Preparation method of waterproof breathable film and waterproof breathable fabric

Through the water bath ultrasonic dispersion technology of polyurethane resin and N,N-dimethylformamide, it forms a microporous waterproof and breathable membrane, and combines it with a nylon fiber surface cloth, solving the problem of insufficient breathable performance of the existing waterproof and breathable membrane, and improving outdoor sports Comfort and functionality of clothing.

CN119019749APending Publication Date: 2024-11-26FILA SPORTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411301238.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing waterproof and breathable membrane has weak breathable performance in outdoor sportswear, resulting in a reduced comfort level for users when wearing it, and cannot meet the functional needs of daily life or casual sports.

Method used

Polyurethane resin is mixed with N,N-dimethylformamide, and it is completely dissolved by ultrasonic dispersion of water bath to form cast film liquid. After laying on the substrate, it is immersed in deionized water to form micropores, and then extracting excess N,N -Dimethylformamide, the waterproof and breathable membrane produced has better breathable properties. This method controls the viscosity of the polyurethane resin within the range of 1500Pa·s-2000Pa·s, ensures the appropriate size and number of micropores, and combines the adhesive connection of the nylon fiber surface cloth to form a waterproof and breathable fabric.

Benefits of technology

The air permeability and mechanical properties of the waterproof breathable membrane are improved, and the stability and durability of the waterproof breathable membrane are ensured. At the same time, micropore clogs caused by glue coverage are avoided, which enhances the comfort and functionality of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019749A_ABST
    Figure CN119019749A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a waterproof breathable film and a waterproof breathable fabric, the preparation method comprises the following steps: mixing polyurethane resin with N, N-dimethylformamide, carrying out water bath ultrasonic dispersion until the mixture is dissolved, sealing and standing to obtain a film casting solution; laying the membrane casting solution on a substrate, and immersing the substrate in deionized water to form a membrane by the membrane casting solution; and separating the prepared membrane from the substrate, extracting excessive N, N-dimethylformamide, and airing to obtain the waterproof breathable membrane. Wherein the viscosity of the polyurethane resin ranges from 1,500 Pa * s to 2,000 Pa * s. The waterproof breathable film prepared by the preparation method has better breathability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof and breathable materials, and in particular to a method for preparing a waterproof and breathable membrane and a waterproof and breathable fabric. Background Art

[0002] With the rise of the trend of outdoor leisure sports among residents, the functional requirements for outdoor sportswear have become more diversified and professional. Previously, jackets were usually used in harsh outdoor off-road scenes. In order to avoid hypothermia, the waterproof performance of jackets was required to be high, but there was not much requirement for breathability. Therefore, the waterproof and breathable membranes developed for this scenario, such as PTFE membranes and non-porous PU membranes, focus more on waterproof performance, resulting in weak breathability despite its breathability. At present, outdoor sportswear such as jackets are also more common in daily life or leisure sports, but the waterproof and breathable membranes they use are still conventional materials with poor moisture discharge and breathability, resulting in reduced comfort for users when wearing them. Summary of the invention

[0003] The purpose of the present invention is to overcome the above-mentioned defects or problems existing in the background technology and provide a method for preparing a waterproof breathable membrane and a waterproof breathable fabric. The waterproof breathable membrane prepared by the preparation method has better breathability.

[0004] To achieve the above object, the present invention adopts the following technical solutions:

[0005] Technical solution 1: A method for preparing a waterproof breathable membrane, which includes the following steps: mixing a polyurethane resin with N,N-dimethylformamide, dispersing the mixture in a water bath until dissolved, sealing the mixture and allowing it to stand to obtain a casting liquid; laying the casting liquid on a substrate, and immersing the substrate in deionized water to form a film with the casting liquid; separating the prepared membrane from the substrate, extracting excess N,N-dimethylformamide, and drying the membrane to obtain the waterproof breathable membrane; wherein the viscosity of the polyurethane resin is in the range of 1500Pa·s-2000Pa·s.

[0006] Technical solution 2 based on technical solution 1: when the polyurethane resin and N,N-dimethylformamide are mixed, the mass ratio of the polyurethane resin to N,N-dimethylformamide is 0.2-0.3:1.

