Composite material, preparation method and application thereof, and cable
By using thermosetting resin prepolymer in the cable and blending it with ant-proof agent, and adding curing agent and defoaming agent to form a high-temperature anti-anti-anti-composite material, the problem of anti-anti-anti-anti-anti-in-high-temperature environment is solved, and the problem of anti-anti-anti-anti-anti-in-high-temperature environment is improved. It has the effect and stability of ant prevention.
Patent Information
- Application Number
- CN202411191999.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-26
AI Technical Summary
Existing cables are prone to evaporation in high-temperature processing environments, resulting in poor termite control effects and affecting signal stability and safety.
Using a composite material, by blending the thermosetting resin prepolymer with ant-proof agent and adding a curing agent and defoaming agent, the ratio and mixing process of each component are controlled to form a high-temperature anti-anti-anti-composite material to ensure that The stability of ant-proof agent in high temperature environment.
It effectively reduces the volatility of ant-proof agent in high-temperature environments, improves the high-temperature resistance and ant-proof effect of the cable, and reduces the potential harm to the human body and the environment.
Smart Images

Figure CN119019818A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cable protection, and in particular to a composite material, a preparation method and application thereof, and a cable. Background Art
[0002] Termites are creatures that like moisture and heat, and the hot and humid operating environment of cables provides them with a suitable living environment.
[0003] Therefore, in the southern region, cables are very vulnerable to termite attacks, resulting in signal interruptions, traffic jams and control misoperation, which in turn cause huge economic losses. At present, the main way to prevent and control termites in cables is to add anti-termite agents to the outer sheath of the cable to achieve the anti-termite effect. However, the high temperature processing environment of the cable will accelerate the volatilization of the anti-termite agent, seriously affecting the long-term anti-termite performance of the cable.
[0004] Therefore, the prior art still needs to be improved. Summary of the invention
[0005] Based on this, it is necessary to provide an efficient, stable, highly heat-resistant and anti-ant composite material and its preparation method and application, and cable.
[0006] The present invention is achieved through the following technical solutions:
[0007] The first aspect of the present invention provides a composite material, wherein the raw materials for preparing the composite material include the following components by mass percentage:
[0008] Thermosetting resin prepolymer 50%~80%;
[0009] Anti-termite agent 1%~30%;
[0010] Curing agent 14%~40%;
[0011] Defoaming agent 0.5%~2%;
[0012] Wherein, the weight ratio of the thermosetting resin prepolymer to the anti-termite agent is (2~79):1.
[0013] The composite material of the present application is a mixture of an anti-termite agent and a high temperature resistant thermosetting resin, and a curing agent and a defoaming agent are introduced to work together. By controlling the specific ratio of each raw material, and controlling the specific weight percentage of the high temperature resistant thermosetting resin prepolymer and the anti-termite agent, each component works synergistically, so that after the curing agent is added, it has a temperature barrier effect on the internal anti-termite agent, while increasing the high temperature resistance of the composite material and maintaining good anti-termite performance. The composite material can be applied to high temperature processing environments, effectively improve the problem of anti-termite agent volatilization during processing, and reduce the harm of anti-termite agent volatilization to the human body and the environment.
[0014] In one embodiment, the raw materials for preparing the composite material include the following components by mass percentage:
[0015] High temperature resistant thermosetting resin prepolymer 60%~78%;
[0016] Anti-termite agent 1%~20%;
[0017] Curing agent 19%~38%;
[0018] Defoaming agent 0.5%~2%.
[0019] In one embodiment, the weight ratio of the high temperature resistant thermosetting resin prepolymer to the anti-termite agent is (35~78):1.
[0020] In one embodiment, the high temperature resistant thermosetting resin is selected from one or more of phenolic epoxy resin, hydrogenated epoxy resin, phenolic resin, and epoxy vinyl resin.
