Preparation method of basalt fiber modified and reinforced polyimide composite friction material

Through chemical graft modification of basalt fibers and electrostatic adsorption of nanomaterials, combined with hot pressing technology, the problem of low bonding strength between basalt fibers and resin matrix is ​​solved, and a composite material with high strength and toughness and stable friction performance is prepared, suitable for new Energy and electric vehicles and other fields.

CN119019844APending Publication Date: 2024-11-26SICHUAN UNIVERSITY OF SCIENCE AND ENGINEERING +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411172642.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The bonding strength between basalt fibers and resin matrix is ​​not high, which makes it difficult to exert excellent performance in actual engineering applications, limiting its application in friction materials.

Method used

The pretreated basalt fibers were subjected to ultrasonic cleaning and chemical graft modification of acetone solution, combined with the electrostatic adsorption of nano-silica and graphene oxide, and then heat-pressed with thermoplastic polyimide in a high-temperature pressurized vulcanization machine. Heat treatment was carried out to prepare composite materials with high strength and toughness and stable and controllable friction coefficient.

Benefits of technology

It has achieved a resin-based composite friction material with uniform dispersion and compatibility of basalt fibers, with high strength, toughness, wear resistance and stable friction performance, and is suitable for new energy electric vehicles and high-performance electromagnetic brakes and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019844A_ABST
    Figure CN119019844A_ABST
Patent Text Reader

Abstract

The invention relates to the field of basalt fiber reinforced resin-based composite friction materials, in particular to a preparation method of a basalt fiber modified and reinforced polyimide composite material. According to the preparation method, nano graphene oxide and nano silicon dioxide are attached to the surface of gamma-aminopropyltriethoxysilane chemically-grafted basalt fiber through an electrostatic self-assembly method, and the composite friction material is prepared from the modified basalt fiber and thermoplastic polyimide in a mold in a hot-pressing forming mode. The invention aims to solve the technical problems that under the condition that the strength of basalt fibers is ensured, the interface bonding between the basalt fibers and a polyimide matrix is improved, so that the composite material is compact in structure, excellent in thermal stability, high in obdurability, stable and controllable in friction coefficient, excellent in wear resistance, simple in process and low in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of basalt fiber reinforced resin composite materials, and in particular relates to a preparation method of a basalt fiber modified reinforced polyimide composite friction material. Background Art

[0002] Friction materials have a key impact on the motion reliability and service stability of various power machines. With the rapid development of the machinery industry, friction and wear have become one of the main factors of material, energy dissipation and part failure, which not only determines the service life of the product, but also affects our lives and the environment. Reducing friction, wear and energy loss during the movement of various components is the primary concern of the industrial revolution. Therefore, developing high-performance lubricating materials to reduce friction and wear is one of the effective ways to improve the reliability and service life of mechanical moving parts.

[0003] As a self-lubricating polymer, polyimide is lightweight, high-strength, high and low temperature resistant, low dielectric, flame retardant and has excellent comprehensive mechanical properties. It has broad application prospects in friction parts of aerospace, new energy vehicles, electronics and microelectronics. In order to improve the tribological properties of polyimide resin, researchers have found that the use of fiber-modified polyimide composite friction materials is an important means to improve tribological properties.

[0004] Basalt fiber is a green and pollution-free high-performance mineral fiber, known as the "green industrial material" of the 21st century. It has the advantages of high strength, heat resistance, good high-temperature dimensional stability, strong corrosion resistance, etc., and is suitable for strengthening and toughening resin-based composite friction materials. However, the surface of basalt fiber is smooth and inert, so the bonding strength with the resin matrix is ​​not high, making it difficult to exert the excellent performance of basalt fiber, which seriously limits its actual engineering application.

[0005] In summary, the present application now proposes a method for preparing a basalt fiber modified and reinforced polyimide composite friction material to solve the above-mentioned problems. Summary of the invention

[0006] The present invention aims to solve the problems raised in the background technology. The purpose of this specification is to prepare a basalt fiber modified and reinforced polyimide composite friction material, which can prepare a resin-based composite friction material with uniform basalt fiber dispersion, good compatibility, high strength and toughness, stable and controllable friction coefficient and excellent wear resistance.