[0007] Technical solution three based on technical solution two: when the mixture of polyurethane resin and N,N-dimethylformamide is dispersed by water bath ultrasound, the water bath temperature is 60°C-70°C, and the dispersion time is 1h-2h.

[0008] Technical solution 4 based on technical solution 3: when laying the casting liquid on the substrate, the laying thickness of the casting liquid is 0.2mm-0.3mm.

[0009] Technical solution five based on technical solution four: the substrate is immersed in deionized water for 48h-72h.

[0010] Technical solution 6 based on technical solution 5: the drying time is 2h-3h, and the temperature is 20℃-30℃.

[0011] Technical solution seven based on technical solution six: the viscosity of the polyurethane resin is 1800 Pa·s.

[0012] In addition, the present invention also provides technical solution eight: a waterproof and breathable fabric, which uses a waterproof and breathable membrane prepared by the method for preparing a waterproof and breathable membrane described in any one of technical solutions one to six as an intermediate layer, and nylon fiber surface cloths are respectively bonded to both sides of the waterproof and breathable membrane.

[0013] Technical solution nine based on technical solution eight: the waterproof breathable membrane is connected to the nylon fiber surface cloth by gluing, the glue on the waterproof breathable membrane is distributed in dots, the thickness of the glue is 0.1mm-0.2mm, the diameter of the glue is 0.2mm-0.3mm, and the glue distributed on one side of the waterproof breathable membrane accounts for 20%-30% of the total area.

[0014] In addition, the present invention also provides technical solution ten: the nylon fiber surface cloth is laminated to the waterproof breathable membrane under the conditions of a temperature of 70°C-90°C and a pressure of 0.5MPa-1MPa, and after lamination, it is matured under the conditions of a temperature of 25°C-30°C and a humidity of 50%-80% to obtain the waterproof breathable fabric.

[0015] It can be seen from the above description of the present invention that, compared with the prior art, the present invention has the following beneficial effects:

[0016] The invention provides a method for preparing a waterproof breathable membrane. The method comprises the following steps: mixing polyurethane resin with N,N-dimethylformamide, using N,N-dimethylformamide as a solvent and polyurethane resin as a solute, and dispersing the polyurethane resin completely in N,N-dimethylformamide through water bath ultrasonic dispersion. Then, the obtained casting liquid is laid on a substrate to ensure that the thickness of the obtained membrane meets the requirements. Then, the substrate is immersed in deionized water. When the casting liquid is immersed in the deionized water, micropores are formed on the membrane due to phase separation. Then, excessive N,N-dimethylformamide is extracted in the deionized water. The extraction process further increases the number of formed micropores, and the final performance of the membrane can be ensured not to be affected by the residual N,N-dimethylformamide by removing the excess N,N-dimethylformamide. The micropores formed on the membrane can allow water vapor to pass through, but water molecules cannot pass through, so that the membrane has the effect of being waterproof and breathable. Moreover, since the number of micropores on the membrane is larger, the waterproof breathable membrane has better breathability. In particular, in the raw materials of the waterproof breathable membrane, the viscosity of the polyurethane resin is determined to be 1500Pa·s-2000Pa·s. Within this viscosity range, the size and quantity of the micropores on the waterproof breathable membrane are appropriate, ensuring that the waterproof breathable membrane not only has excellent waterproof and breathable properties, but also has good mechanical properties. The size stability of the micropores on the waterproof breathable membrane is better and it is not easy to tear. In the process of forming the membrane through phase separation, the process of N,N-dimethylformamide in the casting liquid being replaced and dissolved by water is more stable, and the micropores can also have better size consistency.

[0017] Among them, when the polyurethane resin and N,N-dimethylformamide are mixed, the mass ratio of the polyurethane resin to N,N-dimethylformamide is 0.2-0.3:1; the appropriate mass ratio of the solvent and the solution can ensure that the polyurethane resin is completely dissolved in N,N-dimethylformamide, so that the micropores on the formed waterproof and breathable membrane are more uniform; and at this mass ratio, the speed of phase separation can be controlled to avoid the situation where the phase separation speed is too fast and the micropore size consistency is poor, and at the same time, the structural strength and durability of the formed waterproof and breathable membrane can be better.