[0021] In one embodiment, the anti-termite agent is selected from one or more of imidacloprid, bifenthrin, fipronil and avermectin;
[0022] and / or, the defoamer is selected from one of polysiloxane, polyether and polyacrylate;
[0023] And / or, the curing agent is selected from one or more of p-phenylenediamine, tetrahydrophthalic anhydride, phthalic anhydride, maleic anhydride, diethylenetriamine, ethylenediamine, organic silicon amine curing agent, polyamide, fatty amine, propylene carbonate and butyl titanate.
[0024] A method for preparing a composite material comprises the following steps:
[0025] Providing raw materials according to the above composite materials; and
[0026] The raw materials are mixed and cured to obtain the composite material.
[0027] In one embodiment, mixing the raw materials for curing reaction comprises the following steps:
[0028] The high temperature resistant thermosetting prepolymer is first mixed with the anti-termite agent to obtain a first mixture;
[0029] adding the defoaming agent to the first mixture, performing a second mixing to obtain a second mixture;
[0030] The curing agent is added to the second mixture, and a third mixing is performed to obtain the composite material after a curing reaction.
[0031] In one embodiment, the first mixing conditions include: temperature of 20°C to 140°C, rotation speed of 300r / min to 3000r / min, and stirring time of 10min to 50min;
[0032] And / or, the conditions of the curing reaction include: a curing temperature of 30° C. to 180° C. and a curing time of 2 h to 15 h.
[0033] The second aspect of the present application also provides the use of the above-mentioned composite material in the preparation of cables.
[0034] The third aspect of the present application further provides a cable, comprising a conductor and a protective layer sleeved on the surface of the conductor, wherein the protective layer comprises the above-mentioned composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the SEM result of the composite material in Example 5;
[0036] Figure 2 This is the SEM result of imidacloprid original powder;
[0037] Figure 3 is a thermogravimetric curve of the composite material, imidacloprid and phenolic epoxy resin in Example 5;
[0038] Figure 4 is the ultraviolet absorption spectrum of the composite material in Example 5;
[0039] Figure 5 The graph is a result of the ultraviolet absorption intensity of imidacloprid at different concentrations at 270 nm in Example 5;
[0040] Figure 6 It is a standard curve diagram of imidacloprid concentration and ultraviolet absorption intensity in Example 5. DETAILED DESCRIPTION
[0041] References to embodiments of the present application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.
[0042] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features, and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.
[0043] The term "comprises", "comprising" or any other variant thereof is intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprising one..." do not exclude the presence of other identical elements in the process, method, article or equipment including the elements. The indefinite articles "a kind of" and "one" before the elements or components of the present application are not restrictive to the quantity requirements (i.e., the number of occurrences) of the elements or components. Therefore, "one" or "a kind of" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number obviously refers only to the singular form. The meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0044] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the weight described in the description of the embodiments of the present invention may be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0045] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. For example, therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0046] An embodiment of the present invention provides a composite material. The raw materials for preparing the composite material include the following components by mass percentage:
[0047] High temperature resistant thermosetting resin prepolymer 50%~80%;
[0048] Anti-termite agent 1%~30%;
[0049] Curing agent 14%~40%;
[0050] Defoaming agent 0.5%~2%;
[0051] Wherein, the weight ratio of the above-mentioned high temperature resistant thermosetting resin prepolymer to the above-mentioned anti-termite agent is (2~79):1.
[0052] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0053] It should be noted that the "50% to 80%" of the high temperature resistant thermosetting resin prepolymer can take a numerical range of 50% to 80%, and the range is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. For example, it includes but is not limited to: 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79% or 80%; or a range consisting of any two of these values, as an example, including: 60% to 80%.
[0054] The term "1% to 30%" for termite repellent can be a numerical range of 1% to 30%, which is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Examples include but are not limited to: 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29% or 30%; or a range consisting of any two of these values, including, for example, 1% to 20%.
[0055] The curing agent "14%~40%" can take a numerical range of 14%~40%, which is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. For example, it includes but is not limited to: 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39 or 40; or a range consisting of any two of these values, as an example, including: 20%~30%.
