Flow line master batch for injection molding as well as preparation method and application of flow line master batch

By using injection molded flow grain masterbatch composed of PCT resin and toner pigment in PC materials, combined with appropriate temperature and proportion, the problem of not being able to achieve flow grain effect in PC materials in the prior art is solved, and clear and delicate flow is achieved Reduced texture effect and cost.

CN119019825APending Publication Date: 2024-11-26WANHUA CHEM GRP CO LTD +1

Patent Information

Application Number
CN202411299217.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing flow pattern masterbatch cannot achieve injection molding flow effect in PC materials, and the traditional IML process is costly and lacks differentiation.

Method used

The injection molded flow pattern masterbatch consisting of PCT resin, toner pigment and functional additives is used to form a differentiated flow pattern effect by mixing it with PC and modified PC base material and injection molding at an appropriate temperature.

Benefits of technology

It achieves a clear and delicate flow pattern effect in PC materials, reduces costs, and provides a differentiated random flow pattern line effect, replacing the traditional IML process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005047103260000061
    Figure BDA0005047103260000061
  • Figure BDA0005047103260000091
    Figure BDA0005047103260000091
  • Figure BDA0005047103260000101
    Figure BDA0005047103260000101
Patent Text Reader

Abstract

The invention discloses a flow line master batch for injection molding as well as a preparation method and application thereof. The flow line master batch is prepared from the following components in parts by mass: 98.5 to 99.5 parts of PCT resin; 0.3 to 1 part of toner pigment; and 0.2 to 0.5 part of a functional auxiliary agent. The flow line master batch can be uniformly mixed with PC and modified PC base resin according to a ratio, and the flow line master batch is uniformly mixed with PC and modified PC base resin at the same processing temperature and subjected to injection molding by utilizing the fluidity difference and color difference between the PCT flow line master batch and PC and modified PC materials at the same processing temperature, so that a color-differentiated flow line effect can be formed. The flow line effect brought by the invention can be used for replacing the flow line effect realized by the traditional IML injection molding process, and the differentiated random flow line effect can also be formed while the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a flow pattern masterbatch for injection molding and a preparation method thereof, and belongs to the field of masterbatch materials with special aesthetic effects. Background Art

[0002] PC (polycarbonate) and modified PC materials have excellent mechanical and appearance performance, and are widely used as exterior decoration parts in the fields of electronics and automobiles. The aesthetic appearance effect with marble flow patterns has been applied to more and more products. At present, it is achieved by attaching a layer of marble flow pattern film on the surface of the plastic substrate. The yield rate of this in-mold label injection molding process (IML) is lower than that of ordinary injection molding process, and the cost will be further increased. Its texture effect is expressed by the texture obtained by printing on the film, which lacks differentiation. The marble flow pattern effect produced by injection molding process has been realized in PP, ABS and other materials, but because the injection molding processing temperature of PC material is higher than that of PP, ABS and other materials, the flow pattern masterbatch used in existing materials cannot be applied to the production of flow pattern effects of PC and other materials. Summary of the invention

[0003] Based on the above technical background, the present invention proposes a flow pattern masterbatch for injection molding and a preparation method thereof, and a flow pattern effect product can be obtained by directly injection molding after mixing the flow pattern masterbatch and a base plastic material.

[0004] The present invention provides an injection molding flow pattern masterbatch for injection molding, comprising the following components in parts by mass:

[0005] (PCT resin) Poly(1,4-cyclohexanedimethanol terephthalate) resin: 98.5-99.5 ;

[0006] Toner Pigment: 0.3-1

[0007] Functional additives 0.2-0.5 .

[0008] In the present invention, the intrinsic viscosity of PCT resin is in the range of 0.75-0.90 dL / g. PCT melting point range is 280-300 ℃.

[0009] More preferably, the molar ratio of cis-CHDM to trans-CHDM in CHDM (1,4-cyclohexanedimethanol) used as the raw material for preparing PCT is (30-50):(50-70), Its melting point range can better match the processing temperature of PC and modified PC, thereby obtaining better flow effect.

