Preparation method of Fe / Mn-MOF material suitable for large-scale production
By using the solvothermal method under normal pressure, dissolved iron salt, manganese salt and terephthalic acid and heated and stirred reaction, the problems of long reaction time, high temperature and high pressure in the hydrothermal method were solved, and Fe/Mn- Rapid and stable synthesis and large-scale production of MOF.
Patent Information
- Application Number
- CN202411303472.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-19
AI Technical Summary
The hydrothermal reaction method preparation process of the existing Fe/Mn-MOF materials has a long reaction time, high reaction temperature, high reaction pressure and uncontrollable, resulting in poor repetition of the results and difficulty in achieving large-scale production.
By using the solvent-thermal method under normal pressure, the iron salt, manganese salt and terephthalic acid were dissolved in N,N-dimethylformamide and acetonitrile solvent, the temperature was controlled at 70-90℃. The time is between 50-80 minutes and the stirring rate is between 250-400 rpm, and the nucleation rate and grain size are optimized.
It realizes the rapid and stable synthesis of Fe/Mn-MOF under normal pressure, which is suitable for large-scale production, uniform product quality, safe and controllable reaction process, and is suitable for market-oriented demand.
Smart Images

Figure HDA0005048383650000011 
Figure HDA0005048383650000012 
Figure HDA0005048383650000013
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of MOF material manufacturing, and specifically relates to a method for preparing a Fe / Mn-MOF material. Background Art
[0002] Metal-organic frameworks (MOFs) are porous crystalline materials formed by the self-assembly of metal ions or metal clusters and organic ligands. This material combines the excellent properties of inorganic materials and organic materials. It not only has a high specific surface area, but also has good water stability and acid-base stability. It has attracted the research interest of many scholars. With its unique advantages, it is widely used in catalysis, gas adsorption, gas separation, sensors, drug delivery and other fields, especially for the adsorption and separation of toxic and harmful gases, which can solve some of the increasingly serious environmental problems faced by people. In addition, in the field of separation, the preparation of magnetic composite MOFs materials can be used for the adsorption and separation of toxic and harmful substances and heavy metals, as well as the extraction and separation of target proteins in complex systems. The main synthesis methods of MOF include solvothermal method, hydrothermal method, microwave method, ultrasound-assisted method, etc. The existing Fe / Mn-MOF synthesis method is mainly the hydrothermal reactor synthesis method, which takes a long time to synthesize and needs to be completed in a high-temperature and high-pressure reactor. The pressure in the container during the reaction is uncontrollable, which often leads to poor reproducibility of the results. Therefore, a method for rapidly and stably synthesizing Fe / Mn-MOF under normal pressure was invented.
[0003] For example, Chinese patent CN201911179183.7 discloses a synthesis method of MOF74 (Mn) assembled from sheets into rods, comprising dissolving 2,5-dihydroxyterephthalic acid and 50% manganese nitrate solution in a mixture of N,N-dimethylformamide, anhydrous ethanol, and deionized water to obtain a mixed solution, transferring the mixed solution to a reactor, and heating for a period of time; after the reaction, washing and drying by centrifugation to obtain a sheet-assembled rod-shaped manganese-based MOF. The synthesis method obtains sheet-assembled rod-shaped manganese-based MOF by hydrothermal synthesis, and the size and morphology of the MOFs can be controlled by adjusting the reactant ratio, reaction solvent, reaction temperature, and reaction time. The prepared sheet-assembled rod-shaped MOF74 (Mn) material can be used as a new catalytic material. The synthesis method is carried out at high temperature and high pressure, and also has problems such as long reaction time, uncontrollable pressure in the container during the reaction, and poor reproducibility of results. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing Fe / Mn-MOF materials under normal pressure, with short reaction time, stable and controllable product quality, and suitable for large-scale production, in order to address the technical difficulties of the existing hydrothermal reactor synthesis method for preparing Fe / Mn-MOF materials, such as long preparation process, high reaction temperature, high and uncontrollable reaction pressure, poor repeatability, and difficulty in large-scale production.
[0005] To achieve the above-mentioned object of the present invention, a preparation method of Fe / Mn-MOF material suitable for large-scale production of the present invention comprises the following steps: dissolving an iron salt in solvent A, dissolving a manganese salt in solvent A, and dissolving terephthalic acid in solvent B; respectively adding the three into a reaction container for mixing, heating and stirring, and after reaction, washing and drying to obtain Fe / Mn-MOF; the molar ratio of the iron salt, the manganese salt, and the terephthalic acid is (0.9-1.1):
[0006] (0.9-1.1): 1. The heating and stirring temperature is controlled at 70-90°C and the reaction time is controlled at 50-80min.
[0007] Preferably, the solvent A is N,N-dimethylformamide; and the solvent B is acetonitrile.
[0008] Preferably, the iron salt is ferric chloride hexahydrate; and the manganese salt is manganese acetate tetrahydrate.
[0009] Preferably, the molar ratio of the iron salt, the manganese salt and the terephthalic acid is 1:1:1.
[0010] Preferably, the stirring rate is 250-400 rpm, preferably 320 rpm.
