Room temperature curing electromagnetic shielding chloroprene rubber sealing rubber and preparation method and application thereof
By using a combination of neoprene and organic solvents, combined with the crosslinking reaction of zinc oxide and phenylmethane triisocyanate, the problem of insufficient room temperature curing depth in the prior art is solved, deep curing and high viscosity are achieved, and electromagnetic shielding is ensured. The durability and efficient performance of sealing rubber.
Patent Information
- Application Number
- CN202411287100.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The existing room-temperature cured silicone rubber has limited curing depth in deep gaps, which is prone to layering and self-flow of fillers, resulting in failure of electromagnetic shielding protection.
Neoprene is used as the matrix, and the combination of chloroprene kneading glue and organic solvents is used to convert neoprene into diene structure crosslinking by using zinc oxide and phenylmethane triisocyanate, forming a chemical bridge with magnesium oxide and 2402 phenolic resin. , realize deep room temperature curing, and build a conductive network through conductive metal powder and conductive reinforcement to enhance adhesion and conductivity.
It realizes deep curing and high viscosity at room temperature, ensures the durability and reliability of electromagnetic shielding protection, provides efficient electromagnetic shielding performance and stable construction.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electromagnetic shielding materials, and in particular to a room temperature curing electromagnetic shielding chloroprene rubber sealing rubber and a preparation method and application thereof. Background Art
[0002] In the current information age, electromagnetic interference and radiation from electronic devices are everywhere, which leads to the generation of a large amount of electromagnetic radiation, resulting in serious side effects such as electromagnetic interference and electromagnetic compatibility, which are potentially harmful to the normal operation of electronic equipment and human health. As a flexible material, electromagnetic shielding rubber material can overcome the defects of traditional electromagnetic shielding materials such as difficulty in processing, high density, and corrosion resistance, and is a new development direction of electromagnetic shielding materials.
[0003] Existing electromagnetic shielding rubber types include rubber patches, sealing strips and sealing rubber. For electromagnetic protection in gaps, sealing rubber is required for sealing. At present, the industry often uses room temperature curing silicone rubber to prepare electromagnetic shielding sealing rubber, but since the curing principle of this type of rubber is moisture curing, the curing depth is only 2~4mm, which is difficult to cure in deep gaps. It is easy to cause stratification of fillers and rubber or self-flow of sealing rubber under the action of gravity, resulting in failure of electromagnetic shielding protection. Therefore, it is particularly important to develop a high-performance electromagnetic shielding sealing rubber that can achieve deep curing at room temperature. Summary of the invention
[0004] In view of the shortcomings of the above background technology, the present invention provides a room temperature curing electromagnetic shielding chloroprene rubber sealing rubber and its preparation method and application. The present invention uses chloroprene rubber as a matrix and is expected to prepare an electromagnetic shielding sealing rubber material with high viscosity, easy construction, and deep curing at room temperature.
[0005] To achieve the above objectives, the first objective of the present invention is to provide a room temperature curing electromagnetic shielding chloroprene rubber sealing rubber, comprising component A and component B; The component A comprises a first organic solvent and chloroprene rubber; The chloroprene rubber compound comprises the following components by weight: 100 parts of chloroprene rubber dry glue, 150-400 parts of conductive metal powder, 1-5 parts of conductive reinforcing agent, 3-8 parts of magnesium oxide, 10-20 parts of tackifier, 2-8 parts of anti-settling agent, and 3-8 parts of zinc oxide; the mass ratio of the chloroprene rubber compound to the first organic solvent is 1:(1-2); The B component includes triphenylmethane triisocyanate, dibutyltin dilaurate and a second organic solvent; The mass ratio of the triphenylmethane triisocyanate, dibutyltin dilaurate and the second organic solvent is 1:0.001-0.002:2-4.
[0006] Preferably, the chloroprene rubber dry glue brand is one or more of A-90, A-100, SN242A, SN242B, SN243, and CR244.
[0007] Preferably, the metal powder is one or more of silver-coated copper, silver-coated aluminum, and silver-coated hollow glass microspheres; and the particle size of the metal powder is 10-50 μm.
[0008] Preferably, the conductive reinforcing agent is one or more of silver powder, conductive carbon black, graphene, and carbon nanotubes; wherein the silver powder has a particle size of 1 to 20 μm.
