitrogen and a high adsorption capacity for carbon dioxide, and can achieve the selective adsorption of carbon dioxide in a carbon dioxide-nitrogen mixed system. Fig.19 It can be seen that the adsorption selectivity of Zn / Co(CN-IM)2 material for carbon dioxide in a carbon dioxide-nitrogen mixed system is 192, indicating that the Zn / Co(CN-IM)2 prepared by the present invention has high selective adsorption performance for carbon dioxide in a carbon dioxide-nitrogen mixed system.
[0092] Use as Fig.21 The dynamic adsorption device shown in the figure was used to test the enrichment of carbon dioxide at low concentration on the membrane element prepared in Example 3. The test gas was composed of carbon dioxide and nitrogen, where the concentrations of carbon dioxide were 1 ppm, 10 ppm, and 100 ppm, respectively. The test results are shown in Table 4. The enrichment capacity of the prepared Zn / Co(CN-IM)2 membrane element for carbon dioxide was 0.029 cm 3 / g; through the formula PF = C i / C f The calculated enrichment factor is 950, indicating that the Zn / Co(CN-IM)2 material has a high capacity and high selectivity enrichment effect on carbon dioxide.
[0093] Table 4
[0094]
[0095]
[0096] The elemental composition and content of the powder materials in Examples 1-3 were determined by inductively coupled plasma emission spectroscopy and elemental analyzer, and the results are shown in Table 1.
[0097] Table 1
[0098]
Claims
1. An imidazole-based metal organic framework nanomaterial, It is characterized in that including metal salts and organic ligands; Wherein, the organic ligand is 4,5-dicyanoimidazole.
2. An imidazolyl metal organic framework nanomaterial according to claim 1, It is characterized in that The metal ions in the metal salt include zinc ions or cobalt ions.
3. An imidazole metal organic framework nanomaterial according to claim 1, It is characterized in that The molar ratio of the metal ion to the organic ligand is 1:(1.5-6).
4. An imidazole metal organic framework nanomaterial according to claim 1, It is characterized in that The nano material is a structure, and the grain size is 50-200nm.
5. A method for preparing an imidazole-based metal organic framework nanomaterial according to any one of claims 1 to 4, It is characterized in that The metal salt, the organic ligand and the organic solvent are mixed under normal pressure and stirred, and a coordination reaction is carried out at a certain temperature. Then, the imidazole-based metal organic framework nanomaterial is obtained after centrifugation, washing and drying.
6. The method for preparing an imidazole-based metal organic framework nanomaterial according to claim 5, It is characterized in that The temperature of the coordination reaction is 25-60° C. and the time is 24-96 hours.
7. Use of an imidazolyl metal organic framework according to any one of claims 1 to 4 in the selective adsorption of carbon dioxide.
8. Use of an imidazole-based metal organic framework nanomaterial according to any one of claims 1 to 4 in a low-concentration carbon dioxide enricher, It is characterized in that The preparation method of the low-concentration carbon dioxide enricher is as follows: The prepared imidazole-based metal organic framework nanomaterial is dispersed in an anhydrous organic solvent, and then the obtained dispersion is deposited on the element to form a thin film. After removing the solvent, the enricher is obtained.
9. Use of the membrane element according to claim 8 as a carbon dioxide selective adsorber or a low-concentration carbon dioxide enricher, It is characterized in that The concentration of the dispersion is 5 to 20 mg / mL.
10. Use of the membrane element according to claim 7 as a carbon dioxide selective adsorber or a low-concentration carbon dioxide enricher, It is characterized in that The thickness of the film is ≤60 μm.
Citation Information
Patent Citations
Application of zinc-containing metal organic framework ZIF-8
CN111437211A
Preparation method of cyano-containing functionalized zeolite imidazole skeleton adsorption material
CN115990465A
Cited By
Nano-drug delivery platform of metal organic framework based on Zn / Co-MOF as well as preparation method and application of nano-drug delivery platform
CN122005854A