Polyacrylonitrile-polyimide-montmorillonite double-super-hydrophobic nano composite aerogel as well as preparation method and application thereof
Through the preparation of polyacrylonitrile-polyimide-monmormortar double-superose nanocomposite aerogel, the double-superose performance is achieved using multiple concave structures, and the difficulty in preparing double-superose materials in the prior art is solved. The problem is that efficient oil-water separation and excellent mechanical properties are achieved, and are suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202411102345.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-12
AI Technical Summary
It is difficult to prepare bisuperophobic materials in the prior art, and the same material is difficult to manifest as both sub-oil superhydrophobic and sub-oilophobic, which limits its application in the field of oil-water separation.
The preparation method of polyacrylonitrile-polyimide-montmorillonite double-superose nanocomposite aerogel is used to mix polyacrylonitrile nanofibers, water-soluble polyamic acid fibers and lamellar montmorillonite to perform directionalization Freezing and imidation treatment form a double supersparse nanocomposite aerogel with multiple concave structures.
It realizes the double superradiation performance of aerogel, can be separated on demand oil and water, maintain high separation and filtration efficiency and high throughput, is suitable for industrial production, has excellent mechanical properties and resilience, and is suitable for offshore oil leakage treatment and domestic oil sewage Separation and other fields.
Smart Images

Figure CN119019745A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aerogels, and in particular relates to a polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel, and a preparation method and application thereof. Background Art
[0002] Super-wetting materials have the advantages of high separation efficiency, ease of use and recyclability, and have been widely studied. However, most of the current super-wetting materials only have single wettability and are not convenient to use. Double super-repellent materials can avoid the problem of single usage scenarios. The same material can achieve on-demand oil-water separation, which greatly saves the cost of use.
[0003] Theoretically, it is impossible for the surface of the same solid to be superhydrophobic under oil and superoleophobic under water at the same time. In the same oil-water-solid three-phase system, the underwater oil contact angle and the oil-water contact angle are complementary, that is, the underwater oleophobic interface is hydrophilic in oil, and the hydrophobic interface in oil is oleophilic in water. Due to this thermodynamic contradiction, it is difficult to give a single surface dual superphobic properties.
[0004] Since it is difficult to prepare dual superphobic materials using current technical means, it is necessary to improve this. Summary of the invention
[0005] In view of this, the present invention proposes a polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel and a preparation method and application thereof to solve the technical problems existing in the prior art.
[0006] In a first aspect, the present invention provides a method for preparing a polyacrylonitrile-polyimide-montmorillonite dual superphobic nanocomposite aerogel, comprising the following steps:
[0007] Mixing a polyacrylonitrile nanofiber dispersion, a water-soluble polyamic acid fiber, and lamellar montmorillonite to obtain a mixed dispersion;
[0008] Directingly freezing and freeze-drying the mixed dispersion in sequence to obtain polyacrylonitrile / polyamic acid-montmorillonite macroporous oriented nanofiber composite aerogel;
[0009] The polyacrylonitrile / polyamic acid-montmorillonite macroporous oriented nanofiber composite aerogel is subjected to imidization treatment to obtain a polyacrylonitrile-polyimide-montmorillonite dual superphobic nanocomposite aerogel;
[0010] The mass of the lamellar montmorillonite is 5-10% of the mass of the polyacrylonitrile nano-short fibers in the polyacrylonitrile nano-short fiber dispersion.
[0011] Preferably, the concentration of the polyacrylonitrile nano short fiber dispersion is 6 to 16 wt %;
[0012] The mass of the water-soluble polyamic acid fiber is 5-15% of the mass of the polyacrylonitrile nano-short fiber in the polyacrylonitrile nano-short fiber dispersion.
[0013] Preferably, the imidization treatment comprises in sequence:
[0014] Heating to a first temperature at a first heating rate to perform a first imidization treatment;
[0015] Raising the temperature to a second temperature at a second heating rate to perform a second imidization treatment;
[0016] heating to a third temperature at a third heating rate to perform a third imidization treatment;
[0017] Wherein, the first temperature is 85-115°C, and the first imidization treatment time is 50-80min;
[0018] The second temperature is 185-215° C., and the second imidization treatment time is 50-80 min;
[0019] The third temperature is 285-315° C., and the third imidization treatment time is 50-80 min;
[0020] The first heating rate, the second heating rate and the third heating rate are each independently 3-7°C min -1 .
[0021] Preferably, the directional freezing specifically includes:
[0022] placing the mixed dispersion in a mold, and placing the bottom of the mold in a cold source for directional freezing;
[0023] The mold is made of heat-conducting metal, the cold source is liquid nitrogen, and the directional freezing time is 5 to 15 minutes.
[0024] Before the mixed dispersion is placed in the mold, the mold is placed in a cold source for precooling, and the precooling time is 5 to 8 minutes.
[0025] Preferably, the freeze-drying temperature is -30 to -65°C and the time is 24 to 72 hours.
[0026] Preferably, the method for preparing the polyacrylonitrile nano short fiber dispersion comprises the following steps:
[0027] The polyacrylonitrile solution was spun into polyacrylonitrile nanofibers by electrospinning;
[0028] The polyacrylonitrile nanofibers are dispersed in water, and homogenized and crushed to make the polyacrylonitrile nanofibers short-fibered to obtain a polyacrylonitrile nanofiber dispersion;
[0029] The diameter of the polyacrylonitrile nanofibers is 500 to 680 nm and the length is 45 to 60 μm.