[0011] After a large number of experimental studies, the technical parameters of heating and stirring were optimized as follows: heating and stirring temperature was 80°C, reaction time was 60min, and stirring rate was 320rpm.
[0012] Compared with the prior art, the present invention provides a method for preparing Fe / Mn-MOF materials suitable for large-scale production, provides a special synthesis reaction environment for metal ions and organic ligands, and has the following beneficial effects:
[0013] (1) Compared with the traditional hydrothermal method, the preparation method of the present invention is to carry out the reaction under normal pressure conditions, and the reaction process is safe and reliable.
[0014] (2) The preparation method of the present invention can control the product grain size and nucleation rate by adjusting the solvent ratio and stirring rate, and can also adjust the product morphology according to market demand.
[0015] (3) The preparation method of the present invention can rapidly synthesize and prepare Fe / Mn-MOF at a relatively low temperature of about 80°C, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a SEM image of the Fe / Mn-MOF material obtained in Example 1 of the method of the present invention.
[0017] Figure 2 This is the SEM image of the Fe-MOF material obtained in Comparative Example 1.
[0018] Figure 3 This is a particle size distribution diagram of the Fe / Mn-MOF material obtained in Example 1 of the method of the present invention.
[0019] Figure 4 This is the particle size distribution diagram of the Fe-MOF material obtained in Comparative Example 1. DETAILED DESCRIPTION
[0020] To describe the present invention, a method for preparing a Fe / Mn-MOF material suitable for large-scale production is further described in detail below in conjunction with an embodiment. If no specific conditions are specified in the embodiments, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially. The scope of protection of the present invention is not limited by the following embodiments.
[0021] Example 1
[0022] This embodiment adopts a synthesis method of Fe / Mn-MOF, comprising the following steps:
[0023] (1) Weigh 0.0259 g of ferric chloride hexahydrate and dissolve it in 4 mL of N,N-dimethylformamide.
[0024] (2) Weigh 0.0173 g of manganese acetate tetrahydrate and dissolve it in 4 mL of N,N-dimethylformamide.
[0025] (3) Weigh 0.0166 g of terephthalic acid and dissolve it in 8 mL of acetonitrile.
[0026] (4) The solutions in (1), (2) and (3) are mixed so that the molar ratio of ferric chloride hexahydrate, manganese acetate tetrahydrate and terephthalic acid is close to 1:1:1, and the mixture is transferred into a glass beaker.
[0027] (5) Set the operating parameters of the magnetic stirring heating apparatus: temperature 80°C, reaction time 60 min, and stirring rate 320 rpm.
[0028] (6) Place the magnetic stirring rotor into the sample, connect the temperature probe, and start the operation.
[0029] (7) After the synthesis is completed, the sample is removed and centrifuged. The separated solid is washed three times with ethanol and centrifuged three times. The synthesized Fe / Mn-MOF is dried in a vacuum drying oven at 70° C. to obtain a Fe / Mn-MOF material.
[0030] Comparative Example 1
[0031] This comparative example adopts a synthesis method of Fe-MOF, comprising the following steps:
[0032] (1) Weigh 0.864 g of ferric chloride hexahydrate and dissolve it in 10 mL of N,N-dimethylformamide.
[0033] (2) Weigh 0.532 g of terephthalic acid and dissolve it in 10 mL of N,N-dimethylformamide.
[0034] (3) The solutions in (1) and (2) are mixed, the molar ratio of ferric chloride hexahydrate to terephthalic acid is close to 2:1, the liquid is transferred into a polytetrafluoroethylene lined reactor, and the reactor is placed in a forced air drying oven.
[0035] (4) Set the operating parameters of the blast drying oven to 150°C and a reaction time of 12 hours, and start operation.
[0036] (5) After the synthesis is completed, the sample is removed and centrifuged. The separated solid is washed three times with ethanol and centrifuged three times. The synthesized Fe-MOF is dried in a vacuum drying oven at 70° C. to obtain a Fe-MOF material.
[0037] Example 2
[0038] This embodiment adopts a synthesis method of Fe / Mn-MOF, comprising the following steps:
[0039] (1) Weigh 0.0519 g of ferric chloride hexahydrate and dissolve it in 8 mL of N,N-dimethylformamide.
[0040] (2) Weigh 0.0346 g of manganese acetate tetrahydrate and dissolve it in 8 mL of N,N-dimethylformamide.
[0041] (3) Weigh 0.0332 g of terephthalic acid and dissolve it in 16 mL of acetonitrile.
[0042] (4) The solutions in (1), (2) and (3) are mixed so that the molar ratio of ferric chloride hexahydrate, manganese acetate tetrahydrate and terephthalic acid is close to 1:1:1, and the mixture is transferred into a glass beaker.
[0043] (5) Set the operating parameters of the magnetic stirring heating apparatus: temperature 80°C, reaction time 60 min, and stirring rate 320 rpm.
[0044] (6) Place the magnetic stirring rotor into the sample, connect the temperature probe, and start the operation.