[0009] Preferably, the magnesium oxide is highly active magnesium oxide with an iodine absorption value of 80-180 mg / g; and the zinc oxide is highly active zinc oxide and / or indirect zinc oxide.
[0010] Preferably, the tackifier is a blend of rosin resin, terpene resin, 2402 phenolic resin, and polyisobutylene, and the mass ratio thereof is (1-3): 1:1:1; The anti-settling agent is fumed silica and / or bentonite.
[0011] Preferably, the first organic solvent and the second organic solvent are both dichloromethane.
[0012] The second object of the present invention is to provide a method for preparing a room temperature curing electromagnetic shielding chloroprene rubber sealing rubber, comprising the following steps: In an open mixing mill, chloroprene rubber is plasticized, magnesium oxide, a tackifier, an anti-settling agent, a conductive metal powder, and a conductive reinforcing agent are added, and zinc oxide is added after mixing evenly, and the mixture is mixed evenly again, and then the rubber is discharged and cooled to obtain a mixed rubber; Dissolving the rubber compound in an organic solvent to obtain component A; Triphenylmethane triisocyanate and dibutyltin dilaurate are dissolved in an organic solvent to obtain a B component.
[0013] The third object of the present invention is to provide a method for using a room temperature curing electromagnetic shielding chloroprene rubber sealing rubber, comprising the following steps: Shake component A thoroughly before use, then mix component A and component B thoroughly in a container and then apply; The mass ratio of component A to component B is 80:(1~2).
[0014] The fourth object of the present invention is to provide a chloroprene rubber sealing rubber for use in electromagnetic shielding.
[0015] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a room temperature curing electromagnetic shielding chloroprene rubber sealing rubber and a preparation method and application thereof. The present invention converts chloroprene rubber into a diene structure under the action of zinc oxide and phenylmethane triisocyanate, and then crosslinks into a three-dimensional network, thereby achieving deep room temperature curing of chloroprene rubber, and using dibutyltin dilaurate as a catalyst to shorten the room temperature curing time; zinc oxide and magnesium oxide form a chelate with 2402 phenolic resin in a tackifier to achieve chemical bridging with chloroprene rubber, and the molecular chains of the tackifier are entangled with each other to construct a physical reinforcement network, thereby synergistically increasing the adhesion performance of the system; the conductive metal powder has a large particle size and is easier to build a conductive network that contacts each other, and the conductive reinforcing agent has a small particle size and is dispersed inside the system to fill the gaps in the conductive network, thereby achieving high conductivity; the use of an anti-settling agent reduces the rapid sedimentation of the filler, thereby ensuring the stability of the sealing rubber construction.
[0016] The electromagnetic shielding sealing rubber prepared by the preparation method provided by the present invention can achieve deep curing at room temperature; the prepared electromagnetic shielding sealing rubber has both high shielding performance and high viscosity; the prepared electromagnetic shielding sealing rubber has long-lasting viscosity, ensuring the durability and reliability of electromagnetic shielding protection. DETAILED DESCRIPTION
[0017] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments, but the embodiments are not intended to limit the present invention.
[0018] The present invention is mainly aimed at the fact that due to the presence of chlorine atoms in the molecular chain of chloroprene rubber, chlorine atoms can be replaced by metal oxides to achieve cross-linking, which is different from the moisture curing principle and can achieve deep curing. In addition, the adhesive made of chloroprene rubber has a good bonding effect and can be used for bonding various materials such as rubber, plastic, artificial leather, ceramics, concrete, metal materials, etc., and has a wide range of applications. Therefore, using chloroprene rubber as a matrix is expected to prepare an electromagnetic shielding sealing rubber material with high viscosity, easy construction, and room temperature deep curing.