[0030] Preferably, the preparation method of the water-soluble polyamic acid fiber comprises the following steps:
[0031] Adding 4,4'-diaminodiphenyl ether and pyromellitic acid dianhydride to N,N-dimethylacetamide to carry out polycondensation reaction to obtain water-insoluble polyamic acid;
[0032] Mixing triethylamine with the water-insoluble polyamic acid to modify it and obtain a water-soluble polyamic acid solution;
[0033] The water-soluble polyamic acid solution is subjected to ice water precipitation and then freeze-dried to obtain water-soluble polyamic acid fibers.
[0034] Preferably, polyacrylonitrile powder is dissolved in an organic solvent to obtain a polyacrylonitrile solution; wherein the concentration of the polyacrylonitrile solution is 5 to 15 wt %; and the organic solvent comprises an amide solvent;
[0035] The working parameters of electrospinning control include: extrusion speed is 0.06~0.10mm min -1 , the spinning voltage is 10~14kV;
[0036] The process parameters of the homogenization crushing process control include: the homogenization crushing temperature is 10-30°C, the rotation speed is 10000-16000rpm, and the time is 30-60min.
[0037] Preferably, 4,4'-diaminodiphenyl ether and pyromellitic acid dianhydride are added to N,N-dimethylacetamide, and polycondensation is carried out at -10 to 0°C under an inert atmosphere for 4 to 8 hours to obtain a water-insoluble polyamic acid; wherein the molar ratio of 4,4'-diaminodiphenyl ether, pyromellitic acid dianhydride and N,N-dimethylacetamide is (0.8 to 1.2):(0.8 to 1.2):(25 to 30);
[0038] The triethylamine and the water-insoluble polyamic acid are mixed, and the reaction is continued at -10 to 0°C for 4 to 8 hours to obtain a water-soluble polyamic acid solution; wherein the molar ratio of 4,4'-diaminodiphenyl ether to triethylamine is 1:(0.6 to 1);
[0039] Water is added to the obtained water-soluble polyamic acid solution for precipitation, and the obtained solid product is freeze-dried to obtain water-soluble polyamic acid fiber; wherein the freeze-drying temperature is -30 to -65°C and the time is 24 to 72 hours.
[0040] In a second aspect, the present invention further provides a polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel, which is prepared by the preparation method.
[0041] In a third aspect, the present invention also provides a method for preparing polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel or the use of the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel as an oil-water separation material or an air filtration material.
[0042] The polyacrylonitrile-polyimide-montmorillonite dual superphobic nanocomposite aerogel and its preparation method and application have the following beneficial effects compared with the prior art:
[0043] 1. The preparation method of the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel of the present invention is to use polyamic acid as an adhesive and cross-linking agent, mix it with polyacrylonitrile nanofibers, lamellar montmorillonite and deionized water, and directionally freeze-dry it to obtain a macroporous oriented structure, and then obtain a PAN / PI-MMT double superphobic nanofiber composite aerogel with a certain strength by imidization. After directional freezing and imidization treatment, MMT (lamellar montmorillonite) is evenly distributed on the nanofibers to form a multiple concave structure. The aerogel obtains underwater superoleophobicity and under-oil superhydrophobicity due to the multiple concave structures, and can separate oil and water on demand. The composite aerogel with oriented macropores and secondary pores can maintain high separation filtration efficiency and high flux during the oil-water separation process;
[0044] 2. The preparation method of the polyacrylonitrile-polyimide-montmorillonite dual superphobic nanocomposite aerogel of the present invention is simple to operate, the raw materials for preparation are low-toxic, easy to obtain, green and environmentally friendly, the production cost is low, and it is suitable for industrial production;
[0045] 3. The polyacrylonitrile / polyimide-montmorillonite dual superphobic nanofiber composite aerogel prepared by the preparation method provided by the present invention has a multi-level pore structure, and the multi-level pore structure includes macropores, mesopores and micropores. The aerogel provided by the present invention has a macropore orientation and a multi-level pore structure and a multi-concave micro-nano structure, which gives the aerogel excellent separation efficiency, separation flux, mechanical properties and dual superphobic properties. The aerogel has good application prospects in the fields of offshore oil spill treatment, domestic oil and sewage separation, and sensors;
[0046] 4. The polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel prepared by the present invention has a contact angle of 0° with water or oil in air, and a contact angle of oil under water and a contact angle of water under oil are both greater than 150°, and has double superphobic properties; the oil flux of the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel prepared by the present invention is (2.63±0.08~5.83±0.20)×10 4 L m-2 h -1 , with a compression rebound of 81.43±0.84% at 40% strain, showing the excellent resilience of the aerogel. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0048] Figure 1 The scanning electron microscope images of the composite aerogels prepared in Example 1 and Comparative Examples 1-2;
[0049] Figure 2 The graph is a contact angle test result diagram of the composite aerogels prepared in Example 1 and Comparative Examples 1-2;
[0050] Figure 3 The separation efficiency of the composite aerogels prepared in Example 1 and Comparative Examples 1 to 2 for filtering different oils;
[0051] Figure 4 The flux of the composite aerogels prepared in Example 1 and Comparative Examples 1-2 for filtering different oils;
[0052] Figure 5 This is a graph showing the resilience test results of the composite aerogel adhesive prepared in Comparative Example 2;
[0053] Figure 6 This is a graph showing the resilience test results of the composite aerogel adhesive prepared in Example 1;
[0054] Figure 7 This is a graph showing the resilience test results of the composite aerogel adhesive prepared in Comparative Example 1. DETAILED DESCRIPTION
[0055] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0056] In order to better understand the present invention but not to limit the scope of the present invention, all the numbers used in this application to express the amount, percentage, and other numerical values should be understood as modified by the word "about" in all cases. Therefore, unless otherwise specified, the numerical parameters listed in the specification and the appended claims are approximate values, which may be changed according to the different ideal properties attempted to be obtained. Each numerical parameter should at least be regarded as obtained based on the reported significant figures and by conventional rounding methods.
