Manufacturing method of shelf containing plant fibers and shelf manufactured by same

Through the blending process of halogen-free flame retardant with thermoplastic resin and plant fibers, combined with micro-foaming injection molding technology, the poor flame retardancy and safety of plant fiber composite shelves are solved, and high flame retardancy and lightweight are achieved and excellent strength, suitable for aviation.

CN119019742APending Publication Date: 2024-11-26THE BOEING CO +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310568141.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-18
Publication Date
2024-11-26

Smart Images

  • Figure CN119019742A_ABST
    Figure CN119019742A_ABST
Patent Text Reader

Abstract

The invention relates to a manufacturing method of a shelf containing plant fibers and the shelf manufactured by the manufacturing method. The manufacturing method comprises the following steps: a) homogenizing a halogen-free flame retardant to obtain a homogenized halogen-free flame retardant; b) melting thermoplastic resin, and uniformly blending the molten thermoplastic resin with the plant fibers, the homogeneous halogen-free flame retardant and the compatilizer to obtain a plant fiber composite material; c) extruding and granulating the plant fiber composite material to obtain a granular composite material; and d) mixing the granular composite material with a foaming agent, and performing injection molding to obtain the shelf. The shelf manufactured by the method is green, environment-friendly, non-toxic and harmless, and also has a high flame-retardant effect and a light-weight effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of bio-based composite materials, and in particular, to a method for manufacturing a shelf (tray table) containing plant fibers and a shelf manufactured using the same. Background Art

[0002] Artificial fibers have been widely used as reinforcing phases of composite materials. However, the production of artificial fiber materials consumes a lot of natural resources and energy, may cause harm to humans, is difficult to recycle after the service life expires, and may cause environmental pollution. In contrast, plant fibers have become an ideal substitute for artificial fibers (synthetic fibers) due to their excellent specific strength and modulus, low cost, renewability, degradability, and environmental friendliness.

[0003] Plant fiber composites have been widely used due to their advantages of low cost, renewability, biodegradability, environmental friendliness, high specific strength and specific modulus. However, in actual application, the high flammability of plant fiber composites limits their further application. Conventionally, halogen-containing flame retardants are often added to improve the flame retardant properties of materials. Although ideal flame retardant effects can be obtained, halogen-containing flame retardants will release a large amount of toxic and carcinogenic substances when burned, which will not only pollute the environment, but also seriously affect human health.

[0004] Foam refers to a type of polymer material that has a large number of pores introduced into the polymer. Compared with unfoamed materials, the presence of pores in foam not only makes the product lighter, but also gives the product excellent heat insulation, sound insulation, cushioning and adsorption functions, so that products made of foam can meet the market application needs of lightweight and functionalization. Conventional chemical foaming agents are difficult to completely decompose and may remain inside the product, thus endangering human health. In addition, alkane foaming agents are flammable and explosive, posing safety hazards. Summary of the invention

[0005] The purpose of the present disclosure is to provide a method for manufacturing a shelf containing plant fibers from a plant fiber composite material, so as to solve the technical problems of the known shelves made of fiber materials, such as poor flame retardancy, environmental pollution, high weight and poor safety.

[0006] In order to achieve the above-mentioned purpose, according to one aspect of the present disclosure, there is provided a method for manufacturing a shelf comprising plant fibers, the method comprising the following steps: a) homogenizing a halogen-free flame retardant to obtain a homogeneous halogen-free flame retardant; b) melting a thermoplastic resin, and uniformly blending the molten thermoplastic resin with plant fibers, the homogeneous halogen-free flame retardant and a compatibilizer to obtain a plant fiber composite material; c) extruding and granulating the plant fiber composite material to obtain a granular composite material; and d) mixing the granular composite material with a foaming agent and injection molding to obtain a shelf.