[0010] In the present invention, the color powder pigment in the rhytometric masterbatch includes one or more combinations of dyes, color pigments and effect pigments. Preferably, the dyes include one or more combinations of anthraquinones, coumarins, ketones, condensed rings and heterocyclic dyes. The color pigments include one or more combinations of phthalocyanine, iron red, titanium chrome yellow, carbon black, titanium dioxide, ultramarine, ultramarine violet, cobalt blue and cobalt green. The effect pigments include one or more combinations of metal powders and pearlescent powders.

[0011] In the present invention, the functional additives in the rhytoid masterbatch include one or more combinations of lubricants and antioxidants. The lubricant is pentaerythritol stearate (PETS). The antioxidant is a composite antioxidant, such as B900, B225, etc.

[0012] The preparation method of the rhytoid masterbatch of the present invention comprises the following steps:

[0013] a. Drying the PCT resin so that its moisture content is less than 0.1wt%;

[0014] b. Mix all materials at high speed according to their mass fractions;

[0015] c. The mixed materials are extruded and granulated to obtain the finished flow masterbatch, and the preferred extrusion processing temperature is 280-320°C.

[0016] The application of the rhytide masterbatch of the present invention to produce rhytide effect in the injection molding of substrate plastic materials is specifically as follows:

[0017] Firstly, the base plastic material and the flow pattern master batch are mixed, and then the base plastic material and the flow pattern master batch are mixed and then injection molded to obtain a flow pattern effect product, and the injection molding temperature is preferably 290-310°C.

[0018] Preferably, the substrate plastic material is a plastic material with a processing temperature range of 290-310° C., specifically PC and modified PC materials.

[0019] Among them, the mass fractions of base plastic material and rhytographic masterbatch are as follows:

[0020] Base Plastic Material: 94-99 copies ;

[0021] Rhythm Masterbatch: 1-6 servings .

[0022] The flow masterbatch can be evenly mixed with PC and modified PC base resin according to a proportion, and the PCT flow masterbatch can be evenly mixed with the PC and modified PC base resin at the same processing temperature. The flow effect can be formed by injection molding after uniform mixing, and the flow effect brought by the present invention can be used to replace the flow effect achieved by the traditional IML injection molding process, while achieving cost reduction, and can also form a differentiated random flow line effect.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. It solves the problem that the existing rhytm masterbatch on the market cannot achieve injection molding rhytm effect on PC materials.

[0025] 2. The shape of the flow effect can be further adjusted by adjusting the ratio of the flow masterbatch and the base plastic material, as well as adjusting the injection molding temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a flow pattern effect diagram of the injection molded part of Example 1.

[0027] Figure 2 This is a flow pattern effect diagram of the injection molded part of Example 2.

[0028] Figure 3 This is a flow pattern effect diagram of the injection molded part of Example 3.

[0029] Figure 4 This is a flow pattern effect diagram of the injection molded part of Example 4.

[0030] Figure 5 This is a flow pattern effect diagram of the injection molded part of Example 5.

[0031] Figure 6 This is a flow pattern effect diagram of the injection molded part of Example 6.

[0032] Figure 7 This is a flow pattern effect diagram of the injection molded part of Example 7.

[0033] Figure 8 This is a flow pattern effect diagram of the injection molded part of Example 8.

[0034] Fig. 9 This is a flow pattern effect diagram of the injection molded part of Comparative Example 1.

[0035] Fig.10 This is a flow pattern effect diagram of the injection molded part of Comparative Example 2. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0037] The PCT resin in the present invention is homemade, and the specific homemade steps are:

[0038] S1. Melting the cis- and trans-CHDM mixture at 80°C to a solution;

[0039] S2. PTA (terephthalic acid) and CHDM mixture were added to the flask at a molar ratio of 38:62;

[0040] S3. The flask was filled with nitrogen to replace the air, and heated and stirred until stable;

[0041] S4. When slowly heated to 260°C, the reaction is carried out and water is removed by fractional distillation;

[0042] S5. When no water is distilled out of the reaction, the nitrogen is cut off to obtain an intermediate monomer;

[0043] S6. The obtained intermediate monomer was put into a vacuum reactor, the pressure was reduced to 60Pa, and the temperature was raised to 290°C and maintained for 30 minutes; S7. The temperature was further heated to 320°C and the pressure was reduced to 10Pa to continue the reaction;

[0044] S8. When the torque of the stirrer is stable, slowly increase the pressure to normal pressure and slowly reduce the temperature to normal temperature to obtain PCT resin.