[0018] When the mixture of polyurethane resin and N,N-dimethylformamide is dispersed by water bath ultrasound, the water bath temperature is 60℃-70℃ and the dispersion time is 1h-2h; dispersion by water bath heating can avoid contamination of the mixture, and setting an appropriate water bath temperature can accelerate the dissolution of the polyurethane resin. Ultrasonic waves can effectively disperse the polyurethane resin particles into the solvent through the cavitation effect, and water bath heating reduces the viscosity of the mixture, and the energy of ultrasonic waves can more easily penetrate the mixture, thereby further improving the dispersion efficiency.

[0019] When laying the casting liquid on the substrate, the thickness of the casting liquid is 0.2mm-0.3mm, which can control the thickness of the final waterproof and breathable membrane. At the same time, this thickness range can ensure that the micropores on the membrane are evenly distributed during the phase separation process. If the thickness is too thin, it may lead to insufficient phase separation and uneven micropore distribution. If the thickness is too thick, the micropores formed will be too large, affecting the waterproof effect. In addition, the appropriate thickness can also ensure that the casting liquid is laid evenly during the laying process, making the flatness and uniformity of the membrane better.

[0020] The substrate is immersed in deionized water for 48h-72h to ensure that the phase separation process is fully carried out, and the micropore structure and distribution can be adjusted to ensure the stability of the mechanical properties of the membrane.

[0021] The drying time is set to 2h-3h and the temperature is 20℃-30℃, which can remove residual moisture on the surface and in the gaps of the membrane to avoid affecting the mechanical properties and air permeability of the membrane. At the same time, the slow evaporation of moisture can gradually stabilize the microporous structure on the membrane and will not cause uneven tension inside the membrane due to excessively fast drying speed, thereby avoiding collapse or shrinkage of the microporous structure on the membrane.

[0022] In addition, the present invention also provides a waterproof and breathable fabric, which uses the waterproof and breathable membrane prepared above as an intermediate layer and has nylon fiber surface cloths attached to both sides, so that the waterproof and breathable fabric has excellent mechanical properties and good waterproof and breathable effects.

[0023] Among them, the waterproof breathable membrane and the nylon fiber face cloth are connected by gluing. The glue on the waterproof breathable membrane is distributed in a dotted manner, and the thickness, diameter and area occupied by the glue are limited to ensure that the breathable effect of the waterproof breathable membrane will not fail. If the coverage area of ​​the glue is too large, it may clog the micropores on the membrane, thereby reducing the breathability of the membrane, and may also destroy the waterproof performance of the membrane.

[0024] At the same time, laminating the nylon fiber face cloth and the waterproof breathable membrane under appropriate conditions can ensure that the two are fully bonded. The limited temperature range can increase the activity of the glue without destroying the performance of the glue, ensuring strong bonding. The limited pressure range can avoid effective glue bonding without damaging the membrane. The purpose of the subsequent aging process is to completely cure the glue and ensure strong bonding. The limited humidity range can ensure the flexibility of the fabric during the bonding process and ensure the bonding effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0026] Figure 1 A waterproof breathable membrane prepared by the method for preparing a waterproof breathable membrane provided in Example 2 of the present invention;

[0027] Figure 2 This is the waterproof and breathable membrane provided for Comparative Example 3. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are preferred embodiments of the present invention and should not be regarded as excluding other embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] In the claims, description and drawings of the present invention, if the terms "include", "have" and their variations are used, they are intended to mean "including but not limited to".

[0030] The invention provides a method for preparing a waterproof breathable membrane and a waterproof breathable fabric made of the waterproof breathable membrane obtained by the preparation method.

[0031] The method for preparing the waterproof breathable membrane mainly comprises the following steps:

[0032] Step 1: Mix the polyurethane resin and N,N-dimethylformamide, disperse them in a water bath until they are dissolved, seal them and let them stand to obtain a casting solution;

[0033] Step 2: Laying a casting solution on a substrate, and immersing the substrate in deionized water to allow the casting solution to form a film through phase separation;

[0034] Step 3: Separate the prepared membrane from the substrate, extract excess N,N-dimethylformamide in deionized water, and then dry it to obtain the waterproof and breathable membrane.