[0045] (7) After the synthesis is completed, the sample is removed and centrifuged. The separated solid is washed three times with ethanol and centrifuged three times. The synthesized Fe / Mn-MOF is dried in a vacuum drying oven at 70° C. to obtain a Fe / Mn-MOF material.
[0046] Example 3
[0047] This embodiment adopts a synthesis method of Fe / Mn-MOF, comprising the following steps:
[0048] (1) Weigh 0.0519 g of ferric chloride hexahydrate and dissolve it in 7.5 mL of N,N-dimethylformamide.
[0049] (2) Weigh 0.0346 g of manganese acetate tetrahydrate and dissolve it in 7.5 mL of N,N-dimethylformamide.
[0050] (3) Weigh 0.0332 g of terephthalic acid and dissolve it in 15 mL of acetonitrile.
[0051] (4) The solutions in (1), (2) and (3) are mixed so that the molar ratio of ferric chloride hexahydrate, manganese acetate tetrahydrate and terephthalic acid is close to 1:1:1, and the mixture is transferred into a glass beaker.
[0052] (5) Set the operating parameters of the magnetic stirring heating apparatus: temperature 80°C, reaction time 60 min, and stirring rate 320 rpm.
[0053] (6) Place the magnetic stirring rotor into the sample, connect the temperature probe, and start the operation.
[0054] (7) After the synthesis is completed, the sample is removed and centrifuged. The separated solid is washed three times with ethanol and centrifuged three times. The synthesized Fe / Mn-MOF is dried in a vacuum drying oven at 70° C. to obtain a Fe / Mn-MOF material.
[0055] Depend on Figure 1 From the SEM image of the Fe / Mn-MOF material obtained in Example 1 of the method of the present invention, it can be seen that the method of the present invention can obtain Fe / Mn-MOF with uniform size and morphology, good crystallization, smooth spindle-shaped surface, and uniform particle size distribution.
[0056] Depend on Figure 2 It can be seen from the SEM image of the Fe-MOF material obtained in Comparative Example 1 that in the comparative example, the Fe-MOF has a typical spindle-shaped structure.
[0057] Combination Figure 3 and Figure 4It can be seen that under the same ratio of metal ions to organic ligands, the method for preparing Fe / Mn-MOF according to the present invention has a smaller particle size (D Fe-MOF ≈200D Fe / Mn-MOF ), the morphology is intact, the crystallinity is intact, the reaction is complete, and there is almost no impurity on the surface.
[0058] The SEM images of the Fe / Mn-MOF materials obtained in Examples 2 and 3 of the method of the present invention are similar to those in Example 1.
Claims
1. A method for preparing Fe / Mn-MOF materials suitable for large-scale production, characterized in that The method comprises the following steps: dissolving an iron salt in a solvent A, dissolving a manganese salt in a solvent A, and dissolving terephthalic acid in a solvent B; respectively introducing the three into a reaction container for mixing, heating and stirring, and after reaction, washing and drying to obtain Fe / Mn-MOF; the molar ratio of the iron salt, the manganese salt and the terephthalic acid is (0.9-1.1):(0.9-1.1):1, the heating and stirring temperature is controlled at 70-90°C, and the reaction time is controlled at 50-80min.
2. A method for preparing a Fe / Mn-MOF material suitable for large-scale production as claimed in claim 1, characterized in that: The solvent A is N,N-dimethylformamide.
3. A method for preparing a Fe / Mn-MOF material suitable for large-scale production as claimed in claim 1, characterized in that: The solvent B is acetonitrile.
4. A method for preparing a Fe / Mn-MOF material suitable for large-scale production as claimed in claim 1, characterized in that: The iron salt is ferric chloride hexahydrate.
5. A method for preparing a Fe / Mn-MOF material suitable for large-scale production as claimed in claim 1, characterized in that: The manganese salt is manganese acetate tetrahydrate.
6. A method for preparing a Fe / Mn-MOF material suitable for large-scale production as claimed in claim 1, characterized in that: The solvent A is N,N-dimethylformamide, the solvent B is acetonitrile; the iron salt is ferric chloride hexahydrate; the manganese salt is manganese acetate tetrahydrate; and the molar ratio of the iron salt, the manganese salt and terephthalic acid is 1:1:
1.
7. A method for preparing a Fe / Mn-MOF material suitable for large-scale production as claimed in claim 6, characterized in that: The stirring rate was 250-400 rpm.
8. A method for preparing a Fe / Mn-MOF material suitable for large-scale production as claimed in claim 7, characterized in that: The heating and stirring temperature was 80°C, the reaction time was 60 min, and the stirring rate was 320 rpm.
Citation Information
Patent Citations
Fe-based bimetallic organic framework electrocatalyst, preparation and application thereof
CN111250167A
Green and economic large-scale synthesis method of ZIF-8 material
CN116041717A
Fe / Mn-MOFs composite material and preparation method and application thereof
CN116328737A
Method for synthesizing, regulating and controlling MOF (Metal Organic Framework) material in large scale with high space-time yield and high quality
CN118126343A
Process for the preparation of a metal-organic compound
US20160176070A1