[0045] Preparation Example 1:

[0046] The molar ratio of cis-CHDM to trans-CHDM in the raw material CHDM mixture used in the preparation example PCT resin 1 of the present invention is 30:70;

[0047] The intrinsic viscosity of the obtained PCT resin 1 was 0.78 dL / g, and the melting point was 293°C.

[0048] Preparation Example 2:

[0049] The molar ratio of cis-CHDM to trans-CHDM in the raw material CHDM mixture used in the preparation example PCT resin 2 of the present invention is 40:60;

[0050] The intrinsic viscosity of the obtained PCT resin 2 was 0.85 dL / g, and the melting point was 286°C.

[0051] Preparation Example 3:

[0052] The molar ratio of cis-CHDM to trans-CHDM in the raw material CHDM mixture used in the preparation example PCT resin 3 of the present invention is 50:50;

[0053] The intrinsic viscosity of the obtained PCT resin 3 was 0.89 dL / g, and the melting point was 283°C.

[0054] Preparation Example 4:

[0055] The molar ratio of cis-CHDM to trans-CHDM in the raw material CHDM mixture used in the preparation example PCT resin 4 of the present invention is 70:30;

[0056] The intrinsic viscosity of the obtained PCT resin 4 was 0.92 dL / g, and the melting point was 266°C.

[0057] Example 1

[0058] The raw materials and mass fractions used in the PCT rhytographic masterbatch 1 of the embodiment of the present invention are shown in the following table.

[0059] Components Brand and supplier Mass fraction PCT Resin 1 self made 99.25 Toner Pigment 1-Toner Solvent Blue 97, LANXESS 0.3 Functional additive 1-lubricant PETS,LONZA 0.3 Functional additive 2-Antioxidant B900,BASF 0.15

[0060] PCT Flow Masterbatch 1 Raw Materials List

[0061] The above PCT resin 1 is dried at 90°C for 2 hours; the PCT resin, color powder pigment and functional additives are further mixed by a high-speed mixer at a mixing speed of 1000rpm; and the PCT flow masterbatch 1 is obtained after granulation by a twin-screw extruder, and its processing temperature is 300°C.

[0062] PCT flow pattern masterbatch 1 and PC resin 1 are further mixed. The raw materials used and the mass fractions of the mixture are shown in the following table.

[0063] Components Brand and supplier Mass fraction PCT rhytographic masterbatch 1 \ 3 PC resin 1 A1225, Wanhua Chemical 97

[0064] PCT flow masterbatch 1 and PC resin 1 raw material table

[0065] The square color plate is injection molded by the mixture of the above PCT flow pattern masterbatch 1 and PC resin 1. The molding temperature is 300℃. The flow pattern effect of the molded part is as follows: Figure 1 It can be seen that the PCT flow masterbatch 1 and PC resin 1 injection molded parts at 300°C have obvious flow effect, and the flow lines are clear, but not delicate and continuous enough.

[0066] Example 2

[0067] The raw materials and mass fractions used in the PCT rhytographic masterbatch 2 of the embodiment of the present invention are shown in the following table.

[0068] Components Brand and supplier Mass fraction PCT Resin 2 self made 99.25 Toner Pigment 1-Toner Solvent Blue 97, LANXESS 0.3 Functional additive 1-lubricant PETS,LONZA 0.3 Functional additive 2-Antioxidant B900,BASF 0.15

[0069] PCT Flow Masterbatch 2 Raw Materials List

[0070] The above PCT resin 2 is dried at 90°C for 2 hours; the PCT resin, color powder pigment and functional additives are further mixed by a high-speed mixer at a mixing speed of 1000rpm; and then granulated by a twin-screw extruder to obtain PCT flow masterbatch 2, and its processing temperature is 300°C.