[0007] Based on the above purpose, one or more embodiments of this specification provide a method for preparing a basalt fiber modified reinforced polyimide composite material, comprising the following steps:

[0008] S1, ultrasonically cleaning the pretreated basalt fiber with an acetone solution and then chemically grafting and modifying the fiber to obtain a grafted basalt fiber;

[0009] S2, hydrolyzing tetraethyl silicate and amino-functionalizing it with γ-aminopropyltriethoxysilane to obtain positively charged amino-functionalized nano-silica;

[0010] S3, mixing the grafted basalt fiber obtained in step S1, the nano-silicon dioxide obtained in step S2 and the graphene oxide solution, and then performing electrostatic adsorption to obtain modified basalt fiber;

[0011] S4, mixing the modified basalt fiber prepared in step S3 with thermoplastic polyimide, putting the mixture into a mold, and hot pressing the mixture on a high-temperature pressure vulcanizer:

[0012] S5. heat-treating the formed composite material in an oven.

[0013] According to the method for preparing the basalt fiber modified and reinforced polyimide composite material described in the embodiment of the present invention, the raw materials include the following materials:

[0014] 6-9mm basalt fiber, 15%-20%;

[0015] 800 mesh thermoplastic polyimide, 85%-80%;

[0016] The rest are:

[0017] Monolayer graphene oxide, acetone, γ-aminopropyltriethoxysilane, ammonium hydroxide, concentrated hydrochloric acid, tetraethyl silicate, anhydrous ethanol, and deionized water.

[0018] According to the preparation method of the basalt fiber modified reinforced polyimide composite material described in an embodiment of the present invention, the pretreatment of the basalt fiber in step S1 includes the following steps: placing the basalt fiber in an acetone solution at a ratio of 50 g / L, ultrasonically cleaning it for 24 hours, filtering it, and washing it with deionized water for 5-6 times, and drying it at a temperature of 120°C for 12 hours.

[0019] According to the preparation method of the basalt fiber modified reinforced polyimide composite material described in an embodiment of the present invention, the chemical grafting in step S1 is specifically: a γ-aminopropyltriethoxysilane solution prepared by volume of γ-aminopropyltriethoxysilane, anhydrous ethanol and deionized water in a volume ratio of 1:6:3 is magnetically stirred for 2 hours in a 40°C water bath, and the pretreated basalt fiber is added and stirred for 2-4 hours, and then after washing with deionized water, it is dried at 120°C for 12 hours.

[0020] According to the preparation method of the basalt fiber modified reinforced polyimide composite material described in an embodiment of the present invention, step S2 includes the following steps: anhydrous ethanol, deionized water, ammonia water and tetraethyl silicate are quickly mixed in a volume fraction ratio of 50:6:3:1, and magnetically stirred for 4 hours in a 50°C water bath, and then γ-aminopropyltriethoxysilane is quickly added to the mixed solution at a volume fraction of 100:1, reacted at room temperature for 24 hours, washed with deionized water, and vacuum dried at 50°C for 2.5 hours.

[0021] According to the preparation method of the basalt fiber modified reinforced polyimide composite material described in the embodiment of the present invention, the step S3 includes the following steps: adding graphene oxide to deionized water and ultrasonically dispersing it for 1 hour to obtain a graphene oxide solution with a concentration of 1g / L, then adding concentrated hydrochloric acid to adjust the pH value of the graphene oxide solution to 3, adding the grafted basalt fiber prepared in step S1, and reacting it with magnetic stirring in a water bath at 80°C for 2 hours, then adding the silicon dioxide prepared in step S2 and continuing to react for 2 hours, after the reaction is completed, washing the flocculent precipitate on the fiber surface with deionized water, and finally heat treating it in an oven at 160°C for 12 hours to obtain modified basalt fiber.