[0035] The viscosity of the polyurethane resin used in step 1 is in the range of 1500 Pa·s to 2000 Pa·s. As a preferred embodiment, the viscosity of the polyurethane resin can be selected to be 1800 Pa·s.

[0036] The preparation method comprises mixing polyurethane resin with N,N-dimethylformamide, using N,N-dimethylformamide as solvent and polyurethane resin as solute, dissolving the polyurethane resin completely in N,N-dimethylformamide through water bath ultrasonic dispersion, then laying the obtained casting liquid on a substrate to ensure that the thickness of the obtained film meets the requirements, and then immersing the substrate in deionized water. When the casting liquid is immersed in deionized water, micropores are formed on the film due to phase separation, and then the excess N,N-dimethylformamide is extracted in deionized water. This extraction process further increases the number of micropores formed, and the final performance of the film can be ensured not to be affected by the residue by removing the excess N,N-dimethylformamide; wherein the micropores formed on the film can allow water vapor to pass through, but not water molecules to pass through, which makes the film waterproof and breathable, and because the number of micropores on it is larger, the waterproof and breathable film has better breathability. In particular, in the raw materials of the waterproof breathable membrane, the viscosity of the polyurethane resin is determined to be 1500Pa·s-2000Pa·s. Within this viscosity range, the size and quantity of the micropores on the waterproof breathable membrane are appropriate, ensuring that the waterproof breathable membrane not only has excellent waterproof and breathable properties, but also has good mechanical properties. The size stability of the micropores on the waterproof breathable membrane is better and it is not easy to tear. In the process of forming the membrane through phase separation, the process of N,N-dimethylformamide in the casting liquid being replaced and dissolved by water is more stable, and the micropores can also have better size consistency.

[0037] In addition, in step 1, when the polyurethane resin and N,N-dimethylformamide are mixed, the mass ratio of the polyurethane resin to N,N-dimethylformamide is 0.2-0.3:1. The appropriate mass ratio of the solvent and the solution can ensure that the polyurethane resin is completely dissolved in N,N-dimethylformamide, so that the micropores on the formed waterproof and breathable membrane are more uniform; and under this mass ratio, the speed of phase separation can be controlled to avoid the situation where the micropore size consistency is poor due to the phase separation speed being too fast, and the structural strength and durability of the formed waterproof and breathable membrane can be better.

[0038] In step 1, when the mixture of polyurethane resin and N,N-dimethylformamide is dispersed by water bath ultrasound, the water bath temperature is 60°C-70°C and the dispersion time is 1h-2h. Dispersing by water bath heating can avoid contamination of the mixture, and setting an appropriate water bath temperature can accelerate the dissolution of the polyurethane resin. Ultrasonic waves can effectively disperse the polyurethane resin particles into the solvent through the cavitation effect, and water bath heating reduces the viscosity of the mixture, and the energy of ultrasonic waves can more easily penetrate the mixture, thereby further improving the dispersion efficiency.

[0039] In step 2, when the casting liquid is laid on the substrate, the thickness of the casting liquid is 0.2mm-0.3mm, which can control the thickness of the final waterproof and breathable membrane. At the same time, this thickness range can ensure that the micropores on the membrane are evenly distributed during the phase separation process. If the thickness is too thin, it may lead to insufficient phase separation and uneven distribution of micropores. If the thickness is too thick, the micropores formed will be too large, affecting the waterproof effect. In addition, the appropriate thickness can also ensure that the casting liquid is laid evenly during the laying process, so that the flatness and uniformity of the membrane are better.

[0040] In step 2, the substrate is immersed in deionized water for 48 hours to 72 hours, thereby ensuring that the phase separation process is fully carried out, and the micropore structure and distribution can be adjusted to ensure the stability of the mechanical properties of the membrane.

