Water-swelling rubber waterstop and preparation method thereof

By using materials such as polyether polyurethane rubber and modified bentonite, the tensile strength and volume expansion ratio of the rubber water stop are improved, and the seal failure and fracture problems of traditional rubber water stops are solved, providing more reliable waterproof performance.

CN119019838AInactive Publication Date: 2024-11-26RUNHAITIEJIAN TECH DEV CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411523372.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-30
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional rubber water stops may lead to seal failure during long-term use and are prone to breaking under the action of large external forces, resulting in water leakage, especially in subway tunnel construction, where there is insufficient tensile strength and volume expansion ratio.

Method used

The water-expanded rubber water stop is used composed of polyether polyurethane rubber, modified bentonite and specific vulcanizing agents. By adjusting the hydroxyl value and mass ratio of polyether polyurethane rubber, combined with modified bentonite and vulcanizing agent, the water stop is improved. Tensile strength and volume expansion magnification.

Benefits of technology

It significantly improves the tensile strength and volume expansion ratio of the rubber water stop, enhances its waterproof performance and stability in different engineering environments, and ensures a more reliable sealing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of rubber waterstops, and provides a water-swellable rubber waterstop and a preparation method thereof.The water-swellable rubber waterstop is prepared from, by weight, 100 parts of polyether polyurethane rubber, 5-10 parts of super absorbent resin, 10-20 parts of a reinforcing agent, 1-2 parts of a vulcanizing agent, 0.5-1.5 parts of an anti-aging agent and 1-2 parts of an accelerant; the polyether polyurethane rubber is composed of first polyether polyurethane rubber and second polyether polyurethane rubber, the hydroxyl value of the first polyether polyurethane rubber is different from that of the second polyether polyurethane rubber, and the mass ratio of the first polyether polyurethane rubber to the second polyether polyurethane rubber is 1: 6-6: 1. According to the technical scheme, the problems of low tensile strength and low volume expansion rate of the water-swelling rubber waterstop in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber waterstops, and in particular to a water-swelling rubber waterstop and a preparation method thereof. Background Art

[0002] Rubber waterstop is a rubber product used to prevent water penetration. It is usually made of natural rubber or synthetic rubber and has good elasticity and sealing properties. Rubber waterstop is widely used in the fields of construction, underground engineering, water conservancy and hydropower, such as construction joints and deformation joints of structures such as basements, tunnels, pools, and dams, playing a key role in preventing water leakage. Traditional waterstop materials have certain limitations in performance.

[0003] On the one hand, ordinary rubber waterstops may fail to seal due to aging, deformation and other reasons during long-term use. The emergence of water-swelling rubber waterstops provides a new idea for solving this problem. Water-swelling rubber waterstops have unique properties. After contact with water, they can expand rapidly, fill gaps and form effective seals. This type of waterstop can adapt to different engineering environments and complex hydrological conditions. It has flexible installation methods and can adapt to construction joints of different shapes, providing more reliable protection for the waterproof sealing of the project.

[0004] On the other hand, rubber waterstops are prone to breakage under large external forces. During the construction of subway tunnels, since the tunnels pass through different geological layers, the pressure distribution of the soil is uneven, which may cause the tunnel structure to deform. At this time, the rubber waterstops installed at the construction joints will be subjected to tensile force. If the quality of the rubber waterstops is not up to standard or the installation is not standardized, they may break under such external forces, causing groundwater to seep into the tunnel and affect the safe operation of the subway.

[0005] Therefore, developing a water-swellable rubber waterstop with high tensile strength is of great significance for improving the performance of the waterstop and meeting the needs of different projects. Summary of the invention

[0006] The invention provides a water-swelling rubber waterstop and a preparation method thereof, which solves the problems of low tensile strength and low volume expansion ratio of the water-swelling rubber waterstop in the related art.

[0007] The technical scheme of the present invention is as follows: The present invention provides a water-swellable rubber waterstop, comprising the following component raw materials in parts by weight: 100 parts of polyether polyurethane rubber, 5-10 parts of highly absorbent resin, 10-20 parts of reinforcing agent, 1-2 parts of vulcanizing agent, 0.5-1.5 parts of antioxidant, and 1-2 parts of accelerator; The polyether polyurethane rubber consists of a first polyether polyurethane rubber and a second polyether polyurethane rubber, the first polyether polyurethane rubber and the second polyether polyurethane rubber have different hydroxyl values, and the mass ratio of the first polyether polyurethane rubber to the second polyether polyurethane rubber is 1:6-6:1.