[0007] Furthermore, in an embodiment, step b) is carried out in an internal mixer, the internal mixing time is 10-15 min, the rotation speed is 30-60 r / min, and the internal mixing temperature is 160-180°C; and / or step c) is carried out in a single screw extruder, the temperature of zone 1 of the single screw extruder is 140-160°C, the temperature of zone 2 is 150-175°C, the temperature of zone 3 is 150-170°C and the head temperature is 140-165°C, and the residence time of the plant fiber composite material in the single screw extruder is 1-2 min.

[0008] Further, in an embodiment, step d) is performed in a micro-foam injection molding machine having a blanking port temperature of 20-45°C, a feeding section temperature of 160-175°C, a compression section temperature of 175-195°C and a metering section temperature of 170-195°C.

[0009] Further, in an embodiment the blowing agent is a gaseous blowing agent and comprises CO2 and / or N2.

[0010] Furthermore, the plant fiber is selected from one or more of ramie, flax, jute, sisal, kenaf and bamboo fiber.

[0011] Furthermore, the plant fibers are chopped plant fibers having a length of 4 mm to 10 mm.

[0012] Further, the thermoplastic resin is one or more selected from polyethylene, polypropylene, polyamide and polylactic acid.

[0013] Further, the halogen-free flame retardant is a single flame retardant of diethyl aluminum hypophosphite or melamine urate.

[0014] Furthermore, the halogen-free flame retardant is a binary composite flame retardant of diethylaluminum hypophosphite and melamine urate, wherein the weight ratio of diethylaluminum hypophosphite to melamine urate is 1:1.

[0015] Furthermore, the halogen-free flame retardant is a ternary composite flame retardant of diethyl aluminum hypophosphite, melamine urate and nano-silicon dioxide, wherein the weight ratio of diethyl aluminum hypophosphite, melamine urate and nano-silicon dioxide is 1:1:1.

[0016] Furthermore, the compatibilizer is triglycidyl isocyanurate.

[0017] According to another aspect of the present disclosure, a shelf manufactured by the above method is provided.

[0018] Further, the shelf has a UL 94 rating of V0.

[0019] Further, the shelf is a shelf attached to a passenger seat of a commercial airliner.

[0020] Further, the composite material of the shelf has a tensile strength of 50 MPa to 70 MPa.

[0021] As mentioned above, the known shelf has technical problems such as poor flame retardancy, environmental pollution, high weight and poor safety. According to the technical solution of the present disclosure, a method for manufacturing a shelf comprising plant fiber is provided, by melt blending a certain weight ratio of thermoplastic resin, plant fiber, halogen-free flame retardant and compatibilizer, and then foaming and manufacturing a micro-foamed halogen-free flame retardant composite material, which is not only green and environmentally friendly, non-toxic and harmless, but also has a high flame retardant effect and weight loss effect, and the addition of plant fiber and compatibilizer reduces the damage of halogen-free flame retardant to the mechanical properties of the composite material. Therefore, the shelf manufactured by the plant fiber composite material described herein and the method described herein has the advantages of safety, environmental protection, high flame retardancy, lightweight and excellent strength. The shelf manufactured by the plant fiber composite material described herein and the method described herein can be applied to the aviation field, for example, in commercial airliners as an aircraft dining board. The aviation dining board prepared in the disclosed manner has good flame retardancy, light weight, green and environmental protection and high strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings constituting part of the present application are used to provide a further understanding of the present disclosure. The exemplary embodiments of the present disclosure and their descriptions are used to explain the present disclosure and do not constitute an improper limitation on the present disclosure. In the drawings:

[0023] Figure 1 A top view and a side view of a plant fiber composite material airline meal plate obtained according to Example 1 of the present disclosure are shown, wherein the size measurement of the airline meal plate in mm is shown; and

[0024] Figure 2 The photographs of the plant fiber composite material airline meal plate obtained according to Example 1 of the present disclosure are shown. DETAILED DESCRIPTION

[0025] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present disclosure will be described in detail below in conjunction with the embodiments.