[0041] In step three, the drying time is set to 2h-3h and the temperature is 20℃-30℃, which can remove residual moisture on the surface and in the gaps of the membrane to avoid affecting the mechanical properties and air permeability of the membrane. At the same time, the slow evaporation of moisture can gradually stabilize the microporous structure on the membrane and will not cause uneven tension inside the membrane due to excessively fast drying speed, thereby avoiding collapse or shrinkage of the microporous structure on the membrane.

[0042] In addition, the waterproof and breathable fabric provided by the present invention uses the waterproof and breathable membrane prepared by the above-mentioned method for preparing the waterproof and breathable membrane as the middle layer, and nylon fiber surface cloths are respectively bonded to both sides of the waterproof and breathable membrane. Specifically, as a preferred embodiment, the nylon fiber surface cloth as the surface layer can be selected to adopt a nylon grade with high wear resistance, and a weaving method that improves wear resistance can be adopted, such as twill weaving and other weaving methods. The nylon fiber surface cloth as the inner layer can adopt a weaving method that can improve the softness of the fabric, for example, Torict nylon fabric can be used as the inner layer. The waterproof and breathable fabric uses the above-mentioned waterproof and breathable membrane as the middle layer, and nylon fiber surface cloths are bonded to both sides, so that the waterproof and breathable fabric has excellent mechanical properties and good waterproof and breathable effects.

[0043] The waterproof breathable membrane is connected to the nylon fiber surface cloth by gluing, the glue on the waterproof breathable membrane is distributed in dots, the thickness of the glue is 0.1mm-0.2mm, the diameter of the glue is 0.2mm-0.3mm, and the glue distributed on one side of the waterproof breathable membrane accounts for 20%-30% of the total area. The waterproof breathable membrane is connected to the nylon fiber surface cloth by gluing, the glue on the waterproof breathable membrane is distributed in dots, and the thickness, diameter and area occupied by the glue are limited to ensure that the ventilation effect of the waterproof breathable membrane will not fail, because if the coverage area of ​​the glue is too large, it may block the micropores on the membrane, thereby reducing the breathability of the membrane, and it may also destroy the waterproof performance of the membrane.

[0044] In addition, the nylon fiber face cloth is laminated with the waterproof breathable membrane at a temperature of 70°C-90°C and a pressure of 0.5MPa-1MPa, and then matured at a temperature of 25°C-30°C and a humidity of 50%-80% to obtain the waterproof breathable fabric. Laminating the nylon fiber face cloth with the waterproof breathable membrane under appropriate conditions can ensure that the two are fully bonded, wherein the limited temperature range can increase the activity of the glue without destroying the performance of the glue, ensuring firm bonding, and the limited pressure range can avoid effective bonding of the glue without damaging the membrane; the purpose of the subsequent aging process is to completely solidify the glue and ensure firm bonding, wherein the limited humidity range can ensure the flexibility of the fabric during bonding and ensure the bonding effect.

[0045] In order to further illustrate the performance of the above-mentioned waterproof breathable membrane, the following examples and comparative examples are provided.

[0046] Example 1

[0047] The waterproof and breathable membrane is prepared by the following steps:

[0048] Step 1: Mix the polyurethane resin and N,N-dimethylformamide, disperse them in a water bath until they are dissolved, seal them and let them stand to obtain a casting solution;

[0049] Step 2: Laying a casting solution on a substrate, and immersing the substrate in deionized water to allow the casting solution to form a film through phase separation;

[0050] Step 3: Separate the prepared membrane from the substrate, extract excess N,N-dimethylformamide in deionized water, and then dry it to obtain the waterproof and breathable membrane.

[0051] Wherein, in step 1, the viscosity of the polyurethane resin is selected to be 1500 Pa·s, and the brand is Aladdin 5280. The mass ratio of the polyurethane resin to N,N-dimethylformamide is 0.2:1. The water bath temperature is 60°C, and the dispersion time is 1.5h.

[0052] In step 2, the substrate is made of a glass plate, the casting solution is laid with a thickness of 0.2 mm, and the time of immersion in deionized water is 48 hours.

[0053] In step 3, the drying time is 2 hours and the temperature is 20°C.