[0056] The defoaming agent "0.5%~2%" can take a numerical range of 0.5%~2%, which is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. For example, it includes but is not limited to: 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9% or 2%; or a range consisting of any two of these values, as an example, including: 0.5%~1%.
[0057] In some embodiments, the raw materials for preparing the composite material include the following components by mass percentage:
[0058] High temperature resistant thermosetting resin prepolymer 60%~78%;
[0059] Anti-termite agent 1%~20%;
[0060] Curing agent 19%~38%;
[0061] Defoaming agent 0.5%~2%.
[0062] Furthermore, by controlling the preparation raw materials within the preferred range, the high temperature resistance and anti-termite performance of the composite material are better.
[0063] In some of the embodiments, the weight ratio of the high temperature resistant thermosetting resin prepolymer to the anti-termite agent is (4-78):1.
[0064] In some of the embodiments, the weight ratio of the high temperature resistant thermosetting resin prepolymer to the anti-termite agent is (35-78):1.
[0065] Further controlling the raw materials to be prepared within the preferred range can improve the high temperature resistance and anti-termite performance of the composite material.
[0066] In a specific example, the weight ratio of the high temperature resistant thermosetting resin prepolymer to the anti-termite agent is 78:1.
[0067] In some embodiments, the high temperature resistant thermosetting resin is selected from one or more of phenolic epoxy resin, hydrogenated epoxy resin, phenolic resin, and epoxy vinyl resin.
[0068] In some embodiments, the above-mentioned anti-termite agent is selected from one or more of imidacloprid, bifenthrin, fipronil and avermectin.
[0069] In some embodiments, the defoaming agent is selected from one of polysiloxane, polyether and polyacrylate.
[0070] In some embodiments, the curing agent is selected from one or more of p-phenylenediamine, tetrahydrophthalic anhydride, phthalic anhydride, maleic anhydride, diethylenetriamine, ethylenediamine, silicone amine curing agent, polyamide, fatty amine, propylene carbonate and butyl titanate.
[0071] An embodiment of the present application further provides a method for preparing a composite material, comprising steps S10 to S20.
[0072] Step S10: providing raw materials according to the above composite material.
[0073] Step S20: mixing the raw materials and performing a curing reaction to obtain the composite material.
[0074] Specifically, the step S20 of mixing the raw materials for curing reaction includes steps S21 to S23.
[0075] Step S21: performing a first mixing of the high temperature resistant thermosetting prepolymer and the anti-termite agent to obtain a first mixture.
[0076] Specifically, before the first mixing step is performed in step S21, the anti-termite agent is crushed.
[0077] It can be understood that the particle size of the composite material finally prepared by crushing the anti-termite agent is several to dozens of times the particle size of the anti-termite agent, which makes the anti-termite agent evenly dispersed in the heat-resistant resin prepolymer, thereby obtaining a composite high heat-resistant anti-termite powder.
[0078] Step S22: adding the defoaming agent to the first mixture, performing a second mixing to obtain a second mixture.
[0079] Step S23: adding the curing agent to the second mixture to perform a third mixing, and performing a curing reaction to obtain the composite material.
[0080] In some embodiments, the first mixing conditions include: a temperature of 20° C. to 140° C., a rotation speed of 300 r / min to 3000 r / min, and a stirring time of 10 min to 50 min.
[0081] The temperature "20℃~140℃" can be a numerical range of 20℃~140℃, which is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. For example, it includes but is not limited to 20℃, 25℃, 30℃, 35℃, 40℃, 45℃, 50℃, 55℃, 60℃, 65℃, 70℃, 75℃, 80℃, 85℃, 90℃, 95℃, 100℃, 105℃, 110℃, 115℃, 120℃, 125℃, 130℃, 135℃ or 140℃; or a range consisting of any two of these values, as an example, including: 30℃~120℃.
[0082] In some embodiments, the curing reaction conditions include: a curing temperature of 30° C. to 180° C. and a curing time of 2 h to 15 h.