[0026] In view of the deficiencies in the prior art mentioned in the background technology, a specific embodiment of the present disclosure provides a method for manufacturing a shelf containing plant fibers, the method comprising: a) homogenizing a halogen-free flame retardant to obtain a homogeneous halogen-free flame retardant; b) melting a thermoplastic resin, and uniformly blending the molten thermoplastic resin with plant fibers, the homogeneous halogen-free flame retardant and a compatibilizer to obtain a plant fiber composite material; c) extruding and granulating the plant fiber composite material to obtain a granular composite material; and d) mixing the granular composite material with a foaming agent and injection molding to obtain a shelf.

[0027] The method disclosed in this article is to melt-blend a certain weight proportion of plant fiber, thermoplastic resin, halogen-free flame retardant and compatibilizer to obtain a micro-foamed halogen-free flame retardant composite material, and then foam it. The shelf made of the composite material disclosed in this article and the method disclosed in this article is not only green and environmentally friendly, non-toxic and harmless, and naturally degradable, but also has high flame retardancy and lightweight effects. In addition, the damage of the halogen-free flame retardant to the mechanical properties (such as tensile strength) of the composite material of the shelf can be reduced by adding plant fiber and compatibilizer.

[0028] In some examples, step b) is carried out in an internal mixer, the internal mixer time is 10-15 min, the rotation speed is 30-60 r / min, and the internal mixer temperature is 160-180°C. For example, the internal mixer time is 10 min, 11 min, 12 min, 13 min, 14 min or 15 min, etc. For example, the rotation speed is 30 r / min, 40 r / min, 50 r / min or 60 r / min, etc. For example, the internal mixer temperature is 160°C, 170°C or 180°C, etc. When the internal mixer time, rotation speed and internal mixer temperature are within the scope of the present disclosure, the mixing speed of the materials in the internal mixer can be increased, the mixing time and energy input can be saved, and it is helpful to improve the homogeneity of the mixed materials, thereby further contributing to the balance between the various properties of the obtained plant fiber composite material.

[0029] In some examples, step c) is performed in a single screw extruder, the temperature of the first zone of the single screw extruder is 140-160°C, the temperature of the second zone is 150-175°C, the temperature of the third zone is 150-170°C, and the head temperature is 140-165°C, and the residence time of the plant fiber composite material in the single screw extruder is 1-2min. When the temperature of each section of the single screw extruder is within the range of the present disclosure, the foaming speed can be further increased, energy input and cost can be saved, and it is helpful to improve the micro-foaming effect of the halogen-free flame retardant composite material, thereby further improving the lightweight characteristics of the micro-foamed halogen-free flame retardant composite material.

[0030] In some examples, the foaming agent is a gas foaming agent and includes CO2 and / or N2. When the foaming agent is within the scope of the present disclosure, gases such as CO2 and N2 as physical foaming agents are non-toxic and harmless, and are abundant in source and low in price, which conforms to the concept of green production and helps to further improve the environmentally friendly properties of the micro-foamed halogen-free flame retardant composite material.

[0031] In some examples, the plant fiber is selected from one or more of ramie, flax, jute, sisal, kenaf and bamboo fiber. For example, the plant fiber is ramie, flax, jute, sisal, kenaf or bamboo fiber. Compared with known plant fibers, the use of plant fibers within the scope of the present disclosure can further improve the lightweight characteristics of fiber composite materials, as well as the mechanical properties (such as tensile strength) of plant fiber composite materials, and reduce the damage of halogen-free flame retardants to the mechanical properties (such as tensile strength) of composite materials.

[0032] In some examples, the plant fiber is a short-cut plant fiber with a length of 4 mm to 10 mm. For example, the length of the plant fiber is 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, etc. When the length of the plant fiber is within the range of the present disclosure, it can be better mixed with the composite matrix, thereby further improving the mechanical properties (such as tensile strength) of the plant fiber composite material.