[0008] As a further technical solution, the hydroxyl value of the first polyether polyurethane rubber is 54 mg KOH / g, the hydroxyl value of the second polyether polyurethane rubber is 187 mg KOH / g, and the mass ratio of the first polyether polyurethane rubber to the second polyether polyurethane rubber is 4-5:1.

[0009] As a further technical solution, the reinforcing agent includes one or more of bentonite, carbon black, and talc.

[0010] As a further technical solution, the bentonite is modified bentonite, the modifier of the modified bentonite is a polyamine compound, and the mass ratio of the modifier to the bentonite is 1-3:10.

[0011] The present invention uses a polyamine compound as a modifier to modify bentonite, improve the interlayer structure of bentonite, enhance the hydrophilicity of bentonite and its dispersibility in the polyether polyurethane rubber matrix, help to improve the water absorption uniformity of the waterstop, and improve the tensile strength and volume expansion ratio of the waterstop.

[0012] As a further technical solution, the polyamine compound includes one or more of polyetheramine, polyamide, and polyethyleneimine.

[0013] In the present invention, polyetheramine is preferably used as a modifier for modified bentonite, so as to enhance the bonding strength between the modified bentonite and the polyether polyurethane rubber matrix and improve the tensile strength and volume expansion ratio of the waterstop.

[0014] As a further technical solution, the preparation of the modified bentonite includes the following steps: dissolving the modifier in a solvent, adding the pretreated bentonite, dispersing evenly, heating and stirring to react, and filtering and drying to obtain the modified bentonite.

[0015] As a further technical solution, the vulcanizing agent includes one or more of dicumyl peroxide, benzoyl peroxide, and di-tert-butyl peroxide.

[0016] As a further technical solution, the antioxidant includes one or more of antioxidant RD, antioxidant BZ, and antioxidant MB.

[0017] As a further technical solution, the accelerator includes one or more of accelerator DM, accelerator NS, and accelerator PZ.

[0018] The present invention also provides a method for preparing a water-swellable rubber waterstop, comprising the following steps: S1. Weigh polyether polyurethane rubber, highly absorbent resin, reinforcing agent, vulcanizing agent, antioxidant and accelerator, and mix them evenly to obtain a rubber compound; S2. After the mixed rubber is extruded and vulcanized, a water-swellable rubber waterstop is obtained.

[0019] The working principle and beneficial effects of the present invention are: In the present invention, a first polyether polyurethane rubber and a second polyether polyurethane rubber with different hydroxyl values ​​are added as raw materials, and their mass ratio is adjusted to exert a synergistic effect, control the water absorption rate and expansion uniformity of the waterstop, adjust the number of active sites and the degree of cross-linking during the reaction, and improve the tensile strength and volume expansion ratio of the waterstop. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] In the following examples and comparative examples: Polyetheramine: Model D-230; Polyamide: model PA66; Polyethyleneimine: Model MW1800, manufacturer: Guangdong Wengjiang Chemical Reagent Co., Ltd.; Bentonite: particle size 1 μm; High water-absorbent resin: model 1235, water absorption ratio>400, manufacturer: Shandong Linchuan Water Technology Co., Ltd.; The first polyether polyurethane rubber: hydroxyl value is 54 mg KOH / g, model NS-2400, manufacturer is Aidi Co., Ltd.; The second polyether polyurethane rubber: the hydroxyl value is 187 mg KOH / g, the model is 0310, and the manufacturer is Dow Chemical Company.

[0022] Example 1 S1, weighing 100 parts of polyether polyurethane rubber, 5 parts of super absorbent resin, 10 parts of bentonite, 1 part of dicumyl peroxide, 0.5 parts of antioxidant RD, and 1 part of accelerator DM, and mixing for 20 minutes to obtain a rubber mixture, wherein the polyether polyurethane rubber is composed of a first polyether polyurethane rubber and a second polyether polyurethane rubber in a mass ratio of 3:1; S2. The mixed rubber is pressed into thin sheets by a double-roll mill and vulcanized with hot air to obtain a water-expandable rubber waterstop.