[0019] A first aspect of the present invention provides a room temperature curing electromagnetic shielding chloroprene rubber sealing rubber, comprising component A and component B; The component A comprises a first organic solvent and chloroprene rubber; The chloroprene rubber compound comprises the following components by weight: 100 parts of chloroprene rubber dry glue, 150-400 parts of conductive metal powder, 1-5 parts of conductive reinforcing agent, 3-8 parts of magnesium oxide, 10-20 parts of tackifier, 2-8 parts of anti-settling agent, and 3-8 parts of zinc oxide; the mass ratio of the chloroprene rubber compound to the first organic solvent is 1:(1-2); The B component includes triphenylmethane triisocyanate, dibutyltin dilaurate and a second organic solvent; The mass ratio of the triphenylmethane triisocyanate, dibutyltin dilaurate and the second organic solvent is 1:0.001-0.002:2-4.
[0020] The chloroprene rubber adhesive is one or more chloroprene rubber adhesives of the grades A-90, A-100, SN242A, SN242B, SN243, and CR244.
[0021] The metal powder is one or more of silver-coated copper, silver-coated aluminum, and silver-coated hollow glass microspheres; the particle size of the metal powder is 10-50 μm.
[0022] The conductive reinforcing agent is one or more of silver powder, conductive carbon black, graphene, and carbon nanotubes; wherein the silver powder has a particle size of 1 to 20 μm.
[0023] The magnesium oxide is high-activity magnesium oxide, and the iodine absorption value is 80-180 mg / g; the zinc oxide is high-activity zinc oxide and / or indirect zinc oxide.
[0024] The tackifier is a blend of rosin resin, terpene resin, 2402 phenolic resin and polyisobutylene, and the mass ratio thereof is (1-3): 1:1:1; The anti-settling agent is fumed silica and / or bentonite.
[0025] The first organic solvent and the second organic solvent are both dichloromethane.
[0026] A second aspect of the present invention provides a method for preparing a room temperature curing electromagnetic shielding chloroprene rubber sealing rubber, comprising the following steps: In an open mixing mill, chloroprene rubber is plasticized, magnesium oxide, a tackifier, an anti-settling agent, a conductive metal powder, and a conductive reinforcing agent are added, and zinc oxide is added after mixing evenly, and the mixture is mixed evenly again, and then the rubber is discharged and cooled to obtain a mixed rubber; Dissolving the rubber compound in an organic solvent to obtain component A; Triphenylmethane triisocyanate and dibutyltin dilaurate are dissolved in an organic solvent to obtain a B component.
[0027] In one embodiment, a method for preparing an electromagnetic shielding sealing rubber comprises the following steps: In an open mixing mill, chloroprene rubber is plasticized, magnesium oxide, a tackifier, an anti-settling agent, a conductive metal powder and a conductive reinforcing agent are added, and zinc oxide is added after mixing evenly. After mixing evenly again, the rubber is discharged and cooled to obtain a mixed rubber.
[0028] The above-mentioned rubber compound is dissolved in an organic solvent to obtain component A.
[0029] The B component is obtained by dissolving triphenylmethane triisocyanate in an organic solvent.
[0030] A third aspect of the present invention provides a method for using a room temperature curing electromagnetic shielding chloroprene rubber sealing rubber, comprising the following steps: Shake component A thoroughly before use, then mix component A and component B thoroughly in a container and then apply; The mass ratio of component A to component B is 80:(1~2).
[0031] A fourth aspect of the present invention provides a chloroprene rubber sealing rubber for use in electromagnetic shielding.
[0032] It should be noted that the experimental methods used in the present invention are all conventional methods unless otherwise specified; the reagents and materials used are all commercially available unless otherwise specified.
[0033] The following embodiment provides a method for preparing a room temperature curing electromagnetic shielding chloroprene rubber sealing rubber, which is specifically as follows: According to the formula in Table 1, after weighing the materials according to the mass ratio, adjust the roller distance of the open mill, turn on the cooling water of the open mill, set the temperature of the open mill to 60°C, the speed of the front and rear rollers to 21:18r / min, and plasticize the chloroprene rubber thinly for 5 times, add magnesium oxide, tackifying resin, anti-settling agent, conductive metal powder, and conductive reinforcing agent, mix for 10 minutes, then add zinc oxide, mix again for 5 minutes, drain the glue, cool, and obtain the mixed rubber. Add dichloromethane and mixed rubber in a single-mouth flask in proportion, and use a polytetrafluoroethylene stirring paddle to stir and dissolve for 12 hours. After complete dissolution, take out and divide into component A.