[0022] According to the method for preparing the basalt fiber modified reinforced polyimide composite material described in the embodiment of the present invention, the composite material preparation step S4 comprises the following steps:

[0023] S4-1, cold pressed:

[0024] The modified basalt fiber prepared in step S3 and thermoplastic polyimide are mixed in a stirrer at a mass fraction ratio of 17:5 at a speed of 2500 r / min for 10 minutes, the uniformly mixed raw materials are placed in a mold, the mold is placed on a vulcanizer, and cold pressed at room temperature and a pressure of 5-10 MPa for 20-30 minutes; the cold pressing is repeated 2-4 times;

[0025] S4-2, hot pressing:

[0026] The temperature was raised to 200-220°C at a heating rate of 10°C / min, and the curing was carried out at a temperature of 200-220°C and a pressure of 15-20MPa for 20-30min, and the exhaust was performed every 5min;

[0027] Continue to raise the temperature to 240-260°C, and cure for 20-30 minutes at a temperature of 240-260°C and a pressure of 15-20MPa;

[0028] Finally, the temperature is raised to 280-300°C, and the curing is carried out for 40-60 minutes at a temperature of 280-300°C and a pressure of 15-20MPa;

[0029] S4-3, demoulding after cooling to room temperature.

[0030] According to the method for preparing the basalt fiber modified reinforced polyimide composite material described in the embodiment of the present invention, the composite material heat treatment step S5 comprises the following steps:

[0031] The composite material prepared in step S4 is placed in an oven and heated freely to 200°C and kept warm for 60 minutes, then heated to 220°C and kept warm for 60 minutes, and finally heated to 240°C and kept warm for 120 minutes. The oven is cooled to room temperature and the material is taken out to complete the preparation of the modified basalt fiber reinforced polyimide composite material.

[0032] According to the above, the present invention has the following beneficial effects:

[0033] The present invention aims at the problems of low interface bonding strength, low compatibility, poor wettability and insufficient density between basalt fiber and polyimide, and uneven distribution of fiber and nanofiller. The present invention combines a specific basalt fiber surface modification process, a nanomaterial electrostatic self-assembly process, and cold pressing, hot pressing and heat treatment processes to prepare a friction material with uniform fiber distribution, dense structure, excellent thermal stability, high toughness, stable and controllable friction coefficient and excellent wear resistance, while having the advantages of simple process, low cost and environmental friendliness. It has broad application prospects in the fields of new energy electric vehicles, high-performance electromagnetic brakes, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate one or more embodiments of the present specification or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only one or more embodiments of the present specification. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 This is a scanning electron microscope image of modified basalt fiber (×2000).

[0036] Figure 2 (a) is an electron microscope scanning image of the wear surface (×150) of the unmodified basalt fiber reinforced polyimide composite material (BF / PI) and GCr15 in Comparative Example 1 after grinding for 60 minutes under a load of 10N.

[0037] Figure 2 (b) is an electron microscope scanning image of the worn surface (×150) of the γ-aminopropyltriethoxysilane modified basalt fiber reinforced polyimide composite material (KH550-BF / PI) and GCr15 in Comparative Example 2 after grinding for 60 minutes under a load of 10N.

[0038] Figure 2 (c) is an electron microscope scanning image of the worn surface (×150) of the graphene oxide modified basalt fiber reinforced polyimide composite material (GO-BF / PI) and GCr15 in Comparative Example 3 after grinding for 60 minutes under a load of 10N.

[0039] Figure 2 (d) is an electron microscope scanning image of the wear surface (×150) of the modified basalt fiber reinforced polyimide composite material (SiO2-GO-BF / PI) and GCr15 after grinding for 60 minutes under a load of 10N in Example 1.

[0040] Figure 3 This is the actual friction coefficient curve of the basalt fiber reinforced polyimide resin composite material proposed in the comparative example and the embodiment of the present invention and GCr15 after grinding for 60 minutes under a load of 10N.

[0041] Figure 4 (a) is the friction coefficient of the basalt fiber reinforced polyimide resin composite material proposed in the comparative example and the embodiment of the present invention under loads of 5N, 10N and 20N.