[0023] Example 2 S1, weighing 100 parts of polyether polyurethane rubber, 8 parts of super absorbent resin, 15 parts of bentonite, 1.5 parts of benzoyl peroxide, 1 part of antioxidant BZ, and 1.5 parts of accelerator NS, and mixing for 25 minutes to obtain a rubber mixture, wherein the polyether polyurethane rubber is composed of a first polyether polyurethane rubber and a second polyether polyurethane rubber in a mass ratio of 3:1; S2. The mixed rubber is pressed into thin sheets by a double-roll mill and vulcanized with hot air to obtain a water-expandable rubber waterstop.

[0024] Example 3 S1, weighing 100 parts of polyether polyurethane rubber, 10 parts of super absorbent resin, 20 parts of bentonite, 2 parts of di-tert-butyl peroxide, 1.5 parts of antioxidant MB, and 2 parts of accelerator PZ, and mixing for 30 minutes to obtain a mixed rubber, wherein the polyether polyurethane rubber is composed of a first polyether polyurethane rubber and a second polyether polyurethane rubber in a mass ratio of 1:6; S2. The mixed rubber is pressed into thin sheets by a double-roll mill and vulcanized with hot air to obtain a water-expandable rubber waterstop.

[0025] Example 4 Compared with Example 2, Example 4 is different in that the polyether polyurethane rubber consists of a first polyether polyurethane rubber and a second polyether polyurethane rubber in a mass ratio of 4:1.

[0026] Example 5 Compared with Example 2, the difference in Example 5 is that the polyether polyurethane rubber consists of a first polyether polyurethane rubber and a second polyether polyurethane rubber in a mass ratio of 5:1.

[0027] Example 6 Compared with Example 2, the difference of Example 6 is that the polyether polyurethane rubber consists of a first polyether polyurethane rubber and a second polyether polyurethane rubber in a mass ratio of 6:1.

[0028] Example 7 The preparation of modified bentonite includes the following steps: dissolving 1 part of polyetheramine in 50 parts of ethanol and stirring evenly, crushing and grinding 10 parts of bentonite, passing through a 200-mesh sieve to obtain pretreated bentonite, adding the pretreated bentonite to the polyetheramine solution, dispersing evenly, heating to 70°C, stirring and reacting for 5 hours, filtering and drying to obtain modified bentonite.

[0029] Compared with Example 5, the difference of Example 7 is that bentonite is replaced by modified bentonite obtained by the above preparation method.

[0030] Example 8 Compared with Example 7, the difference in Example 8 is that the added amount of polyetheramine is 3 parts.

[0031] Example 9 Compared with Example 8, Example 9 is different in that the polyetheramine is replaced by an equal amount of polyamide.

[0032] Example 10 Compared with Example 8, Example 10 is different in that the polyetheramine is replaced by an equal amount of polyethyleneimine.

[0033] Comparative Example 1 Compared with Example 2, the difference in Comparative Example 1 is that the polyether polyurethane rubber is only the first polyether polyurethane rubber.

[0034] Comparative Example 2 Compared with Example 2, Comparative Example 2 is different in that the polyether polyurethane rubber is only the second polyether polyurethane rubber.

[0035] The water-swellable rubber waterstops prepared in Examples 1 to 10 and Comparative Examples 1 to 2 were tested according to the following method: 1. Tensile strength: Test the tensile strength of the sample according to the tensile strength test method specified in GB / T 18173.3-2014 "Polymer waterproof materials Part 3: Water-swelling rubber".

[0036] 2. Volume expansion ratio: According to the volume expansion ratio test method specified in GB / T 18173.3-2014 "Polymer waterproof materials Part 3: Water-swelling rubber", the volume expansion ratio of the test sample is tested.