[0057] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the numbered range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0058] The present invention provides a method for preparing a polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel, comprising the following steps:
[0059] S1, mixing a polyacrylonitrile nano short fiber dispersion, a water-soluble polyamic acid fiber, and a lamellar montmorillonite to obtain a mixed dispersion;
[0060] S2, sequentially performing directional freezing and freeze drying on the mixed dispersion to obtain polyacrylonitrile / polyamic acid-montmorillonite macroporous oriented nanofiber composite aerogel;
[0061] S3, subjecting the polyacrylonitrile / polyamic acid-montmorillonite macroporous oriented nanofiber composite aerogel to imidization treatment to obtain the polyacrylonitrile-polyimide-montmorillonite dual superphobic nanocomposite aerogel;
[0062] The mass of the lamellar montmorillonite is 5-10% of the mass of the polyacrylonitrile nano-short fibers in the polyacrylonitrile nano-short fiber dispersion.
[0063] The preparation method of the polyacrylonitrile-polyimide-montmorillonite double superphobic nano composite aerogel of the present invention comprises the following steps: mixing a polyacrylonitrile nano short fiber dispersion, a water-soluble polyamic acid fiber and a lamellar montmorillonite to obtain a mixed dispersion; then directionally freezing and freeze-drying the mixed dispersion to obtain a polyacrylonitrile / polyamic acid-montmorillonite macroporous oriented nano fiber composite aerogel; and then subjecting the polyacrylonitrile / polyamic acid-montmorillonite macroporous oriented nano fiber composite aerogel to imidization treatment to obtain a polyacrylonitrile-polyimide-montmorillonite double superphobic nano composite aerogel.
[0064] The present invention introduces multiple concave structures on the surface of the material, combines the polar-nonpolar theory and the liquid injection theory, and allows water or oil to enter the multiple concave micro / nano structures to form a liquid film. The multiple concave structures on the solid surface can capture air and form a negative Laplace pressure difference at the gas-liquid interface, thereby transforming the gas-liquid interface from a concave surface to a convex surface of a liquid-liquid interface, preventing the infiltration of the other phase. Therefore, the multiple concave structures can effectively maintain the oil-water interface. The material can be wetted by oil as an "oil removal type" separation material, and can also be wetted by water as a "water removal type" separation material, which can achieve on-demand separation of oil-water mixtures.
[0065] Specifically, the lamellar montmorillonite and the polyacrylonitrile nanofibers of the present invention are hydrophilic materials, and the polyimide is a hydrophobic material. The ratio of the three is adjusted to adjust the hydrophilicity and lipophilicity of the material in the air. Due to the hydrogen bonding effect, the montmorillonite is evenly distributed on the surface of the polyacrylonitrile nanofibers to form a multiple concave structure, thereby achieving dual superphobic properties.
[0066] The present invention uses polyamic acid as an adhesive and a cross-linking agent, mixes with polyacrylonitrile nanofibers, lamellar montmorillonite and deionized water, and freeze-dries in a directional manner to obtain a macroporous oriented structure, and then imidates to obtain a PAN / PI-MMT double super-phobic nanofiber composite aerogel with a certain strength. After directional freezing and imidation treatment, MMT (montmorillonite) is evenly distributed on the nanofibers to form a multiple concave structure. The aerogel obtains underwater super-oleophobicity and oil-under-water super-hydrophobicity due to the multiple concave structures, and can separate oil and water on demand. The composite aerogel with oriented macropores and secondary pores can maintain high separation and filtration efficiency and high flux during the oil-water separation process.
[0067] In some embodiments, the lamellar montmorillonite is specifically lamellar sodium-montmorillonite.
[0068] In some embodiments, the concentration of the polyacrylonitrile nano short fiber dispersion is 6 to 16 wt % (mass concentration); preferably, the concentration is 9 to 12 wt %.
[0069] In some embodiments, the mass of the water-soluble polyamic acid fiber is 5-15% of the mass of the polyacrylonitrile nano-short fibers in the polyacrylonitrile nano-short fiber dispersion. Preferably, the mass of the water-soluble polyamic acid fiber is 10% of the mass of the polyacrylonitrile nano-short fibers in the polyacrylonitrile nano-short fiber dispersion.