[0042] Figure 4 (b) is the wear rate of the basalt fiber reinforced polyimide resin composite material proposed in the comparative example and the embodiment of the present invention under loads of 5N, 10N and 20N. DETAILED DESCRIPTION

[0043] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in conjunction with specific embodiments.

[0044] Example 1

[0045] Step 1: Place chopped basalt fibers with a diameter of 7-15 μm and a length of 3-6 mm in a ratio of 50 g / L into a 20% acetone solution, ultrasonically clean the fibers for 12 hours, then take them out and ultrasonically clean them with deionized water for 5 times, each time for 10 minutes, and then bake them in a 120°C oven for 8 hours;

[0046] γ-aminopropyl triethoxysilane (KH550) was added to a mixed solution of anhydrous ethanol and deionized water in a volume ratio of 6:3 to prepare a KH550 solution with a volume fraction of 5-10%, and then 1-2 ml of concentrated hydrochloric acid was added to adjust the pH value of the mixed solution to 4, and the solution was placed in a 40°C water bath in a magnetic stirrer and hydrolyzed with magnetic stirring for 2 hours. Then, the desizing short-cut basalt fiber was placed in the treated mixed solution, and the reaction was continued under magnetic stirring in a 40°C water bath for 2-4 hours. After the reaction, it was washed with an appropriate amount of deionized water for 3 times, and placed in an 80°C oven for 12 hours to obtain the grafted basalt fiber.

[0047] Step 2: Anhydrous ethanol, deionized water, ammonia water and tetraethyl silicate are quickly mixed at a volume fraction ratio of 50:6:3:1, and the resulting solution is magnetically stirred in a 50°C water bath for 4-6 hours. Then, the grafted basalt fiber is quickly added to the mixed solution after the reaction at a volume ratio of 100:1, and the reaction is carried out at room temperature for 24 hours. After the reaction, it is washed with an appropriate amount of deionized water and placed in a 50°C oven for 2.5 hours to obtain positively charged amino-functionalized nano-silica.

[0048] Step 3: ultrasonically disperse an appropriate amount of graphene oxide in deionized water for 1 h to obtain a 1 g / L graphene oxide solution with negative charge, add concentrated hydrochloric acid to adjust the pH value to 3, add the above-mentioned grafted basalt fiber, and react with magnetic stirring in a 40°C water bath for 2 h, then add the above-mentioned amino-functionalized nano-silica and continue to react for 2 h. After the reaction is completed, wash the flocculent precipitate on the fiber surface with deionized water, and finally heat treat in an oven at 160°C for 12 h to obtain modified basalt fiber, such as Figure 1 shown.

[0049] Step 4:

[0050] Cold Pressed:

[0051] The modified basalt fiber prepared in step S3 and thermoplastic polyimide are mixed in a stirrer at a mass fraction ratio of 17:5 at a speed of 2500 r / min for 10 minutes, the uniformly mixed raw materials are placed in a mold, the mold is placed on a vulcanizer, and cold pressed at room temperature and a pressure of 5-10 MPa for 20-30 minutes; the cold pressing is repeated 2-4 times;

[0052] Heat Pressing:

[0053] The temperature was raised to 200-220°C at a heating rate of 10°C / min, and the curing was carried out at a temperature of 200-220°C and a pressure of 15-20MPa for 20-30min, and the exhaust was performed every 5min;

[0054] Continue to raise the temperature to 240-260°C, and cure for 20-30 minutes at a temperature of 240-260°C and a pressure of 15-20MPa;

[0055] Finally, the temperature is raised to 280-300°C, and the curing is carried out for 40-60 minutes at a temperature of 280-300°C and a pressure of 15-20MPa;

[0056] Cool to room temperature and then demould.

[0057] Step 5: Place the composite material obtained in step 5 in an oven and heat it freely to 200°C and keep it warm for 60 minutes, then heat it to 220°C and keep it warm for 60 minutes, and finally heat it to 240°C and keep it warm for 120 minutes. Wait for the oven to cool to room temperature and take out the material to complete the preparation of the modified basalt fiber reinforced polyimide composite material.

[0058] Comparative Example 1

[0059] Compared with Example 1, only the basalt fiber was pretreated to prepare an unmodified basalt fiber reinforced polyimide composite material (BF / PI).