[0083] The curing temperature "30°C~180°C" can be a numerical range of 30°C~180°C, which is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. For example, it includes but is not limited to 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C or 180°C; or a range consisting of any two of these values, as an example, including: 30°C~150°C.
[0084] The curing time "2h~15h" can be a numerical range of 2h~15h, which is considered continuous and includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. For example, it includes but is not limited to 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h or 15h; or a range consisting of any two of these values, as an example, including: 3h~15h.
[0085] In some embodiments, the composite material has a particle size of 10 μm to 300 μm.
[0086] One embodiment of the present application also provides an application of the above composite material in preparing cables.
[0087] An embodiment of the present application further provides a cable, comprising a conductor and a protective layer sleeved on the surface of the conductor, wherein the protective layer comprises the composite material.
[0088] The composite material can be applied to high-temperature processing environments, effectively improve the problem of volatilization of anti-termite agents during processing, and reduce the harm of volatilization of anti-termite agents to human body and environment.
[0089] In order to make the purpose, technical solutions and advantages of the present invention more concise and clear, the present invention is described with the following specific embodiments, but the present invention is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present invention, which can be used to describe the present invention and cannot be understood as limiting the scope of the present invention. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0090] In order to better illustrate the present invention, the content of the present invention is further described below in conjunction with embodiments.
[0091] Example 1
[0092] S1. First, pour imidacloprid technical drug (purchased from Hubei Huiheyuan Chemical Co., Ltd., with a purity of 98%) into a grinder for mechanical crushing to obtain imidacloprid technical drug powder. The mechanical crushing time of imidacloprid is 30 minutes, and the crushing speed is controlled at 30000r / min.
[0093] S2. Weigh 78% phenolic epoxy resin (purchased from Guangzhou Tongxin Chemical Co., Ltd., model phenolic epoxy resin F51) and 1% imidacloprid technical powder and pour them into a mixing mixer. Control the temperature in the mixer at 60°C and the speed at 500 r / min for 15 min to obtain imidacloprid-phenolic epoxy mixture A.
[0094] S3. Add 1% low molecular weight polysiloxane (purchased from Guangzhou Haoliangda International Trade Co., Ltd., model number: Deqian 6500) to the imidacloprid-phenolic epoxy mixture A obtained in S2, and mix and stir at a speed of 600 r / min for 10 min to obtain the imidacloprid-phenolic epoxy mixture B.
[0095] S4. Then weigh 20% of p-phenylenediamine curing agent (purchased from Guangzhou Tongxin Chemical Co., Ltd., model number: epoxy resin curing agent T31) and add it to the imidacloprid-phenolic epoxy mixture B obtained in S3 to mix them evenly. The curing temperature is controlled at 30° C. and the curing time is controlled at 8 hours to obtain a cured imidacloprid-phenolic epoxy mixture C.
[0096] S5. Pour the imidacloprid-phenolic epoxy mixture C cured in S4 into a mechanical grinder and grind it at a speed of 28000 r / min for 25 min to obtain a composite material.
[0097] Example 2
[0098] S1. First, pour imidacloprid technical drug (purchased from Hubei Huiheyuan Chemical Co., Ltd., with a purity of 98%) into a grinder for mechanical crushing to obtain imidacloprid technical drug powder. The mechanical crushing time of imidacloprid is 30 minutes, and the crushing speed is controlled at 30000r / min.
[0099] S2. Weigh 70% phenolic epoxy resin (purchased from Guangzhou Tongxin Chemical Co., Ltd., model phenolic epoxy resin F51) and 1% imidacloprid technical powder and pour them into a mixing mixer. Control the temperature in the mixer at 60°C and the speed at 500 r / min for 15 min to obtain imidacloprid-phenolic epoxy mixture A.