[0070] In some embodiments, the imidization treatment is preferably a programmed imidization treatment, and the programmed imidization treatment preferably includes sequentially performing a first heating, a first imidization, a second heating, a second imidization, a third heating, and a third imidization; specifically, the imidization treatment sequentially includes:
[0071] Heating to a first temperature at a first heating rate to perform a first imidization treatment;
[0072] Raising the temperature to a second temperature at a second heating rate to perform a second imidization treatment;
[0073] heating to a third temperature at a third heating rate to perform a third imidization treatment;
[0074] Wherein, the first temperature is 85-115°C, and the first imidization treatment time is 50-80 min; preferably, the first temperature is 95-105°C, and the first imidization treatment time is 60-70 min;
[0075] The second temperature is 185-215°C, and the second imidization treatment time is 50-80 min; preferably, the second temperature is 195-205°C, and the second imidization treatment time is 60-70 min;
[0076] The third temperature is 285-315° C., and the third imidization treatment time is 50-80 min; preferably, the third temperature is 295-305° C., and the third imidization treatment time is 60-70 min;
[0077] The first heating rate, the second heating rate and the third heating rate are each independently 3-7°C min -1 , preferably 4~6℃min -1 .
[0078] In some embodiments, the directional freezing is preferably directional freezing using unidirectional oriented ice crystal template method.
[0079] In some embodiments, directional freezing specifically comprises:
[0080] placing the mixed dispersion in a mold, and placing the bottom of the mold in a cold source for directional freezing;
[0081] The mold is made of heat-conducting metal, the cold source is liquid nitrogen, and the directional freezing time is 5 to 15 minutes.
[0082] Specifically, the mixed dispersion is placed in a mold, the material of the mold is preferably a heat-conducting metal, more preferably copper or iron; the cold source preferably includes liquid nitrogen; the time for directional freezing is preferably 5 to 15 minutes, more preferably 7 to 13 minutes; the bottom surface of the mold is placed in the cold source for directional freezing.
[0083] In some embodiments, before placing the mixed dispersion into the mold, the mold is placed in a cold source for precooling, and the precooling time is 5 to 8 minutes.
[0084] In some embodiments, in step S2, the freeze-drying temperature is -30 to -65°C, preferably -40 to 60°C; the freeze-drying time is 24 to 72 hours, preferably 52 to 60 hours.
[0085] In some embodiments, a method for preparing a polyacrylonitrile nanofiber dispersion comprises the following steps:
[0086] S11, spinning the polyacrylonitrile solution into polyacrylonitrile nanofibers by electrospinning;
[0087] S12, dispersing the polyacrylonitrile nanofibers into water, and performing homogenization and crushing treatment to make the polyacrylonitrile nanofibers short fibers, to obtain a polyacrylonitrile nanofiber dispersion;
[0088] The diameter of the polyacrylonitrile nanofibers is 500 to 680 nm and the length is 45 to 60 μm.
[0089] In some embodiments, the method for preparing water-soluble polyamic acid fiber comprises the following steps:
[0090] S21, adding 4,4'-diaminodiphenyl ether and pyromellitic acid dianhydride to N,N-dimethylacetamide to carry out polycondensation reaction to obtain water-insoluble polyamic acid;
[0091] S22, mixing triethylamine with water-insoluble polyamic acid to modify it and obtain a water-soluble polyamic acid solution;
[0092] S23, subjecting the water-soluble polyamic acid solution to ice-water precipitation, and then freeze-drying to obtain water-soluble polyamic acid fibers.
[0093] In some embodiments, the polyacrylonitrile solution is obtained by dissolving polyacrylonitrile powder in an organic solvent, the organic solvent is preferably an amide solvent, more preferably N,N'-dimethylformamide (DMF); the dissolution temperature is preferably room temperature, the dissolution time is preferably 8 to 12 hours, more preferably 10 hours; the concentration of the polyacrylonitrile solution is 5 to 15 wt%; the electrospinning process includes: the extrusion speed is preferably 0.06 to 0.10 mm min -1, more preferably 0.07 to 0.09 mm min -1 ; The distance between the needle cylinder and the roller is preferably 15-25cm, more preferably 18-22cm; the voltage is preferably 10-14kV, more preferably 11-13kV; the process parameters controlled by the homogenization crushing process include: the temperature of the homogenization crushing is preferably 10-30℃, more preferably 20-25℃; the speed of the homogenization crushing is preferably 10000-16000rpm, more preferably 15000rpm; the time of the homogenization crushing is preferably 30-60min, more preferably 40-50min.
[0094] It can be understood that the polyacrylonitrile nanofibers are formed into polyacrylonitrile nanofibers after homogenization and crushing. The diameter of the polyacrylonitrile nanofibers is preferably 500-680 nm, more preferably 530-660 nm, and the length is preferably 45-60 μm.
[0095] In some embodiments, 4,4'-diaminodiphenyl ether (ODA) and pyromellitic acid dianhydride (PMDA) are added to N,N-dimethylacetamide, and polycondensation reaction is carried out at -10 to 0°C under an inert atmosphere for 4 to 8 hours to obtain a water-insoluble polyamic acid; wherein the molar ratio of 4,4'-diaminodiphenyl ether, pyromellitic acid dianhydride, and N,N-dimethylacetamide is (0.8 to 1.2):(0.8 to 1.2):(25 to 30);
[0096] The triethylamine and the water-insoluble polyamic acid are mixed and reacted at -10 to 0°C for 4 to 8 hours to obtain a water-soluble polyamic acid solution; wherein the molar ratio of 4,4'-diaminodiphenyl ether to triethylamine is 1:(0.6 to 1);
[0097] The water-soluble polyamic acid solution obtained by water precipitation is freeze-dried to obtain a solid product to obtain a water-soluble polyamic acid fiber; wherein the freeze-drying temperature is -30 to -65°C and the time is 24 to 72 hours.