[0071] PCT flow masterbatch 2 and PC resin 1 are further mixed. The raw materials used and the mass fractions of the mixture are shown in the following table.

[0072] Components Brand and supplier Mass fraction PCT rhytographic masterbatch 2 \ 3 PC resin 1 A1225, Wanhua Chemical 97

[0073] PCT rhytographic masterbatch 2 and PC resin 1 raw material table

[0074] The square color plate is injection molded by the mixture of the above PCT flow pattern masterbatch 2 and PC resin 1. The molding temperature is 300℃. The flow pattern effect of the molded part is as follows: Figure 2 It can be seen that the PCT flow masterbatch 2 and PC resin 1 injection molded parts at 300°C have obvious flow effect, and the flow lines are clear and delicate.

[0075] Example 3

[0076] The raw materials and mass fractions used in the PCT rhytographic masterbatch 3 of the embodiment of the present invention are shown in the following table.

[0077] Components Brand and supplier Mass fraction PCT Resin 3 \ 99.25 Toner Pigment 1-Toner Solvent Blue 97, LANXESS 0.3 Functional additive 1-lubricant PETS,LONZA 0.3 Functional additive 2-Antioxidant B900,BASF 0.15

[0078] PCT Flow Masterbatch 3 Raw Materials List

[0079] The above PCT resin 3 is dried at 90°C for 2 hours; the PCT resin, color powder pigment and functional additives are further mixed by a high-speed mixer at a mixing speed of 1000rpm; and then granulated by a twin-screw extruder to obtain PCT flow masterbatch 3, whose processing temperature is 300°C.

[0080] PCT flow masterbatch 3 and PC resin 1 are further mixed. The raw materials used and the mass fractions of the mixture are shown in the following table.

[0081]

[0082]

[0083] PCT rhytographic masterbatch 3 and PC resin 1 raw material table

[0084] The square color plate is injection molded by the mixture of the above PCT flow pattern masterbatch 3 and PC resin 1. The molding temperature is 300℃. The flow pattern effect of the molded part is as follows: Figure 3It can be seen that the injection molded parts of PCT flow pattern masterbatch 3 and PC resin 1 at 300℃ have obvious flow pattern effects, and the flow pattern lines are clear and delicate.

[0085] Example 4

[0086] The raw materials and mass fractions used in the PCT rhytographic masterbatch 4 of the embodiment of the present invention are shown in the following table.

[0087] Components Brand and supplier Mass fraction PCT Resin 4 self made 99.25 Toner Pigment 1-Toner Solvent Blue 97, LANXESS 0.3 Functional additive 1-lubricant PETS,LONZA 0.3 Functional additive 2-Antioxidant B900,BASF 0.15

[0088] PCT rhytometric masterbatch 4 raw material table

[0089] The above PCT resin 4 is dried at 90°C for 2 hours; the PCT resin, color powder pigment and functional additives are further mixed by a high-speed mixer at a mixing speed of 1000rpm; and then granulated by a twin-screw extruder to obtain PCT flow masterbatch 4, whose processing temperature is 300°C.

[0090] PCT flow masterbatch 4 and PC resin 1 are further mixed. The raw materials used and the mass fractions of the mixture are shown in the following table.

[0091] Components Brand and supplier Mass fraction PCT rhytographic masterbatch 4 \ 3 PC resin 1 A1225, Wanhua Chemical 97

[0092] PCT rhytographic masterbatch 4 and PC resin 1 raw material table

[0093] The square color plate is injection molded by the mixture of the above PCT flow pattern masterbatch 4 and PC resin 1. The molding temperature is 300℃. The flow pattern effect of the molded part is as follows: Figure 4 It can be seen that the injection molded parts of PCT flow pattern masterbatch 4 and PC resin 1 at 300°C have a certain flow pattern effect locally, and the lines are not clear enough.

[0094] Example 5

[0095] The raw materials and mass fractions used in the PCT rhytographic masterbatch 2 of the embodiment of the present invention are shown in the following table.