[0054] Example 2

[0055] The waterproof and breathable membrane is prepared by the following steps:

[0056] Step 1: Mix the polyurethane resin and N,N-dimethylformamide, disperse them in a water bath until they are dissolved, seal them and let them stand to obtain a casting solution;

[0057] Step 2: Laying a casting solution on a substrate, and immersing the substrate in deionized water to allow the casting solution to form a film through phase separation;

[0058] Step 3: Separate the prepared membrane from the substrate, extract excess N,N-dimethylformamide in deionized water, and then dry it to obtain the waterproof and breathable membrane.

[0059] In step 1, the viscosity of the polyurethane resin is selected to be 1800 Pa·s, and the brand is Aladdin 5280. The mass ratio of the polyurethane resin to N,N-dimethylformamide is 0.25:1. The water bath temperature is 65° C., and the dispersion time is 1.5 h.

[0060] In step 2, the substrate is made of a glass plate, the casting solution is laid with a thickness of 0.25 mm, and the time of immersion in deionized water is 60 hours.

[0061] In step 3, the drying time is 2.5 hours and the temperature is 25°C.

[0062] Example 3

[0063] The waterproof and breathable membrane is prepared by the following steps:

[0064] Step 1: Mix the polyurethane resin and N,N-dimethylformamide, disperse them in a water bath until they are dissolved, seal them and let them stand to obtain a casting solution;

[0065] Step 2: Laying a casting solution on a substrate, and immersing the substrate in deionized water to allow the casting solution to form a film through phase separation;

[0066] Step 3: Separate the prepared membrane from the substrate, extract excess N,N-dimethylformamide in deionized water, and then dry it to obtain the waterproof and breathable membrane.

[0067] Wherein, in step 1, the viscosity of the polyurethane resin is selected to be 2000 Pa·s, and the brand is Aladdin 5280. The mass ratio of the polyurethane resin to N,N-dimethylformamide is 0.3:1. The water bath temperature is 70°C, and the dispersion time is 2h.

[0068] In step 2, the substrate is made of a glass plate, the casting solution is laid with a thickness of 0.3 mm, and the time of immersion in deionized water is 72 hours.

[0069] In step 3, the drying time is 3 hours and the temperature is 30°C.

[0070] Comparative Example 1

[0071] Comparative Example 1 is based on Example 2, and differs from Example 2 in that the viscosity of the polyurethane resin is selected to be 3500 Pa·s.

[0072] Comparative Example 2

[0073] Comparative Example 2 is based on Example 2, and differs from Example 2 in that the mass ratio of the polyurethane resin to N,N-dimethylformamide is 0.1:1.

[0074] Comparative Example 3

[0075] Comparative Example 3 is a commercially available hydrophilic polyurethane nonporous membrane, produced by Dongguan Weixin Polymer Materials Co., Ltd., with a thickness of 14.5 μm and a total weight of 14 g / m 2 .

[0076] The waterproof and breathable membranes provided in the above-mentioned Examples 1 to 3 and Comparative Examples 1 to 3 are used as the middle layer, and nylon fiber surface fabrics are laminated on both sides thereof, and the nylon fiber surface fabrics laminated in all the Examples and Comparative Examples are the same, so as to prepare waterproof and breathable fabrics. The relevant lamination parameters are as follows: the glue thickness is 0.15 mm, the diameter is 0.25 mm, the glue distributed on one side accounts for 25% of the total area, the lamination is carried out at 80°C and 1 MPa, and the aging is carried out at 30°C and 70% humidity.

[0077] Reference Figure 1 , which shows a microscopic schematic diagram of the waterproof breathable membrane prepared in Example 2, and referring to Figure 2 , which shows a microscopic schematic diagram of the polyurethane non-porous membrane provided in Example 3.

[0078] The waterproof and breathable fabric prepared above was tested, and the test items and standards are as follows:

[0079] Water vapor transmission rate test: in accordance with GB / T 12704.1-2009 (calcium chloride method);

[0080] Air permeability test: GB / T 5453-1997;

[0081] Hydrostatic pressure test: in accordance with GB / T 8629-2017.