[0098] In the above embodiment, water is added to the obtained water-soluble polyamic acid solution for precipitation, and the obtained solid product is freeze-dried to obtain water-soluble polyamic acid fibers; wherein, the amount of water is not particularly limited, as long as the precipitation product no longer increases.
[0099] Specifically, in some embodiments, the preparation method of water-soluble polyamic acid preferably includes the following steps: adding 4,4'-diaminodiphenyl ether and pyromellitic dianhydride to a polar solvent (recorded as the first mixing), performing a polycondensation reaction, and obtaining a water-insoluble polyamic acid; mixing triethylamine with the water-insoluble polyamic acid (recorded as the second mixing), performing modification, and obtaining a water-soluble polyamic acid solution; precipitating the water-soluble polyamic acid solution with ice water, and then freeze-drying to obtain a water-soluble polyamic acid fiber. In the present invention, the molar ratio of 4,4'-diaminodiphenyl ether (ODA) and pyromellitic dianhydride (PMDA) is preferably 1:1; the polar solvent is preferably an amide solvent: N,N'-dimethylacetamide (DMAc); the present invention has no special limitation on the amount of the polar solvent, as long as it can ensure that the polycondensation reaction proceeds smoothly. In the present invention, the temperature of the first mixing, condensation reaction, modification and second mixing is preferably independently -10 to 0°C, more preferably -5 to 0°C; the polycondensation reaction is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably an inert gas, more preferably argon or helium; the present invention has no special restrictions on the time of the first mixing and the second mixing, as long as the raw materials can be mixed evenly. In the present invention, the molar ratio of 4,4'-diaminodiphenyl ether to triethylamine is preferably 1: (0.6 to 1), more preferably 1: (0.9 to 1). The present invention has no special restrictions on the amount of ice water, and the ice water precipitation product is no longer increased. After completing the ice water precipitation, the present invention preferably further includes freeze-drying the obtained ice water precipitation product to obtain water-soluble polyamic acid nanofibers; the freeze-drying temperature is preferably -30 to -65°C, more preferably -40 to -60°C; the freeze-drying time is preferably 24 to 72h, more preferably 52 to 60h.
[0100] In some embodiments, a polyacrylonitrile nano-short fiber dispersion, water-soluble polyamic acid fiber, and lamellar montmorillonite are mixed to obtain a mixed dispersion. Specifically, the polyacrylonitrile nano-short fiber dispersion and the lamellar montmorillonite are first mixed and then homogenized. The homogenization speed is preferably 15,000 rpm, and the homogenization time is preferably 10 to 15 minutes. The obtained dispersion of polyacrylonitrile nano-short fibers and montmorillonite is mixed with the water-soluble polyamic acid fiber to obtain a mixed dispersion.
[0101] The present invention utilizes directional freezing technology to obtain macroporous oriented structure, and polyacrylonitrile nanofiber, polyamic acid and montmorillonite are squeezed by growing ice crystals to generate fiber wall during freezing, and macropores are generated after ice crystal sublimation, and secondary pores of mesopores and micropores are formed on fiber wall due to cross-entanglement of nano-level polyacrylonitrile staple fibers, and montmorillonite is evenly distributed on polyacrylonitrile nanofiber due to hydrogen bonding, and multiple concave structures are constructed, and polyamic acid is squeezed into the nodes of polyacrylonitrile nanofiber; polyamic acid firmly wraps polyacrylonitrile nanofiber after imidization and produces chemical crosslinking with it, and polyacrylonitrile is cyclized after self-heating at the node to produce chemical crosslinking; when aerogel is subjected to external pressure, stress is first concentrated at the node, and due to the strong crosslinking at the node, pressure can be well released, so that aerogel shows excellent resilience. The present invention utilizes hydrophilic polyacrylonitrile nanofiber, hydrophilic lamellar montmorillonite and hydrophobic polyamic acid to adjust the hydrophilicity and surface energy of aerogel, and multiple concave structures are constructed, so that aerogel shows underwater superoleophobicity and superhydrophobicity under oil. The preparation method provided by the invention is simple to operate, the preparation raw materials are low-toxic, easy to obtain, green and environmentally friendly, the production cost is low, and it is suitable for industrial production.
[0102] The polyacrylonitrile / polyimide-montmorillonite dual superphobic nanofiber composite aerogel prepared by the preparation method provided by the present invention has a multi-level pore structure, and the multi-level pore structure includes macropores, mesopores and micropores. The aerogel provided by the present invention has a macropore orientation and a multi-level pore structure and a multi-concave micro-nano structure, which gives the aerogel excellent separation efficiency, separation flux, mechanical properties and dual superphobic properties. The aerogel has good application prospects in the fields of offshore oil spill treatment, domestic oil and sewage separation, and sensors.
[0103] Based on the same inventive concept, the present invention also provides a polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel, which is prepared by the above-mentioned preparation method.
[0104] The polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel prepared by the invention has a multiple concave structure, and the multiple concave structure is a micro-nano structure composed of polyacrylonitrile nanofibers and two-dimensional lamellae montmorillonite.
[0105] The polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel prepared by the present invention has a contact angle of 0° with water or oil in air, an underwater oil contact angle and an oil underwater water contact angle both greater than 150°, and has double superphobic properties; the oil flux of the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel prepared by the present invention is (2.63±0.08~5.83±0.20)×10 4 L m -2 h -1, with a compression rebound of 81.43±0.84% at 40% strain, showing the excellent resilience of the aerogel.