[0096] Components Brand and supplier Mass fraction PCT Resin 2 self made 99.25 Toner Pigment 1-Toner Solvent Blue 97, LANXESS 0.3 Functional additive 1-lubricant PETS,LONZA 0.3 Functional additive 2-Antioxidant B900,BASF 0.15

[0097] PCT Flow Masterbatch 2 Raw Materials List

[0098] The above PCT resin 1 is dried at 90°C for 2 hours; the PCT resin, color powder pigment and functional additives are further mixed by a high-speed mixer at a mixing speed of 1000rpm; and then granulated by a twin-screw extruder to obtain PCT flow masterbatch 2, whose processing temperature is 300°C.

[0099] PCT flow masterbatch 2 and PC resin 1 are further mixed. The raw materials used and the mass fractions of the mixture are shown in the following table.

[0100] Components Brand and supplier Mass fraction PCT rhytographic masterbatch 2 \ 3 PC resin 1 A1225, Wanhua Chemical 97

[0101] PCT rhytographic masterbatch 2 and PC resin 1 raw material table

[0102] The square color plate was injection molded by the mixture of PCT flow masterbatch 2 and PC resin 1, and the molding temperature was 290℃. The flow effect of the molded part is shown in Figure 5. It can be seen that the flow effect of the injection molded parts of PCT flow masterbatch 2 and PC resin 1 at 290℃ is obvious, and the flow lines are rough.

[0103] Example 6

[0104] The raw materials and mass fractions used in the PCT rhytographic masterbatch 2 of the embodiment of the present invention are shown in the following table.

[0105] Components Brand and supplier Mass fraction PCT Resin 2 self made 99.25 Toner Pigment 1-Toner Solvent Blue 97, LANXESS 0.3 Functional additive 1-lubricant PETS,LONZA 0.3 Functional additive 2-Antioxidant B900,BASF 0.15

[0106] PCT Flow Masterbatch 2 Raw Materials List

[0107] The above PCT resin 2 is dried at 90°C for 2 hours; the PCT resin, color powder pigment and functional additives are further mixed by a high-speed mixer at a mixing speed of 1000rpm; and then granulated by a twin-screw extruder to obtain PCT flow masterbatch 2, and its processing temperature is 300°C.

[0108] PCT flow masterbatch 2 and PC resin 1 are further mixed. The raw materials used and the mass fractions of the mixture are shown in the following table.

[0109] Components Brand and supplier Mass fraction PCT rhytographic masterbatch 2 \ 3 PC resin 1 A1225, Wanhua Chemical 97

[0110] PCT rhytographic masterbatch 2 and PC resin 1 raw material table

[0111] The square color plate was injection molded by the mixture of PCT flow masterbatch 2 and PC resin 1, and the molding temperature was 310℃. The flow effect of the molded part is shown in Figure 6. It can be seen that the injection molded parts of PCT flow masterbatch 2 and PC resin 1 at 310℃ have obvious flow effect, and the flow lines are clear and delicate.

[0112] Example 7

[0113] The raw materials and mass fractions used in the PCT rhytographic masterbatch 2 of the embodiment of the present invention are shown in the following table.

[0114] Components Brand and supplier Mass fraction PCT Resin 2 self made 99.25 Toner Pigment 1-Toner Solvent Blue 97, LANXESS 0.3 Functional additive 1-lubricant PETS,LONZA 0.3 Functional additive 2-Antioxidant B900,BASF 0.15

[0115] PCT Flow Masterbatch 2 Raw Materials List

[0116] The above PCT resin 2 is dried at 90°C for 2 hours; the PCT resin, color powder pigment and functional additives are further mixed by a high-speed mixer at a mixing speed of 1000rpm; and then granulated by a twin-screw extruder to obtain PCT flow masterbatch 2, and its processing temperature is 300°C.

[0117] PCT flow masterbatch 2 and PC resin 1 are further mixed. The raw materials used and the mass fractions of the mixture are shown in the following table.