[0100] S3. Add 1% low molecular weight polysiloxane (purchased from Guangzhou Haoliangda International Trade Co., Ltd., model number: Deqian 6500) to the imidacloprid-phenolic epoxy mixture A obtained in S2, and mix and stir at a speed of 600 r / min for 10 min to obtain the imidacloprid-phenolic epoxy mixture B.
[0101] S4. Then weigh 28% of p-phenylenediamine curing agent (purchased from Guangzhou Tongxin Chemical Co., Ltd., model number: epoxy resin curing agent T31) and add it to the imidacloprid-phenolic epoxy mixture B obtained in S3 to mix them evenly. The curing temperature is controlled at 30° C. and the curing time is controlled at 8 hours to obtain a cured imidacloprid-phenolic epoxy mixture C.
[0102] S5. Pour the imidacloprid-phenolic epoxy mixture C cured in S4 into a mechanical grinder and grind it at a speed of 28000 r / min for 25 min to obtain a composite material.
[0103] Example 3
[0104] S1. First, pour imidacloprid into a pulverizer and fully pulverize it to obtain imidacloprid technical powder. The mechanical pulverization time of imidacloprid is 30 minutes, and the pulverization speed is controlled at 30000r / min.
[0105] S2. Weigh 69.5% modified epoxy resin (purchased from Guangzhou Xingyao Chemical Co., Ltd., model 014U) and 1% imidacloprid technical powder and pour them into a mixing mixer. Control the temperature in the mixer at 130°C and the speed at 400 r / min for 15 min to obtain imidacloprid-modified epoxy mixture A. The drying temperature is 80 and the drying time is 30 h.
[0106] S3. Add 0.5% low molecular weight polysiloxane to the imidacloprid-modified epoxy mixture A obtained in S2, and mix and stir at a speed of 6000 r / min for 10 min to obtain the imidacloprid-modified epoxy mixture B.
[0107] S4. Then weigh 29% tetrahydrophthalic anhydride curing agent (purchased from Guangzhou Ruishi Biotechnology Co., Ltd., with a purity of 99%) and add it to the imidacloprid-modified epoxy mixture B obtained in S3 to mix them evenly. The curing temperature is controlled at 150° C. and the curing time is controlled at 15 h to obtain a cured imidacloprid-modified epoxy mixture C.
[0108] S5. Pour the imidacloprid-modified epoxy mixture C cured in S4 into a grinder and grind it at a speed of 30000 r / min for 20 min to obtain a composite material.
[0109] Example 4
[0110] S1. First, pour the imidacloprid technical drug (purchased from Hubei Huiheyuan Chemical Co., Ltd., model: technical drug purity 98%) into a grinder for mechanical crushing to obtain imidacloprid technical drug powder. The mechanical crushing time of imidacloprid is 30 minutes, and the crushing speed is controlled at 30000r / min.
[0111] S2. Weigh 70% phenolic epoxy resin (purchased from Guangzhou Tongxin Chemical Co., Ltd., model phenolic epoxy resin F51) and 2% imidacloprid technical powder and pour them into a mixing mixer. Control the temperature in the mixer at 60°C and the speed at 500 r / min for 15 min to obtain imidacloprid-phenolic epoxy mixture A.
[0112] S3. Add 2% low molecular weight polysiloxane (purchased from Guangzhou Haoliangda International Trade Co., Ltd., model number: Deqian 6500) to the imidacloprid-phenolic epoxy mixture A obtained in S2, and mix and stir at a speed of 600 r / min for 10 min to obtain the imidacloprid-phenolic epoxy mixture B.
[0113] S4. Then weigh 26% of p-phenylenediamine curing agent (purchased from Guangzhou Tongxin Chemical Co., Ltd., model number epoxy resin curing agent T31) and add it to the imidacloprid-phenolic epoxy mixture B obtained in S3 to mix them evenly. The curing temperature is controlled at 30° C. and the curing time is controlled at 8 hours to obtain a cured imidacloprid-phenolic epoxy mixture C.