[0106] Based on the same inventive concept, the present invention also provides a method for preparing polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel or the use of the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel as an oil-water separation material.
[0107] The polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel of the present invention is used as an oil-water separation material or an air filtration material. The polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel provided by the present invention has the advantages of double superphobic switchability, high recycling rate, macropore orientation, multi-level pore structure, high specific surface area, stable physical and chemical properties, etc., and is an ideal high-performance oil-water separation material. The aerogel has good application prospects in the fields of offshore oil spill treatment, domestic oil and sewage separation, and sensors.
[0108] The following further describes the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel and its preparation method and application of the present application with specific examples. This section further describes the content of the present invention in conjunction with specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0109] Example 1
[0110] The present invention provides a method for preparing a polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel, comprising the following steps:
[0111] S1. Add polyacrylonitrile powder to N,N'-dimethylformamide, and stir and mix at room temperature (25°C) for 10 hours to obtain a polyacrylonitrile solution with a concentration of 10 wt%;
[0112] The polyacrylonitrile solution was transferred to a 10 mL syringe for electrospinning to obtain polyacrylonitrile nanofibers (with a diameter of 530-660 nm). The electrospinning process conditions were as follows: an extrusion speed of 0.08 mm / min, a distance from the needle to the roller of 21 cm, and a voltage of 12 kV.
[0113] The polyacrylonitrile nanofibers were dispersed in deionized water, and subjected to a short-fiber treatment using a homogenizer at room temperature and 15,000 rpm for 45 minutes to obtain a polyacrylonitrile nanofiber dispersion (with a concentration of 7.5 wt % and a short fiber length of 45 to 60 μm);
[0114] S2, dissolving 4.31 g of 4,4'-diaminodiphenyl ether in 51 g of N,N'-dimethylacetamide, adding 4.69 g of pyromellitic anhydride, placing in an ice-water bath (0°C), and polycondensing for 5.5 hours under an argon atmosphere; then adding 2.18 g of triethylamine, continuing the reaction for 5.5 hours, adding 3 L of deionized water to the obtained water-soluble polyamic acid solution for precipitation, washing the obtained solid component with water and freeze-drying it at -55°C to constant weight, to obtain a water-soluble polyamic acid fiber;
[0115] S3, placing lamellar montmorillonite in a dispersion of polyacrylonitrile nano-short fibers, homogenizing for 15 min at room temperature and a rotation speed of 15000 rpm to obtain a stable dispersion containing polyacrylonitrile nano-short fibers and lamellar montmorillonite; wherein the mass of the lamellar montmorillonite added (the lamellar montmorillonite was purchased from Guzhang County Shanlin Shiyu Mineral Products Co., Ltd., and its model is CAS [1318-93-0]) is 10wt% of the mass of the polyacrylonitrile nano-short fibers in the dispersion of polyacrylonitrile nano-short fibers;
[0116] S4, placing the water-soluble polyamic acid fiber in the dispersion in S3, stirring at room temperature until the water-soluble polyamic acid fiber is completely dissolved, to obtain a mixed dispersion; wherein the mass of the water-soluble polyamic acid fiber is 10% of the mass of the polyacrylonitrile nano-short fiber in the polyacrylonitrile nano-short fiber dispersion;
[0117] S5, contacting the bottom surface of the iron mold with liquid nitrogen to precool the mold for 10 minutes; then transferring the mixed dispersion in S4 to the iron mold and directionally freezing it for 10 minutes; then freeze-drying it at -55°C for 48 hours to obtain polyacrylonitrile / polyamic acid-montmorillonite macroporous oriented nanofiber composite aerogel (denoted as PAN / PAA-MMT-10);
[0118] S6, placing the polyacrylonitrile / polyamic acid-montmorillonite macroporous oriented nanofiber composite aerogel in a tubular furnace, and performing a programmed imidization treatment in air to obtain a polyacrylonitrile-polyimide-montmorillonite dual superphobic nanocomposite aerogel (denoted as PAN / PI-MMT-10); wherein the imidization treatment process is: 5°C min -1 The heating rate was from room temperature to 100 °C and then kept at this temperature for 1 h, and then at 5 °C min -1 The temperature was raised to 200℃ at a rate of 1 h, then kept at 5℃min -1 The temperature was raised to 300°C at a rate of 1°C and kept at that temperature for 1 h.
[0119] Comparative Example 1
[0120] This comparative example provides a method for preparing a composite aerogel, which is the same as that in Example 1, except that in step S3, the mass of the lamellar montmorillonite added is 15wt% of the mass of the polyacrylonitrile nano-short fibers in the polyacrylonitrile nano-short fiber dispersion, and the other process parameters are the same as those in Example 1; the prepared composite aerogel is recorded as PAN / PI-MMT-15.
[0121] Comparative Example 2
[0122] This comparative example provides a method for preparing a composite aerogel, which is the same as that of Example 1, except that in step S3, lamellar montmorillonite is not added, and the other process parameters are the same as those of Example 1; the prepared composite aerogel is recorded as PAN / PI.
[0123] Performance Testing
[0124] (1) Scanning electron microscope test
[0125] Figure 1 is a scanning electron microscope image of the composite aerogel prepared in Example 1 and Comparative Examples 1-2; wherein (a 1 ) and (a 2 ) is PAN / PI prepared in Comparative Example 2, (b 1 ) and (b 2 ) is PAN / PI-MMT-10 prepared in Example 1, (c 1 ) and (c 2 ) are SEM images of PAN / PI-MMT-15 prepared in Comparative Example 1 at different magnifications.