[0118] Components Brand and supplier Mass fraction PCT rhytographic masterbatch 2 \ 6 PC resin 1 A1225, Wanhua Chemical 94

[0119] PCT rhytographic masterbatch 2 and PC resin 1 raw material table

[0120] The square color plate was injection molded by the mixture of the above PCT flow masterbatch 2 and PC resin 1, and the molding temperature was 300°C. The flow effect of the molded part obtained is shown in Figure 7. It can be seen that the injection molded parts of PCT flow masterbatch 2 and PC resin 1 at 300°C have obvious flow effect, and the flow lines are clear, the base color is darker than that of Example 2, and the color difference between the flow lines and the base color is smaller than that of Example 2.

[0121] Example 8

[0122] The raw materials and mass fractions used in the PCT rhytographic masterbatch 5 of the embodiment of the present invention are shown in the following table.

[0123]

[0124]

[0125] PCT Flow Masterbatch 5 Raw Materials List

[0126] The above PCT resin 2 is dried at 90°C for 2 hours; the PCT resin, color powder pigment and functional additives are further mixed by a high-speed mixer at a mixing speed of 1000rpm; and then granulated by a twin-screw extruder to obtain PCT flow masterbatch 5, whose processing temperature is 300°C.

[0127] PCT flow masterbatch 5 and PC resin 1 are further mixed. The raw materials used and the mass fractions of the mixture are shown in the following table.

[0128] Components Brand and supplier Mass fraction PCT rhytographic masterbatch 5 \ 3 PC resin 1 A1225, Wanhua Chemical 97

[0129] PCT flow masterbatch 5 and PC resin 1 raw material table

[0130] The square color plate was injection molded by the mixture of the above PCT flow masterbatch 5 and PC resin 1, and the molding temperature was 300°C. The flow effect of the molded part is shown in Figure 8. It can be seen that the injection molded parts of PCT flow masterbatch 5 and PC resin 1 at 300°C have obvious flow effect, and the flow lines are clear, the base color is darker than that of Example 2, and the color difference between the flow lines and the base color is smaller than that of Example 2.

[0131] Comparative Example 1

[0132] The comparative example of the present invention uses PET rhytometric masterbatch 1 and PC resin 1 available on the market for mixing. The raw materials used and the mass fractions of the mixture are shown in the following table.

[0133]

[0134] PET flow masterbatch 1 and PC resin 1 raw material list

[0135] The square color plate was injection molded by the mixture of the above PET flow masterbatch 1 and PC resin 1, and the molding temperature was 300℃. The flow effect of the molded part is shown in Figure 9. It can be seen that the flow performance of the injection molded part of the PET flow masterbatch 1 in the PC resin 1 is not good, the lines are basically dispersed, and there are no obvious clear lines.

[0136] Comparative Example 2

[0137] The comparative example of the present invention uses PET rhytometric masterbatch 1 and PC resin 1 available on the market for mixing. The raw materials used and the mass fractions of the mixture are shown in the following table.

[0138]

[0139] PET flow masterbatch 1 and PC resin 1 raw material list

[0140] The square color plate was injection molded by the mixture of the above PET flow masterbatch 1 and PC resin 1, and the molding temperature was 290℃. The flow effect of the molded part is shown in Figure 10. It can be seen that the flow performance of the injection molded part of the PET flow masterbatch 1 in the PC resin 1 is not good, the lines are basically dispersed, and there are no obvious clear lines.

[0141] The flow effect involved in the above embodiments and comparative examples can be evaluated based on the width and length of the flow lines, the contrast between the flow lines and the base color, and the flow distribution range. According to the above three dimensions, it is divided into 4 levels according to the visual effect, with level 1 being the worst flow effect and level 4 being the best flow effect.