[0114] S5. Pour the imidacloprid-phenolic epoxy mixture C cured in S4 into a mechanical grinder and grind it at a speed of 28000 r / min for 25 min to obtain a composite material.
[0115] Example 5
[0116] S1. First, pour imidacloprid into a pulverizer and fully pulverize it to obtain imidacloprid technical powder. The mechanical pulverization time of imidacloprid is 40 minutes, and the pulverization speed is controlled at 32000r / min.
[0117] S2. Weigh 68% phenolic epoxy resin and 15% imidacloprid original drug powder and pour them into a mixing mixer. Control the temperature in the mixer at 60° C. and the speed at 600 r / min for 15 min to obtain imidacloprid-phenolic epoxy mixture A.
[0118] S3. Add 1% low molecular weight polysiloxane to the imidacloprid-phenolic epoxy mixture A obtained in S2, and mix and stir at a speed of 600 r / min for 10 min to obtain the imidacloprid-phenolic epoxy mixture B.
[0119] S4, then weigh 16% of p-phenylenediamine curing agent and add it to the imidacloprid-phenolic epoxy mixture B obtained in S3 to mix them evenly, control the curing temperature at 30° C. and the curing time at 8 h to obtain the imidacloprid-phenolic epoxy mixture C.
[0120] S5. Pour the imidacloprid-phenolic epoxy mixture C of S4 into a grinder and grind it at a speed of 28000 r / min for 20 min to obtain a composite material.
[0121] Example 6
[0122] S1. First, pour imidacloprid into a pulverizer and fully pulverize it to obtain imidacloprid technical powder. The mechanical pulverization time of imidacloprid is 30 minutes, and the pulverization speed is controlled at 32000r / min.
[0123] S2. Weigh 56.5% of modified epoxy resin and 20% of imidacloprid original powder and pour them into a mixing mixer. Control the temperature in the mixer at 140°C and the speed at 500 r / min for 15 min to obtain imidacloprid-modified epoxy mixture A.
[0124] S3. Add 0.5% low molecular weight polysiloxane to the imidacloprid-modified epoxy mixture obtained in S2, and mix and stir at a speed of 600 r / min for 10 min to obtain the imidacloprid-modified epoxy mixture B.
[0125] S4. Then weigh 23% tetrahydrophthalic anhydride curing agent and add it to the imidacloprid-modified epoxy mixture B obtained in S3 to mix them evenly. The curing temperature is controlled at 150° C. and the curing time is controlled at 15 h to obtain a cured imidacloprid-modified epoxy mixture C.
[0126] S5. Pour the imidacloprid-modified epoxy mixture C cured in S4 into a grinder and grind it at a speed of 30,000 r / min for 20 minutes to obtain a composite material.
[0127] Example 7
[0128] S1. First, pour imidacloprid into a pulverizer and fully pulverize it to obtain imidacloprid technical powder. The mechanical pulverization time of imidacloprid is 30 minutes, and the pulverization speed is controlled at 32000r / min.
[0129] S2. Weigh 75.5% of modified epoxy resin and 20% of imidacloprid original powder and pour them into a mixing mixer. Control the temperature in the mixer at 30°C and the speed at 500 r / min for 25 min to obtain imidacloprid-phenolic resin mixture A.
[0130] S3. Add 0.5% low molecular weight polysiloxane to the imidacloprid-phenolic resin mixture obtained in S2, and mix and stir at a speed of 600 r / min for 10 min to obtain an imidacloprid-phenolic resin mixture B.
[0131] S4. Then weigh 4% propylene carbonate curing agent (purchased from Guangzhou Xingchuangzhi New Materials Co., Ltd., with a purity of 99%) and add it to the imidacloprid-phenolic resin mixture B obtained in S3 to mix them evenly. The curing temperature is controlled at 180° C. and the curing time is controlled at 5 h to obtain a cured imidacloprid-phenolic resin mixture C.
[0132] S5. Pour the imidacloprid-phenolic resin mixture C cured in S4 into a grinder and grind it at a speed of 30000 r / min for 20 min to obtain a composite material.