[0033] In some examples, the thermoplastic resin is one or more selected from polyethylene, polypropylene, polyamide and polylactic acid. For example, the thermoplastic resin is polyethylene, polypropylene, polyamide or polylactic acid. More preferably, the thermoplastic resin is polylactic acid. Compared with known thermoplastic resins, the use of thermoplastic resins within the scope of the present disclosure can achieve a good melting effect at the operating temperature of the internal mixer, improve the uniformity of the molten mixture, and further contribute to the good balance of flame retardancy, safety, lightweight and mechanical properties of the plant fiber composite material.

[0034] In some examples, the halogen-free flame retardant is a single flame retardant of diethyl aluminum hypophosphite or melamine urate. For example, the halogen-free flame retardant is diethyl aluminum hypophosphite, or the halogen-free flame retardant is melamine urate. In some examples, the halogen-free flame retardant is a binary composite flame retardant of diethyl aluminum hypophosphite and melamine urate, and the weight ratio of diethyl aluminum hypophosphite to melamine urate is 1:1. In some examples, the halogen-free flame retardant is a ternary composite flame retardant of diethyl aluminum hypophosphite, melamine urate and nano-silicon dioxide, and the weight ratio of diethyl aluminum hypophosphite, melamine urate and nano-silicon dioxide is 1:1:1. Compared with known halogen-free flame retardants, the use of halogen-free flame retardants within the scope of the present disclosure can further improve the flame retardant effect of plant fiber composite materials.

[0035] In some examples, the compatibilizer is triglycidyl isocyanurate. Compared with known compatibilizers, the use of the compatibilizer within the scope of the present disclosure can further reduce the damage of the halogen-free flame retardant to the mechanical properties (such as tensile strength) of the composite material, thereby further improving the mechanical properties (such as tensile strength) of the plant fiber composite material.

[0036] According to another embodiment of the present invention, a shelf made by the above method is provided.

[0037] In some examples, the shelf has a UL 94 rating of V0.

[0038] In some examples, the shelf is a shelf attached to a passenger seat of a commercial airliner.

[0039] In some examples, the composite fiber of the shelf has an increased tensile strength. For example, the composite fiber has a tensile strength of 50 MPa to 70 MPa, or a tensile strength of 50 MPa to 65 MPa, or a tensile strength of 51 MPa to 62 MPa.

[0040] Another specific embodiment of the present disclosure provides a plant fiber composite material, which comprises: 59.1-74.2 parts by weight of a thermoplastic resin; 3-10 parts by weight of plant fiber; 15-25 parts by weight of a halogen-free flame retardant; and 0.3-0.9 parts by weight of a compatibilizer, wherein the halogen-free flame retardant comprises one or more selected from diethyl aluminum hypophosphite, melamine urate and nano-silica.

[0041] As mentioned above, the known shelves have technical problems such as poor flame retardancy, environmental pollution, high weight and poor safety. Based on the above problems, the present disclosure provides a plant fiber composite material and a method for manufacturing a shelf from the plant fiber composite material, by controlling the weight ratio of thermoplastic resin, plant fiber, halogen-free flame retardant and compatibilizer within the scope of this article, and selecting the halogen-free flame retardant as one or more of diethyl aluminum hypophosphite, melamine urate and nano-silica, a fiber composite material with a good balance of flame retardancy, safety, lightweight characteristics and mechanical properties (such as tensile strength) can be provided.

[0042] The present disclosure also provides implementations according to the following items:

[0043] Item 1: A plant fiber composite material, comprising: 59.1-74.2 parts by weight of a thermoplastic resin; 3-10 parts by weight of plant fiber; 15-25 parts by weight of a halogen-free flame retardant; and 0.3-0.9 parts by weight of a compatibilizer, wherein the halogen-free flame retardant comprises one or more selected from diethyl aluminum hypophosphite, melamine urate and nano-silica.