[0037] The test results are shown in the following table: Table 1 Performance test results of water-swellable rubber waterstops prepared in Examples 1 to 10 and Comparative Examples 1 to 2

[0038] Compared with Example 2, Comparative Example 1 only adds the first polyether polyurethane rubber, and Comparative Example 2 only adds the second polyether polyurethane rubber. As a result, the tensile strength and volume expansion ratio of Example 2 are better than those of Comparative Examples 1 and 2, indicating that the first polyether polyurethane rubber and the second polyether polyurethane rubber play a synergistic role and can improve the tensile strength and volume expansion ratio of the waterstop. In Examples 2 and Examples 4 to 6, different mass ratios of the first polyether polyurethane rubber and the second polyether polyurethane rubber are added. As a result, the tensile strength and volume expansion ratio of Examples 4 and 5 are better than those of Examples 2 and 6, indicating that when the mass ratio of the first polyether polyurethane rubber to the second polyether polyurethane rubber is 4 to 5:1, the tensile strength and volume expansion ratio of the obtained waterstop are better.

[0039] Compared with Example 5, modified bentonite was added in Examples 7 and 8. As a result, the tensile strength and volume expansion ratio of Examples 7 and 8 were better than those of Example 5, indicating that the addition of modified bentonite can improve the tensile strength and volume expansion ratio of the waterstop.

[0040] Compared with Example 8, Examples 9 and 10 added different modifiers to modify the bentonite. As a result, the tensile strength and volume expansion ratio of Example 8 were better than those of Examples 9 and 10, indicating that when the modifier is polyetheramine, the tensile strength and volume expansion ratio of the obtained waterstop are better.

[0041] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A water-swellable rubber waterstop, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of polyether polyurethane rubber, 5-10 parts of highly absorbent resin, 10-20 parts of reinforcing agent, 1-2 parts of vulcanizing agent, 0.5-1.5 parts of antioxidant and 1-2 parts of accelerator; the polyether polyurethane rubber consists of a first polyether polyurethane rubber and a second polyether polyurethane rubber, the first polyether polyurethane rubber and the second polyether polyurethane rubber have different hydroxyl values, and the mass ratio of the first polyether polyurethane rubber to the second polyether polyurethane rubber is 1:6-6:

1.

2. The water-swellable rubber waterstop according to claim 1, characterized in that: The hydroxyl value of the first polyether polyurethane rubber is 54 mg KOH / g, the hydroxyl value of the second polyether polyurethane rubber is 187 mg KOH / g, and the mass ratio of the first polyether polyurethane rubber to the second polyether polyurethane rubber is 4-5:

1.

3. The water-swellable rubber waterstop according to claim 1, characterized in that: The reinforcing agent includes one or more of bentonite, carbon black and talc.

4. The water-swellable rubber waterstop according to claim 3, characterized in that: The bentonite is modified bentonite, the modifier of the modified bentonite is a polyamine compound, and the mass ratio of the modifier to the bentonite is 1-3:

10.

5. The water-swellable rubber waterstop according to claim 4, characterized in that: The polyamine compound includes one or more of polyetheramine, polyamide and polyethyleneimine.

6. The water-swellable rubber waterstop according to claim 4, characterized in that: The preparation of the modified bentonite comprises the following steps: The modifier is dissolved in a solvent, and the pretreated bentonite is added and dispersed evenly. After heating and stirring for reaction, the modified bentonite is obtained by filtering and drying.

7. The water-swellable rubber waterstop according to claim 1, characterized in that: The vulcanizing agent includes one or more of dicumyl peroxide, benzoyl peroxide, and di-tert-butyl peroxide.

8. The water-swellable rubber waterstop according to claim 1, characterized in that: The antioxidant includes one or more of antioxidant RD, antioxidant BZ, and antioxidant MB.

9. The water-swellable rubber waterstop according to claim 1, characterized in that: The accelerator includes one or more of accelerator DM, accelerator NS and accelerator PZ.

10. A method for preparing a water-swellable rubber waterstop according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Weigh polyether polyurethane rubber, highly absorbent resin, reinforcing agent, vulcanizing agent, antioxidant and accelerator, and mix them evenly to obtain a rubber compound; S2. After the mixed rubber is extruded and vulcanized, a water-swellable rubber waterstop is obtained.

Citation Information

Patent Citations

  • Polyurethane-based sealing material composition

    JP2010018762A

  • Solvent-free reactive adhesive agent, cured product thereof, and laminate

    JP2022082441A

  • Low-k dielectric functional imprinting materials

    US20060081557A1

  • One-part, curable polyurethane

    US4412033A

  • Foamed polyurethane resin composition, foamed polyurethane elastomer, and mid-sole

    WO2020203399A1