[0034] Weigh phenylmethane triisocyanate, dibutyltin dilaurate and dichloromethane in proportion, stir to dissolve, and take out and divide into component B.
[0035] The components A and B are prepared in proportion to prepare the electromagnetic shielding chloroprene rubber sealing rubber for construction.
[0036] Table 1 Electromagnetic shielding chloroprene rubber sealing rubber formula (weight ratio) project Example 1 Example 2 Example 3 Example 4 Component A Neoprene Adhesive A-90 100 0 0 0 Neoprene adhesive SN242A 0 100 0 20 Neoprene adhesive CR244 0 0 100 80 Magnesium oxide 5 5 5 5 Silver coated aluminum powder 300 0 250 150 Silver coated copper powder 0 300 0 0 Silver powder 10 0 5 0 Conductive carbon black 0 10 0 5 Rosin resin 6 5 10 7 Terpene resin 3 5 5 3 Polyisobutylene 3 5 5 3 2402 phenolic resin 3 5 5 3 Fumed silica 2 2 2 5 Indirect zinc oxide 6 6 5 5 Dichloromethane 500 500 400 300 Component B Phenylmethane triisocyanate 5 5 4 3 Dibutyltin dilaurate 0.005 0.005 0.004 0.003 Dichloromethane 15 15 12 9 The sealing rubbers of Examples 1 to 4 were subjected to performance tests.
[0037] 1. Test the electromagnetic shielding performance of the rubber compound according to MIL-G-83528.
[0038] 2. Cure depth test: Pour the electromagnetic shielding neoprene sealant into several disposable plastic cups, scrape them flat, and cut the plastic cups at 12h, 24h, 48h, and 72h to observe the cure depth.
[0039] 3. Adhesion strength test: Take a common rubber sheet as the substrate, cut the rubber sheet into 25cm wide strips as the substrate, use a grinding wheel or sandpaper to grind the bonding surface of the two substrates, use a cleaning agent to wash away the surface debris, expose the fresh interface, brush the prepared electromagnetic shielding neoprene sealing rubber on the two substrates, dry for 20 minutes, continue to brush and dry 2 times, brush again, dry for 10 minutes, and bond the two substrates. After the sample is placed for 4h, 8h, 16h, 24h, and 48h, the sample is peeled 180° and the peeling force is tested at a test speed of 100mm / min.
[0040] Table 2 Performance of the embodiments project Example 1 Example 2 Example 3 Example 4 Electromagnetic shielding performance Shielding effectiveness, 10MHz 65 68 45 28 Shielding Effectiveness, 10GHz 85 88 58 42 Shielding Effectiveness, 18GHz 115 112 75 68 Curing depth 12h curing depth, mm 4.2 4.5 5.0 5.5 24h curing depth, mm 11.2 10.4 12.5 14.2 48h curing depth, mm 14.8 14.6 16.2 20.5 72h curing depth, mm 16.5 17.2 20.7 24.5 Adhesion strength 4h peeling force, N 12.5 12.5 21.2 25 8h peeling force, N 20.2 26.4 32.5 54.8 16h peeling force, N 49.5 62.2 72.5 78.4 24h peeling force, N 67.5 77.5 105 117.5 48h peeling force, N 72.5 82.4 110 135 From the results in Table 2, it can be seen that due to the synergistic effect of zinc oxide, phenylmethane triisocyanate and dibutyltin dilaurate, the present invention is guaranteed to achieve rapid and deep curing at room temperature; the chelation of zinc oxide and magnesium oxide with 2402 phenolic resin and the mutual entanglement between the tackifier achieve the high bonding strength of the present invention, the synergistic cooperation between the conductive metal powder and the conductive reinforcing agent constructs a complete conductive network to provide high conductivity and achieve excellent electromagnetic shielding effect; the anti-settling agent ensures the construction stability of the sealing rubber.
[0041] The electromagnetic shielding sealing rubber provided by the present invention has good electromagnetic shielding effect, high bonding strength with the substrate, high viscosity after 4 hours, and basically completes curing after 24 hours. The bonding force is not easy to decrease during use, the curing speed is fast, and the depth is large, which is of great significance for electromagnetic shielding protection in deep gaps.