[0126] Depend on Figure 1 It can be seen that the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel prepared by the present invention has a skeleton macroporous structure, the composite aerogel wall is composed of secondary pores formed by polyacrylonitrile nanofibers, and lamellar montmorillonite is distributed on the fiber surface to form multiple concave structures. Polyimide is used as an adhesive and cross-linking agent to connect polyacrylonitrile nanofibers to construct a double superphobic aerogel with a multi-level pore structure.
[0127] Figure 2 The contact angle test results of the composite aerogels prepared in Example 1 and Comparative Examples 1-2 are shown in FIG. 1 ) and (a 2 ) is PAN / PI prepared in Comparative Example 2, (b 1 ) and (b 2 ) is PAN / PI-MMT-10 prepared in Example 1, (c 1 ) and (c 2 ) is PAN / PI-MMT-15 prepared in Comparative Example 1. Figure 2 China, C.A. O / WRepresents the underwater oil contact angle of different nanocomposite aerogels, CA W / O Represents the water contact angle of different nanocomposite aerogels under oil.
[0128] Specifically, the contact angle test method is:
[0129] When testing the contact angle of water under oil, the operation is as follows: the aerogel is immersed in 30mL of n-hexane for 1 hour. At this time, the aerogel completely sinks to the bottom of the solvent and no bubbles emerge, and the oil-water test sample is obtained. Then it is placed in a glass box filled with n-hexane, 3μL of water is dropped on the surface of the aerogel, and the oil-water contact angle is recorded;
[0130] Underwater oil contact angle: Soak the aerogel in ethanol and water for 1 h in turn to make the inside of the aerogel completely filled with water. Then place the aerogel in an optical glass box filled with water, drop 5 μl of n-hexane on the sample surface, and observe the n-hexane contact angle.
[0131] Depend on Figure 2 It can be seen that the PAN / PI-MMT-10 prepared in Example 1 has an underwater oil contact angle and an oil-under-water contact angle greater than 150°, and has a dual superphobic property; while the underwater oil contact angle of the PAN / PI-MMT-15 prepared in Comparative Example 1 is less than 150°; the underwater oil contact angle and the oil-under-water contact angle of the PAN / PI prepared in Comparative Example 2 are both less than 150°; the aerogels prepared in Comparative Examples 1 to 2 can only achieve dual superphobicity. The contact angles of the PAN / PI-MMT-10 prepared in Example 1 with water or oil in air are all 0°.
[0132] (3) Oil-water separation performance test
[0133] Test method: Oil-water separation is carried out under the drive of liquid gravity, using a variety of oily organic solvents (including dichloromethane and n-hexane) and oil (vegetable oil and pump oil); a mixture of heavy oil (specifically dichloromethane) and water at a mass ratio of 4:1 and light oil (n-hexane, vegetable oil and pump oil) and water at a mass ratio of 1:4 is prepared, and homogenized at a speed of 10000rpm for 5 minutes using a high-speed homogenizer. The filtration efficiency is calculated by the oil mass formula before and after filtration:
[0134]
[0135] In the formula, m 0 and m 1 are the mass of oil before and after separation, respectively. The oil flux of aerogel can be calculated by Eq. 2
[0136]
[0137] Where V is the volume of the filtered liquid; A is the filtration area; t is the time required to filter a certain volume of liquid.
[0138] Figures 3-4 The oil-water separation test results of the composite aerogels prepared in Example 1 and Comparative Examples 1-2 are shown; Figure 3 It can be seen that the average efficiency of the composite aerogel prepared in Example 1 in filtering different oils is 95.43-99.31%, which is greater than that of Comparative Examples 1-2. Figure 4 It can be seen that the average flux of the composite aerogel prepared in Example 1 of the present invention for filtering different oils is 2.534-5.358×10 4 L m -2 h -1 .
[0139] (4) Rebound performance test
[0140] Test method: The compression resilience of the composite aerogels prepared in Example 1 and Comparative Examples 1-2 was tested using a high and low temperature material universal testing machine, using a 50N pressure sensor and a compression rate of 1.0 mm min -1 The test results are as follows: Figures 5 to 7 shown.
[0141] Depend on Figures 5 to 7 It can be seen that the polyacrylonitrile / polyimide-montmorillonite double superphobic nanofiber composite aerogel PAN / PI-MMT-10 prepared in Example 1 has a rebound rate of 81.43% at a strain of 40%, which is greater than the aerogels PAN / PI-MMT-15 and PAN / PI prepared in Comparative Examples 1 to 2, and has excellent compression resilience.
[0142] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel, characterized in that: The following steps are involved: Mixing a polyacrylonitrile nanofiber dispersion, a water-soluble polyamic acid fiber, and lamellar montmorillonite to obtain a mixed dispersion; Directingly freezing and freeze-drying the mixed dispersion in sequence to obtain polyacrylonitrile / polyamic acid-montmorillonite macroporous oriented nanofiber composite aerogel; The polyacrylonitrile / polyamic acid-montmorillonite macroporous oriented nanofiber composite aerogel is subjected to imidization treatment to obtain a polyacrylonitrile-polyimide-montmorillonite dual superphobic nanocomposite aerogel; The mass of the lamellar montmorillonite is 5-10% of the mass of the polyacrylonitrile nano-short fibers in the polyacrylonitrile nano-short fiber dispersion.