[0044] Item 2: The plant fiber composite material according to Item 1, wherein the plant fiber is selected from one or more of ramie, flax, jute, sisal, kenaf and bamboo fiber.

[0045] Item 3: The plant fiber composite material according to item 1 or 2, wherein the plant fiber is chopped fibers having a length of 4 mm to 10 mm.

[0046] Item 4: The plant fiber composite material according to Item 1 or 2, wherein the thermoplastic resin is one or more selected from polyethylene, polypropylene, polyamide and polylactic acid.

[0047] Item 5: For the plant fiber composite material according to item 1 or 2, the halogen-free flame retardant is a single flame retardant of diethyl aluminum hypophosphite or melamine urate.

[0048] Item 6: According to the plant fiber composite material of Item 1 or 2, the halogen-free flame retardant is a binary composite flame retardant of diethyl aluminum hypophosphite and melamine urate, wherein the weight ratio of diethyl aluminum hypophosphite to melamine urate is 1:1.

[0049] Item 7: According to the plant fiber composite material of Item 1 or 2, the halogen-free flame retardant is a ternary composite flame retardant of diethyl aluminum hypophosphite, melamine urate and nano-silica, wherein the weight ratio of diethyl aluminum hypophosphite, melamine urate and nano-silica is 1:1:1.

[0050] Item 8: The plant fiber composite material according to item 1 or 2, wherein the compatibilizer is triglycidyl isocyanurate.

[0051] Item 9: A shelf made from the plant fiber composite material according to any one of Items 1 to 8.

[0052] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0053] The parts of each component used in the following examples and comparative examples refer to parts by weight of the corresponding component.

[0054] Example 1

[0055] (1) Preparation process of halogen-free flame retardant: 5 parts of diethyl aluminum hypophosphite, 5 parts of melamine urate and 5 parts of nano-silicon dioxide are uniformly mixed to obtain a ternary composite halogen-free flame retardant, wherein the weight ratio of diethyl aluminum hypophosphite, melamine urate and nano-silicon dioxide in the ternary composite flame retardant is 1:1:1.

[0056] (2) Preparation process of plant fiber composite material: 66.4 parts of polylactic acid resin are added to an internal mixer, and after it is melted, 3 parts of ramie fiber, 0.6 parts of triglycidyl isocyanurate (compatibilizer) and 15 parts of the ternary composite halogen-free flame retardant obtained in step (1) are added in sequence, and after they are melted and blended uniformly, the plant fiber composite material is taken out, and then extruded and granulated by a single screw extruder to obtain a granular composite material. The internal mixing time in the single screw extruder is 12 minutes, the speed is 50r / min, and the internal mixing temperature is 170°C; the temperatures of each section of the single screw extruder are as follows: zone 1 145°C, zone 2 155°C, zone 3 155°C, and the head temperature is 145°C.

[0057] (3) Manufacturing process of airline meal board: 100 parts of the granular composite material obtained in step (2) and 0.4 parts of the physical foaming agent N2 are mixed in a micro-foaming injection molding machine, and then injection molding is performed to obtain an airline meal board. The temperature of each section of the micro-foaming injection molding machine is as follows: 25°C for the blanking port, 170°C for the feeding section, 185°C for the compression section, and 175°C for the metering section.

[0058] Example 2

[0059] An airline meal plate was prepared in the same manner as in Example 1, except that the weights of the components added to the internal mixer in step (2) were as follows: 74.2 parts of polylactic acid resin, 10 parts of ramie fiber, 0.9 parts of triglycidyl isocyanurate (compatibilizer), and 25 parts of the ternary composite halogen-free flame retardant obtained in step (1).

[0060] Example 3

[0061] An airline meal plate was prepared in the same manner as in Example 1, except that the weights of the components added to the internal mixer in step (2) were as follows: 59.1 parts of polylactic acid resin, 3 parts of ramie fiber, 0.3 parts of triglycidyl isocyanurate (compatibilizer), and 15 parts of the ternary composite halogen-free flame retardant obtained in step (1).