[0082] The test results are as follows:

[0083]

[0084]

[0085] It can be seen from the above test results that Examples 1, 2, and 3 all have good waterproof and breathable properties. Although Comparative Example 3 has better waterproof performance, its breathability is poor and it is difficult to meet the user's wearing comfort requirements. The test results of moisture permeability, air permeability, and hydrostatic pressure of Comparative Example 1 are worse than those of Examples 1, 2, and 3. This is because the viscosity of the polyurethane resin used is too large, resulting in poor consistency in the size of the micropores on the membrane. Some micropores are too large, and some are too small, resulting in the membrane failing to meet the requirements in terms of air permeability and waterproof performance; Comparative Example 2 has better moisture permeability and air permeability, but its waterproof performance is poor. This is because the porosity of the membrane increases, and the size of the micropores increases, resulting in improved air permeability, but due to its poor waterproof performance, it cannot meet functional requirements.

[0086] The description of the above specification and embodiments is used to explain the protection scope of the present invention, but does not constitute a limitation on the protection scope of the present invention. Through the enlightenment of the present invention or the above embodiments, ordinary technicians in this field can obtain modifications, equivalent substitutions or other improvements to the embodiments of the present invention or part of the technical features thereof through logical analysis, reasoning or limited experiments, which should be included in the protection scope of the present invention.

Claims

1. A method for preparing a waterproof breathable membrane, characterized in that: The following steps are involved: The polyurethane resin is mixed with N,N-dimethylformamide, dispersed by ultrasonication in a water bath until dissolved, and then sealed and allowed to stand to obtain a casting solution; Laying a film casting solution on a substrate, and immersing the substrate in deionized water, so that the film casting solution forms a film through phase separation; The prepared membrane is separated from the substrate, and after the excess N,N-dimethylformamide is extracted in deionized water, it is dried to obtain the waterproof and breathable membrane; Wherein, the viscosity of the polyurethane resin ranges from 1500 Pa·s to 2000 Pa·s.

2. The method for preparing a waterproof breathable membrane according to claim 1, characterized in that: When the polyurethane resin and N,N-dimethylformamide are mixed, the mass ratio of the polyurethane resin to the N,N-dimethylformamide is 0.2-0.3:

1.

3. The method for preparing a waterproof breathable membrane according to claim 2, characterized in that: When the mixture of the polyurethane resin and N,N-dimethylformamide is dispersed by water bath ultrasound, the water bath temperature is 60° C.-70° C., and the dispersion time is 1 h-2 h.

4. The method for preparing a waterproof breathable membrane according to claim 3, characterized in that: When the casting liquid is laid on the substrate, the thickness of the casting liquid is 0.2 mm to 0.3 mm.

5. The method for preparing a waterproof breathable membrane according to claim 4, characterized in that: The substrate is immersed in deionized water for 48 h to 72 h.

6. The method for preparing a waterproof breathable membrane according to claim 5, characterized in that: The drying time is 2h-3h, and the temperature is 20℃-30℃.

7. The method for preparing a waterproof breathable membrane according to claim 1, characterized in that: The viscosity of the polyurethane resin is 1800 Pa·s.

8. A waterproof and breathable fabric, characterized in that: The waterproof breathable membrane prepared by the method for preparing the waterproof breathable membrane according to any one of claims 1 to 6 is used as the middle layer, and nylon fiber surface cloths are respectively attached to both sides of the waterproof breathable membrane.

9. The waterproof and breathable fabric according to claim 8, characterized in that: The waterproof breathable membrane is connected to the nylon fiber surface cloth by gluing. The glue on the waterproof breathable membrane is distributed in dots, the thickness of the glue is 0.1mm-0.2mm, the diameter of the glue is 0.2mm-0.3mm, and the glue distributed on one side of the waterproof breathable membrane accounts for 20%-30% of the total area.

10. The waterproof and breathable fabric according to claim 9, characterized in that: The nylon fiber surface cloth is laminated with the waterproof breathable membrane at a temperature of 70°C-90°C and a pressure of 0.5MPa-1MPa, and then cured at a temperature of 25°C-30°C and a humidity of 50%-80% to obtain the waterproof breathable fabric.