[0042] The above is only the best implementation mode of the present invention, but the protection scope of the patent of the present invention is not limited to this. All technicians familiar with this technical field can also make various corresponding changes and deformations to the present invention. Under the premise of not violating the principles of the invention, they should all fall within the protection scope of the claims attached to the present invention.
Claims
1. A room temperature curing electromagnetic shielding chloroprene rubber sealing rubber, It is characterized in that It includes component A and component B; The component A comprises a first organic solvent and chloroprene rubber; The chloroprene rubber compound comprises the following components by weight: 100 parts of chloroprene rubber dry glue, 150-400 parts of conductive metal powder, 1-5 parts of conductive reinforcing agent, 3-8 parts of magnesium oxide, 10-20 parts of tackifier, 2-8 parts of anti-settling agent, and 3-8 parts of zinc oxide; the mass ratio of the chloroprene rubber compound to the first organic solvent is 1:(1-2); The B component includes triphenylmethane triisocyanate, dibutyltin dilaurate and a second organic solvent; The mass ratio of the triphenylmethane triisocyanate, dibutyltin dilaurate and the second organic solvent is 1:0.001-0.002:2-4.
2. The room temperature curing electromagnetic shielding chloroprene rubber sealing rubber according to claim 1, It is characterized in that The chloroprene rubber dry glue brand is one or more of A-90, A-100, SN242A, SN242B, SN243, and CR244.
3. The room temperature curing electromagnetic shielding chloroprene rubber sealing rubber according to claim 1, It is characterized in that The metal powder is one or more of silver-coated copper, silver-coated aluminum, and silver-coated hollow glass microspheres; the particle size of the metal powder is 10-50 μm.
4. The room temperature curing electromagnetic shielding chloroprene rubber sealing rubber according to claim 1, It is characterized in that The conductive reinforcing agent is one or more of silver powder, conductive carbon black, graphene, and carbon nanotubes; wherein the silver powder has a particle size of 1 to 20 μm.
5. The room temperature curing electromagnetic shielding chloroprene rubber sealing rubber according to claim 1, It is characterized in that The magnesium oxide is high-activity magnesium oxide, and the iodine absorption value is 80-180 mg / g; the zinc oxide is high-activity zinc oxide and / or indirect zinc oxide.
6. The room temperature curing electromagnetic shielding chloroprene rubber sealing rubber according to claim 1, It is characterized in that The tackifier is a blend of rosin resin, terpene resin, 2402 phenolic resin and polyisobutylene, and the mass ratio thereof is (1-3): 1:1:1; The anti-settling agent is fumed silica and / or bentonite.
7. The room temperature curing electromagnetic shielding chloroprene rubber sealing rubber according to claim 1, It is characterized in that The first organic solvent and the second organic solvent are both dichloromethane.
8. A method for preparing the room temperature curing electromagnetic shielding chloroprene rubber sealing rubber according to any one of claims 1 to 7, It is characterized in that The following steps are involved: In an open mixing mill, chloroprene rubber is plasticized, magnesium oxide, a tackifier, an anti-settling agent, a conductive metal powder, and a conductive reinforcing agent are added, and zinc oxide is added after mixing evenly, and the mixture is mixed evenly again, and then the rubber is discharged and cooled to obtain a mixed rubber; Dissolving the rubber compound in an organic solvent to obtain component A; Triphenylmethane triisocyanate and dibutyltin dilaurate are dissolved in an organic solvent to obtain a B component.
9. A method for using the room temperature curing electromagnetic shielding chloroprene rubber sealing rubber according to any one of claims 1 to 7, It is characterized in that The following steps are involved: Shake component A thoroughly before use, then mix component A and component B thoroughly in a container and then apply; The mass ratio of component A to component B is 80:(1~2).
10. Use of the chloroprene rubber sealing rubber according to any one of claims 1 to 7 in electromagnetic shielding.
Citation Information
Patent Citations
Normal-temperature-curable high-temperature-resistant conveyer belt adhesive and preparation and application method thereof
CN102153965A
Electromagnetic shielding rubber with high thermal conductivity, preparation method and application thereof
CN107236161A
Semi-conductive metal shielding water-blocking tape and preparation method thereof
CN109300596A
Graphene / silver-plated hollow glass microsphere electromagnetic shielding coating and preparation method thereof
CN110819220A