[0062] Example 4

[0063] An airline meal plate was prepared in the same manner as in Example 1, except that in step (1), 10 parts of diethyl aluminum hypophosphite and 10 parts of melamine urate were used as binary composite halogen-free flame retardants, and the weight ratio of diethyl aluminum hypophosphite to melamine urate was 1:1.

[0064] Example 5

[0065] An airline meal plate was prepared in the same manner as in Example 1, except that 20 parts of diethyl aluminum hypophosphite were used as a halogen-free flame retardant in step (1), and no foaming agent was used in the foaming process in step (3).

[0066] Comparative Example 1

[0067] (1) Preparation process of polylactic acid resin: 100 parts of polylactic acid resin are added to an internal mixer, and the mixture is taken out after internal mixing for a period of time, and then extruded and granulated by a single screw extruder to obtain granular polylactic acid material. The internal mixing time in the single screw extruder is 12 minutes, the rotation speed is 50r / min, and the internal mixing temperature is 170°C; the temperatures of each section of the single screw extruder are as follows: zone 1 145°C, zone 2 155°C, zone 3 155°C, and die head temperature 145°C.

[0068] (2) Manufacturing process of airline meal plates: 100 portions of granular polylactic acid material obtained in step (1) are injection molded in an injection molding machine to produce airline meal plates. The temperatures of each section of the injection molding machine are as follows: 25°C for the blanking port, 170°C for the feeding section, 185°C for the compression section, and 175°C for the metering section.

[0069] Comparative Example 2

[0070] An airline meal plate was prepared in the same manner as in Example 1, except that the weights of the components added to the internal mixer in step (2) were as follows: 79.4 parts of polylactic acid resin, 30 parts of ramie fiber, and 0.6 parts of triglycidyl isocyanurate (compatibilizer).

[0071] Performance Testing

[0072] 1. Tensile performance test

[0073] According to GB / T 1040.1-2006 standard, the tensile strength of each embodiment and each comparative example was measured on a HDW-2000 microcomputer-controlled rubber tensile testing machine; the test specimen size was 75×10×2 mm 3 , the tensile rate is 10mm / min, five specimens are tested for each material, and the average value is calculated.

[0074] 2. UL 94 vertical burning rating test

[0075] According to GB / T 2408-2008 standard, the UL 94 vertical burning rating of each embodiment and each comparative example was tested on a horizontal vertical burning tester (CZF-5), and the sample size was 125×13×3mm 3 V0 means that after two 10-second combustion tests were conducted on the sample, the flame went out within 10 seconds; NC means that the sample burned until it was completely burned out during the combustion test, and the flame did not go out during the combustion process.

[0076] The tensile properties and flame retardant test results of the composite materials are shown in Table 1. PLA represents polylactic acid, RF represents ramie fiber, A represents diethyl aluminum hypophosphite, M represents melamine urate, and S represents nano silicon dioxide. xAyMzS represents that the weight ratio of the three flame retardants A, M and S is x:y:z.

[0077] Table 1

[0078]

[0079] As can be seen from the above results, the flame retardant disclosed herein can effectively improve the flame retardant properties of polylactic acid resin relative to polylactic acid resin without flame retardant. More significantly, the ternary composite flame retardant disclosed herein (diethyl aluminum hypophosphite, melamine urate and nano-silica) improves the flame retardant properties of polylactic acid resin (UL 94 grade is the plastic flammability standard) to V0 level. The addition of plant fiber and compatibilizer causes only a slight decrease in the tensile strength of polylactic acid resin after blending with flame retardant, ensuring that the aviation dining board has sufficient supporting strength during use. The micro-foaming process significantly increases the weight loss rate of the composite material. The aviation dining board manufactured by the plant fiber composite material disclosed herein has a higher strength, thereby successfully preparing a lightweight and high-strength aviation dining board.