[0142] The flow effect classification standards are as follows:

[0143] Level 1: There is basically no flow effect, and the flow and the base color are mixed into one color;

[0144] Level 2: There is a flow effect locally, with a significant color difference between the flow and the base color, but no obvious flow lines;

[0145] Level 3: There is a flow effect, the flow and the background color have obvious color difference, there are flow lines in some parts, and the lines are not fine and continuous;

[0146] Level 4: There is an obvious flow effect, the flow and the background color have a very obvious color difference, there are obvious flow lines in the whole picture, the lines are fine and continuous;

[0147] According to the above standards, the flow effect of the above 8 groups of examples and comparative examples of injection molded color plates was rated, and the results are shown in the following table.

[0148]

[0149] It can be concluded from the above embodiments and comparative examples that the PCT flow pattern masterbatch of the present invention is more suitable for presenting the flow pattern effect of PC as the substrate, and the PET flow pattern masterbatch available on the market is not suitable for presenting the flow pattern effect of PC resin.

[0150] Similarly, PCT rhyme masterbatch is also suitable for the rhyme effect presentation of the above modified PC as the base material.

[0151] The applicant declares that the present invention illustrates a thermoplastic polymer flow length measuring device of the present invention through the above-mentioned embodiment, but the present invention is not limited to the above-mentioned structure and method, that is, it does not mean that the present invention must rely on the above-mentioned structure and method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A rhytide masterbatch for injection molding, characterized in that: Contains the following components by mass: PCT Poly(1,4-cyclohexanedimethanol terephthalate) resin: 98.5 Servings - 99.5; Toner Pigment: 0.3 share- 1 share Functional additives 0.2 share- 0.5 share.

2. The rhytide masterbatch according to claim 1, characterized in that: The intrinsic viscosity range of the PCT resin is 0.75- 0.90 dL / g; and / or, the melting point range of the PCT resin is 280-300 ℃.

3. The rhytide masterbatch according to claim 1 or 2, characterized in that: The molar ratio of cis-CHDM and trans-CHDM in CHDM1,4-cyclohexanedimethanol, a raw material for preparing the PCT resin, is (30-50):(50-70) .

4. The rhytide masterbatch according to any one of claims 1 to 3, characterized in that: The toner pigments include one or more combinations of dyes, color pigments and effect pigments.

5. The rhytide masterbatch according to claim 4, characterized in that: The dyes include one or more combinations of anthraquinone, coumarin, ketone, condensed ring and heterocyclic dyes.

6. The rhytide masterbatch according to claim 4, characterized in that: The color pigments include one or more combinations of phthalocyanine, iron oxide red, titanium chrome yellow, carbon black, titanium dioxide, ultramarine, ultramarine violet, cobalt blue, and cobalt green, and / or the effect pigments include one or more combinations of metal powder and pearlescent powder.

7. The rhytide masterbatch according to any one of claims 1 to 6, characterized in that: The functional additives include one or more combinations of lubricants and antioxidants; preferably, the lubricant is pentaerythritol stearate PETS.

8. The method for preparing the rhytide masterbatch according to any one of claims 1 to 7, characterized in that: The following steps are involved: a. Dry the PCT resin so that its moisture content is less than 0.1wt%; b. Mix all materials at high speed according to their mass fractions; c. Extrude and granulate the mixed materials to obtain the finished product of flow masterbatch, and the preferred extrusion processing temperature is 280-320℃.

9. Use of the rhytide masterbatch according to any one of claims 1 to 7 to produce rhytide effect in injection molding of substrate plastic materials, characterized in that: The substrate plastic material is a plastic material with a processing temperature range of 290-310°C, preferably PC or modified PC material; and / or the injection molding processing temperature is 290-310°C.

10. The use according to claim 9, characterized in that: The mass fractions of base plastic material and rhytographic masterbatch are as follows: Base Plastic Material: 94-99 copies ; Rhythm Masterbatch: 1-6 servings .

Citation Information

Patent Citations

  • Master batch with laminated wood-grain-like effect, preparation method and application

    CN118165472A

  • Polycyclohexylenedimethylene terephthalate resin composition

    WO2015099494A1

  • Master batch, resin composition and resin molded body

    WO2022201977A1

Cited By

  • Flow-line colorful PC-PMMA composite board and preparation method thereof

    CN121316375A

  • A textured, multi-colored PC-PMMA composite board and its preparation method

    CN121316375B