[0133] Embodiment 8-9
[0134] The preparation methods of the composite materials in Examples 8-9 are basically the same as those in Example 1, except that the preparation process parameters of the composite materials are different, as shown in Table 1.
[0135] The remaining steps and conditions are the same as those in Example 1.
[0136] Comparative Examples 1 to 3
[0137] The preparation methods of the composite materials in Comparative Examples 1 to 3 are basically the same as those in Example 1, except that the amounts of the components of the raw materials used in preparing the composite materials are different, as shown in Table 1.
[0138] The remaining steps and conditions are the same as those in Example 1.
[0139] The following is a performance test.
[0140] The composite materials products prepared in the above-mentioned specific examples 1 to 9 and comparative examples 1 to 3 were subjected to the following tests:
[0141] 1. Microscopic morphology: In order to characterize the particle size and surface morphology of the synthesized high heat-resistant anti-ant powder, the present invention adopts a field emission scanning electron microscope (SEM, Inspect-F, FEI, Finland) at an accelerating voltage of 5 kV to characterize the imidacloprid original powder and the composite materials prepared in Examples 1 to 9 and Comparative Examples 1 to 3.
[0142] 2. Heat resistance: In order to highlight the excellent thermal stability of the final synthesized anti-ant powder, the thermogravimetric curves of the anti-ant agent - imidacloprid, phenolic epoxy resin, and the final synthesized composite material were measured.
[0143] 3. Qualitative characterization: According to literature reports, imidacloprid has specific absorption of 270nm ultraviolet light, and a specific absorption peak will appear in the ultraviolet spectrum; in order to determine that the prepared composite material contains imidacloprid, the ultraviolet absorption spectra of the prepared composite material and phenolic epoxy resin were measured using dichloromethane as solvent.
[0144] 4. Content determination: Results In order to determine the content of imidacloprid in the highly heat-resistant anti-ant powder, dichloromethane was used as the solvent to measure the ultraviolet absorption intensity of imidacloprid at different concentrations at 270nm; according to the Lumberton law A=kbc, where A is absorbance, k is the absorption coefficient, b is the liquid layer thickness, and c is the sample concentration, that is, the sample concentration is proportional to the absorbance, and a standard curve of imidacloprid concentration and ultraviolet absorption intensity was drawn. Then the ultraviolet absorbance of a certain concentration of the composite material at 270nm was read out, and the concentration of imidacloprid in the solution can be obtained according to the standard curve. The mass fraction of imidacloprid can be obtained by the ratio of the concentration of imidacloprid in the solution to the concentration of imidacloprid-phenolic epoxy in the solution, and the content of imidacloprid in the composite material can be obtained by calculation.
[0145] The test results are shown in Table 1 below:
[0146] Table 1
[0147]
[0148] Figure 1 This is the SEM result of the composite material prepared in Example 5. Figure 2 This is the SEM result of imidacloprid original powder. Figure 1 It can be seen that the length of the final synthesized composite material is 30-100 μm, and the synthesized composite material is several to dozens of times larger than the imidacloprid original drug powder. The thermogravimetric curve results of the composite material, imidacloprid original drug and phenolic epoxy resin prepared in Example 5 are shown in Figure 3The initial decomposition temperature of imidacloprid is 230℃ (288), the initial decomposition temperature of phenolic epoxy resin is 310℃ (359), and the initial decomposition temperature of the synthesized composite material is 271 (337)℃. This is because the outer layer of heat-resistant thermosetting resin blocks part of the heat transfer, which increases the initial decomposition temperature of imidacloprid inside. The results show that the prepared composite material has excellent thermal stability. Figure 4 The UV absorption spectrum of the composite material in Example 5 shows that the phenolic epoxy resin has no absorption peak at 270 nm, while the composite material (imidacloprid-phenolic epoxy) has an absorption peak at 270 nm, confirming that the composite material contains imidacloprid. Figure 5 As shown, it can be seen that as the concentration of imidacloprid increases, the ultraviolet absorbance of the solution at 270nm increases; according to the Ludwig-Beer law A=kbc, where A is absorbance, k is the absorption coefficient, b is the liquid layer thickness, and c is the sample concentration, that is, the sample concentration is proportional to the absorbance, and a standard curve of imidacloprid concentration and ultraviolet absorption intensity is drawn, as shown in Figure 6 Then read Figure 4 The ultraviolet absorbance of a certain concentration of the composite material at 270 nm can be used to obtain the concentration of imidacloprid in the solution according to the standard curve. The mass fraction of imidacloprid can be obtained by the ratio of the concentration of imidacloprid in the solution to the concentration of the composite material in the solution. It can be calculated that the content of imidacloprid in the composite material prepared in Example 5 is 10.2%.