[0080] The above embodiments are merely descriptions of the technical solutions of the present disclosure, rather than limiting the scope thereof. Although ordinary technicians in the field can make various modifications with reference to the above examples, they should be within the protection scope of the present disclosure as long as they do not deviate from the design spirit of the present disclosure.

[0081] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.

[0082] The above description only relates to specific embodiments of the present disclosure and is not intended to limit the present disclosure. For those skilled in the art, the present disclosure may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present disclosure shall be included in the protection scope of the present disclosure.

Claims

1. A method for producing a shelf comprising plant fibers, It is characterized in that The method comprises the following steps: a) homogenizing the halogen-free flame retardant to obtain a homogeneous halogen-free flame retardant; b) melting a thermoplastic resin, and uniformly blending the molten thermoplastic resin with plant fibers, the homogeneous halogen-free flame retardant and a compatibilizer to obtain a plant fiber composite material; c) extruding and granulating the plant fiber composite material to obtain a granular composite material; and d) mixing the granular composite material with a foaming agent and performing injection molding to obtain the shelf.

2. The method according to claim 1, It is characterized in that Step b) is carried out in an internal mixer, the mixing time is 10-15 min, the rotation speed is 30-60 r / min, and the mixing temperature is 160-180° C.; and / or Step c) is carried out in a single screw extruder, wherein the temperature of zone 1, zone 2, zone 3, zone 3 and die head of the single screw extruder are 140-160°C, 150-175°C, 150-170°C and 140-165°C, and the residence time of the plant fiber composite material in the single screw extruder is 1-2 min.

3. The method according to claim 1 or 2, It is characterized in that Step d) is carried out in a micro-foam injection molding machine, wherein the temperature of the blanking port of the micro-foam injection molding machine is 20-45°C, the temperature of the feeding section is 160-175°C, the temperature of the compression section is 175-195°C and the temperature of the metering section is 170-195°C.

4. The method according to claim 1 or 2, It is characterized in that The blowing agent is a gas blowing agent and comprises CO 2 and / or N 2 .

5. The method according to claim 1 or 2, It is characterized in that The plant fiber is selected from one or more of ramie, flax, jute, sisal, kenaf and bamboo fiber.

6. The method according to claim 1 or 2, It is characterized in that The plant fibers are short-cut plant fibers with a length of 4 mm to 10 mm.

7. The method according to claim 1 or 2, It is characterized in that The thermoplastic resin is one or more selected from polyethylene, polypropylene, polyamide and polylactic acid.

8. The method according to claim 1 or 2, It is characterized in that The halogen-free flame retardant is a single flame retardant of diethyl aluminum hypophosphite or melamine urate.

9. The method according to claim 1 or 2, It is characterized in that The halogen-free flame retardant is a binary composite flame retardant of diethyl aluminum hypophosphite and melamine urate, wherein the weight ratio of diethyl aluminum hypophosphite to melamine urate is 1:

1.

10. The method according to claim 1 or 2, It is characterized in that The halogen-free flame retardant is a ternary composite flame retardant of diethyl aluminum hypophosphite, melamine urate and nano silicon dioxide, wherein the weight ratio of diethyl aluminum hypophosphite, melamine urate and nano silicon dioxide is 1:1:

1.

11. The method according to claim 1 or 2, It is characterized in that The compatibilizer is triglycidyl isocyanurate.

12. A shelf made by the method of claim 1 or 2.

13. The shelf according to claim 12, It is characterized in that The shelf has a UL 94 rating of V0.

14. A shelf according to claim 12 or 13, It is characterized in that The shelf is a shelf that is attached to a passenger seat of a commercial airliner.

15. The shelf according to claim 12 or 13, It is characterized in that The composite material of the shelf has a tensile strength of 50 MPa to 70 MPa.

Citation Information

Cited By

  • Bamboo-based flame-retardant degradable foam material and preparation method thereof

    CN120944316A