2. The method for preparing the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel according to claim 1, characterized in that: The concentration of the polyacrylonitrile nano short fiber dispersion is 6 to 16 wt %; The mass of the water-soluble polyamic acid fiber is 5-15% of the mass of the polyacrylonitrile nano-short fiber in the polyacrylonitrile nano-short fiber dispersion.
3. The method for preparing the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel according to claim 1, characterized in that: The imidization treatment comprises in sequence: Heating to a first temperature at a first heating rate to perform a first imidization treatment; Raising the temperature to a second temperature at a second heating rate to perform a second imidization treatment; heating to a third temperature at a third heating rate to perform a third imidization treatment; Wherein, the first temperature is 85-115°C, and the first imidization treatment time is 50-80min; The second temperature is 185-215° C., and the second imidization treatment time is 50-80 min; The third temperature is 285-315° C., and the third imidization treatment time is 50-80 min; The first heating rate, the second heating rate and the third heating rate are each independently 3-7°C min -1 ; And / or, the directional freezing specifically includes: placing the mixed dispersion in a mold, and placing the bottom of the mold in a cold source for directional freezing; The mold is made of heat-conducting metal, the cold source is liquid nitrogen, and the directional freezing time is 5 to 15 minutes. Before the mixed dispersion is placed in the mold, the mold is placed in a cold source for precooling, and the precooling time is 5 to 8 minutes.
4. The method for preparing the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel according to claim 1, characterized in that: The freeze-drying temperature is -30 to -65°C and the time is 24 to 72 hours.
5. The method for preparing the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel according to claim 1, characterized in that: The method for preparing the polyacrylonitrile nano short fiber dispersion comprises the following steps: The polyacrylonitrile solution was spun into polyacrylonitrile nanofibers by electrospinning; The polyacrylonitrile nanofibers are dispersed in water, and homogenized and crushed to make the polyacrylonitrile nanofibers short-fibered to obtain a polyacrylonitrile nanofiber dispersion; The diameter of the polyacrylonitrile nanofibers is 500 to 680 nm and the length is 45 to 60 μm.
6. The method for preparing the polyacrylonitrile-polyimide-montmorillonite sheet-montmorillonite double superphobic nanocomposite aerogel according to claim 1, characterized in that: The preparation method of the water-soluble polyamic acid fiber comprises the following steps: Adding 4,4'-diaminodiphenyl ether and pyromellitic acid dianhydride to N,N-dimethylacetamide to carry out polycondensation reaction to obtain water-insoluble polyamic acid; Mixing triethylamine with the water-insoluble polyamic acid to modify it and obtain a water-soluble polyamic acid solution; The water-soluble polyamic acid solution is subjected to ice water precipitation and then freeze-dried to obtain water-soluble polyamic acid fibers.
7. The method for preparing the polyacrylonitrile-polyimide-montmorillonite dual superphobic nanocomposite aerogel according to claim 5, characterized in that: Dissolving polyacrylonitrile powder in an organic solvent to obtain a polyacrylonitrile solution; wherein the concentration of the polyacrylonitrile solution is 5 to 15 wt %; and the organic solvent comprises an amide solvent; The working parameters of electrospinning control include: extrusion speed is 0.06~0.10mm min -1 , the spinning voltage is 10~14kV; The process parameters of the homogenization crushing process control include: the homogenization crushing temperature is 10-30°C, the rotation speed is 10000-16000rpm, and the time is 30-60min.
8. The method for preparing the polyacrylonitrile-polyimide-montmorillonite dual superphobic nanocomposite aerogel according to claim 6, characterized in that: Add 4,4'-diaminodiphenyl ether and pyromellitic acid dianhydride to N,N-dimethylacetamide, and carry out polycondensation reaction at -10 to 0°C under an inert atmosphere for 4 to 8 hours to obtain water-insoluble polyamic acid; wherein the molar ratio of 4,4'-diaminodiphenyl ether, pyromellitic acid dianhydride and N,N-dimethylacetamide is (0.8 to 1.2):(0.8 to 1.2):(25 to 30); The triethylamine and the water-insoluble polyamic acid are mixed, and the reaction is continued at -10 to 0°C for 4 to 8 hours to obtain a water-soluble polyamic acid solution; wherein the molar ratio of 4,4'-diaminodiphenyl ether to triethylamine is 1:(0.6 to 1); Water is added to the obtained water-soluble polyamic acid solution for precipitation, and the obtained solid product is freeze-dried to obtain water-soluble polyamic acid fiber; wherein the freeze-drying temperature is -30 to -65°C and the time is 24 to 72 hours.
9. A polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel, characterized in that: The preparation is obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel prepared by the preparation method according to any one of claims 1 to 8 or the polyacrylonitrile-polyimide-montmorillonite double superphobic nanocomposite aerogel according to claim 9 as an oil-water separation material or an air filtration material.
Citation Information
Patent Citations
Inorganic / organic composite polyimide-based nanofiber membranes, their preparation methods and applications
CN102277648A
Polyacrylonitrile nanofiber / polyimide-based carbon aerogel adsorption material and preparation method thereof
CN105923622A
Double-seal waterproof thermal insulation material and preparation method and application thereof
CN114103332A
Polyacrylonitrile-polyimide macroporous oriented nanofiber composite aerogel as well as preparation method and application thereof
CN115895159A
Nanofiber composite aerogel as well as preparation method and application thereof
CN116199931A