[0149] It can be seen that the composite material prepared by adopting the technical solution of the present application has both good high temperature resistance and anti-ant performance.
[0150] The technical features of the above-described embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above-described embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. The above-described embodiments only express several implementation methods of the present invention, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present invention, several variations and improvements can be made, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. A composite material, characterized in that: The raw materials for preparing the composite material include the following components by mass percentage: High temperature resistant thermosetting resin prepolymer 50%~80%; Anti-termite agent 1%~30%; Curing agent 14%~40%; Defoaming agent 0.5%~2%; Wherein, the weight ratio of the high temperature resistant thermosetting resin prepolymer to the anti-termite agent is (2~79):
1.
2. The composite material according to claim 1, characterized in that The raw materials for preparing the composite material include the following components by mass percentage: High temperature resistant thermosetting resin prepolymer 60%~78%; Anti-termite agent 1%~20%; Curing agent 19%~38%; Defoaming agent 0.5%~2%.
3. The composite material according to claim 1, characterized in that The weight ratio of the high temperature resistant thermosetting resin prepolymer to the anti-termite agent is (35-78):
1.
4. The composite material according to claim 1, characterized in that The high temperature resistant thermosetting resin is selected from one or more of phenolic epoxy resin, hydrogenated epoxy resin, phenolic resin and epoxy vinyl resin.
5. The composite material according to any one of claims 1 to 4, characterized in that The anti-ant agent is selected from one or more of imidacloprid, bifenthrin, fipronil and avermectin; and / or, the defoamer is selected from one of polysiloxane, polyether and polyacrylate; And / or, the curing agent is selected from one or more of p-phenylenediamine, tetrahydrophthalic anhydride, phthalic anhydride, maleic anhydride, diethylenetriamine, ethylenediamine, organic silicon amine curing agent, polyamide, fatty amine, propylene carbonate and butyl titanate.
6. A method for preparing a composite material, characterized in that: The steps include: Providing a raw material according to the composite material according to any one of claims 1 to 5; and The raw materials are mixed and cured to obtain the composite material.
7. The method for preparing a composite material according to claim 6, characterized in that: Mixing the raw materials for curing reaction includes the following steps: The high temperature resistant thermosetting prepolymer is first mixed with the anti-termite agent to obtain a first mixture; adding the defoaming agent to the first mixture, performing a second mixing to obtain a second mixture; The curing agent is added to the second mixture, and a third mixing is performed to obtain the composite material after a curing reaction.
8. The method for preparing a composite material according to claim 7, characterized in that: The first mixing conditions include: temperature of 20°C to 140°C, rotation speed of 300r / min to 3000r / min, and stirring time of 10min to 50min; And / or, the conditions of the curing reaction include: a curing temperature of 30° C. to 180° C. and a curing time of 2 h to 15 h.
9. Use of the composite material according to any one of claims 1 to 5 in the preparation of cables.
10. A cable, characterized in that: It comprises a conductor and a protective layer sleeved on the surface of the conductor, wherein the protective layer comprises the composite material according to any one of claims 1 to 5.
Citation Information
Cited By
Anti-termite powder as well as preparation method and application thereof