[0060] Comparative Example 2

[0061] Compared with Example 1, on the basis of pretreatment of basalt fiber, only KH550-modified basalt fiber was performed to prepare a KH550-modified basalt fiber reinforced polyimide composite material (KH550-BF / PI).

[0062] Comparative Example 3

[0063] Compared with Example 1, on the basis of pretreatment of basalt fiber and KH550 modification, graphite oxide was adsorbed on the surface of basalt fiber by electrostatic self-loading method to prepare graphene oxide modified basalt fiber reinforced polyimide composite material (GO-BF / PI).

[0064] In order to verify the changes in mechanical and thermal properties of basalt fiber reinforced polyimide composites (BF / PI, KH550-BF / PI, GO-BF / PI, SiO2-GO-BF / PI) treated with different modification methods, BF / PI, KH550-BF / PI, GO-BF / PI, SiO2-GO-BF / PI samples were tested. The results are shown in Table 1:

[0065]

[0066] Table 1 Mechanical and thermal properties of BF / PI, KH550-BF / PI, GO-BF / PI, and SiO2-GO-BF / PI samples

[0067] like Figure 2 As shown, after 60 minutes of wear, the wear surfaces of Comparative Examples 1 and 2 are rough and have obvious fatigue wear cracks, a large number of pits and furrows, and the basalt fibers are exposed or lost; although obvious furrows and a small amount of wear debris can be seen on the wear surfaces of Comparative Example 3 and Example 1, there are no grooves or holes on the surface, and the wear surfaces are relatively smooth, indicating that there is no obvious tearing or damage on the wear surfaces.

[0068] like Figure 3The figure shows the friction coefficient-time curves of the composite friction materials prepared in Comparative Example 1, Comparative Example 2, Comparative Example 3 and Example 1 when they were ground against GCr15 for 60 minutes. It can be seen that the friction coefficient curve of Comparative Example 1 fluctuates greatly, and the average friction coefficient is the highest; the friction coefficient curve of Example 1 fluctuates more smoothly, and the average friction coefficient is the lowest.

[0069] like Figure 4 As shown, Figure 4 (a) is the friction coefficient of the composite friction materials prepared in Comparative Example 1, Comparative Example 2, Comparative Example 3 and Example 1 under loads of 5N, 10N and 20N, Figure 4 (b) is the wear rate of the composite friction materials prepared in Comparative Example 1, Comparative Example 2, Comparative Example 3 and Example 1 under loads of 5N, 10N and 20N. It can be seen that the friction coefficient and wear rate of Example 1 are the lowest under different loads.

[0070] One or more embodiments of this specification are intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of one or more embodiments of this specification should be included in the scope of protection of this disclosure.

Claims

1. A method for preparing a basalt fiber modified and reinforced polyimide composite material, It is characterized in that The following steps are involved: S1, ultrasonically cleaning the pretreated basalt fiber with an acetone solution and then chemically grafting and modifying the fiber to obtain a grafted basalt fiber; S2, hydrolyzing tetraethyl silicate and amino-functionalizing it with γ-aminopropyltriethoxysilane to obtain positively charged amino-functionalized nano-silica; S3, mixing the grafted basalt fiber obtained in step S1, the nano-silicon dioxide obtained in step S2 and the graphene oxide solution, and then performing electrostatic adsorption to obtain modified basalt fiber; S4, mixing the modified basalt fiber prepared in step S3 with thermoplastic polyimide, putting the mixture into a mold, and hot pressing the mixture on a high-temperature pressure vulcanizer: S5. heat-treating the formed composite material in an oven.

2. The method for preparing the basalt fiber modified and reinforced polyimide composite material according to claim 1, Features: The raw materials include the following materials: 6-9mm basalt fiber, 15%-20%; 800 mesh thermoplastic polyimide, 85%-80%; The rest are: Monolayer graphene oxide, acetone, γ-aminopropyltriethoxysilane, ammonium hydroxide, concentrated hydrochloric acid, tetraethyl silicate, anhydrous ethanol, and deionized water.

3. The method for preparing the basalt fiber modified and reinforced polyimide composite material according to claim 2, It is characterized in that The pretreatment of basalt fiber in step S1 comprises the following steps: placing the basalt fiber in an acetone solution at a ratio of 50 g / L, ultrasonically cleaning it for 24 hours, filtering it, washing it with deionized water for 5-6 times, and drying it at a temperature of 120° C. for 12 hours.

4. The method for preparing the basalt fiber modified and reinforced polyimide composite material according to claim 3, It is characterized in that The chemical grafting in step S1 is specifically as follows: a γ-aminopropyltriethoxysilane solution prepared by volume of γ-aminopropyltriethoxysilane, anhydrous ethanol and deionized water in a volume ratio of 1:6:3 is magnetically stirred for 2 hours in a 40°C water bath, and the pretreated basalt fiber is added and stirred for 2-4 hours, and then washed with deionized water and dried at 120°C for 12 hours.

5. The method for preparing the basalt fiber modified and reinforced polyimide composite material according to claim 4, It is characterized in that The step S2 comprises the following steps: quickly mixing anhydrous ethanol, deionized water, ammonia water and tetraethyl silicate at a volume fraction ratio of 50:6:3:1, and magnetically stirring for 4 hours in a 50°C water bath, and then quickly adding γ-aminopropyltriethoxysilane to the mixed solution at a volume fraction of 100:1, reacting at room temperature for 24 hours, washing with deionized water, and vacuum drying at 50°C for 2.5 hours.

6. The method for preparing the basalt fiber modified and reinforced polyimide composite material according to claim 5, It is characterized in that The step S3 comprises the following steps: adding graphene oxide to deionized water and ultrasonically dispersing it for 1 hour to obtain a graphene oxide solution with a concentration of 1 g / L, then adding concentrated hydrochloric acid to adjust the pH value of the graphene oxide solution to 3, adding the grafted basalt fiber prepared in step S1, and reacting it under magnetic stirring for 2 hours in a water bath at 80° C., then adding the silicon dioxide prepared in step S2 and continuing to react for 2 hours, after the reaction is completed, washing the flocculent precipitate on the fiber surface with deionized water, and finally heat treating it in an oven at 160° C. for 12 hours to obtain the modified basalt fiber.

7. The method for preparing the basalt fiber modified and reinforced polyimide composite material according to claim 6, It is characterized in that The composite material preparation step S4 comprises the following steps: S4-1, cold pressed: The modified basalt fiber prepared in step S3 and thermoplastic polyimide are mixed in a stirrer at a mass fraction ratio of 17:5 at a speed of 2500 r / min for 10 minutes, the uniformly mixed raw materials are placed in a mold, the mold is placed on a vulcanizer, and cold pressed at room temperature and a pressure of 5-10 MPa for 20-30 minutes; the cold pressing is repeated 2-4 times; S4-2, hot pressing: The temperature was raised to 200-220°C at a heating rate of 10°C / min, and the curing was carried out at a temperature of 200-220°C and a pressure of 15-20MPa for 20-30min, and the exhaust was performed every 5min; Continue to raise the temperature to 240-260°C, and cure for 20-30 minutes at a temperature of 240-260°C and a pressure of 15-20MPa; Finally, the temperature is raised to 280-300°C, and the curing is carried out for 40-60 minutes at a temperature of 280-300°C and a pressure of 15-20MPa; S4-3, demoulding after cooling to room temperature.

8. The method for preparing the basalt fiber modified and reinforced polyimide composite material according to claim 7, It is characterized in that The composite material heat treatment step S5 comprises the following steps: The composite material prepared in step S4 is placed in an oven and heated freely to 200°C and kept warm for 60 minutes, then heated to 220°C and kept warm for 60 minutes, and finally heated to 240°C and kept warm for 120 minutes. The oven is cooled to room temperature and the material is taken out to complete the preparation of the modified basalt fiber reinforced polyimide composite material.

Citation Information

Cited By

  • Basalt fiber drawing control method, system, equipment and medium

    CN120553980A